A kinetic energy conversion gradient thermal shot peening method and system
By using the kinetic energy conversion gradient thermal shot peening method, the instantaneous temperature rise generated by the shot in different areas of the workpiece is utilized, which solves the problems of complex equipment and thermal damage in the existing thermal shot peening technology, and realizes high-precision and low-cost metal surface strengthening.
Patent Information
- Application Number
- CN202611324272.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-28
- Publication Date
- 2026-11-17
AI Technical Summary
Existing thermal shot peening technology requires an external heat source, resulting in complex and costly equipment. It also makes it difficult to achieve millisecond-level instantaneous heating and precise temperature control, leading to problems such as thermal inertia delay and unintended thermal damage.
The kinetic energy conversion gradient thermal shot peening method is adopted. By accelerating the shot to the critical ejection velocity, it is converted into thermal energy and plastic deformation energy when it impacts the workpiece. Different instantaneous temperature rises are generated in different areas of the workpiece by the shot, so as to achieve differentiated thermal shot peening strengthening and form a gradient-distributed residual compressive stress layer.
High-precision shot peening can be achieved without an external heat source, avoiding thermal inertia delay and unintended thermal damage, significantly improving the fatigue resistance and stress relaxation resistance of parts, and precisely matching the strengthening effect with service requirements.
Smart Images

Figure CN123108250A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of shot peening technology, and in particular to a kinetic energy conversion gradient thermal shot peening method and system. Background Technology
[0002] Hot shot peening is an advanced metal surface strengthening process. It involves heating the surface of a workpiece to a specific temperature using an external heat source before shot peening. This technology utilizes the thermo-mechanical synergistic effect to reduce the plastic deformation capacity of materials, induces a deeper and higher residual compressive stress layer, and refines the grain structure, thereby significantly improving the fatigue resistance and stress relaxation resistance of parts.
[0003] Existing thermal shot peening technologies all require an external heat source to heat the workpiece, such as induction heating shot peening, thermal radiation shot peening, and laser-assisted thermal shot peening. The basic process is as follows: First, the workpiece or its surface is heated to a preset temperature by an external heating device. Then, the shot peening equipment is started to perform shot peening strengthening treatment on the heated area. During this process, the workpiece temperature is monitored in real time by a temperature sensor and fed back to the control system to maintain temperature stability. After shot peening is completed, heating is stopped, and the workpiece is unloaded after cooling.
[0004] However, the introduction of external heat sources leads to complex structures and high manufacturing costs for thermal shot peening equipment, which severely restricts the industrial application of this technology. This external heating method has a thermal inertia delay effect, making it difficult to achieve millisecond-level instantaneous heating and precise temperature control, which reduces the workpiece strengthening accuracy. Furthermore, external heating inevitably causes heat input to non-shot-peened areas, resulting in thermal damage problems such as unexpected phase transformation and grain coarsening. Summary of the Invention
[0005] This invention provides a kinetic energy conversion gradient thermal shot peening method and system, which can complete shot peening of workpieces at low cost and high precision.
[0006] This invention provides a kinetic energy conversion gradient thermal shot peening method and system, comprising the following steps: accelerating the projectile to a critical ejection velocity or higher, so that the projectile acquires sufficient kinetic energy to generate a thermal effect upon impact, wherein the critical ejection velocity is the minimum velocity at which the kinetic energy of the projectile upon impact with the workpiece is sufficient to be converted into thermal energy to bring the surface layer of the workpiece to the temperature required for thermal shot peening; spraying the accelerated projectile into different areas of the workpiece, wherein the projectiles sprayed into different areas have different ejection velocities, so that the kinetic energy carried by the projectile upon impact with the workpiece is converted into plastic deformation energy and thermal energy of the workpiece surface material, thereby utilizing the thermal energy to cause different instantaneous temperature rises in different areas of the workpiece; under the synergistic effect of the plastic deformation energy and thermal energy generated by the kinetic energy conversion, differentiated thermal shot peening is performed on different areas of the workpiece, forming a gradient-distributed residual compressive stress layer in different areas of the workpiece.
[0007] Preferably, the projectile is accelerated to the critical shot peening velocity of 100 m / s to 250 m / s.
[0008] Preferably, the step of spraying accelerated projectiles into different areas of the workpiece, with the projectiles sprayed into different areas having different ejection velocities, specifically includes: presetting corresponding surface temperature rise target values for different areas of the workpiece; adjusting the shot peening pressure according to the preset surface temperature rise target values to change the ejection velocity of the projectiles, so that the projectiles sprayed into different areas have different impact velocities.
[0009] Preferably, in the gradient control step: a first shot peening zone, a second shot peening zone, and a third shot peening zone are sequentially set along the axial direction of the workpiece; the spray gun is controlled to perform shot peening in the first shot peening zone at a first shot peening pressure to obtain a first surface temperature rise and a first residual compressive stress layer; the spray gun is controlled to perform shot peening in the second shot peening zone at a second shot peening pressure to obtain a second surface temperature rise and a second residual compressive stress layer; the spray gun is controlled to perform shot peening in the third shot peening zone at a third shot peening pressure to obtain a third surface temperature rise and a third residual compressive stress layer; wherein the first shot peening pressure, the second shot peening pressure, and the third shot peening pressure are different from each other, and the first surface temperature rise, the second surface temperature rise, and the third surface temperature rise correspond to different thermal shot peening temperature ranges.
[0010] Preferably, the first shot peening pressure is 0.09 MPa to 1.01 MPa, corresponding to a first surface temperature rise of 152°C to 162°C; the second shot peening pressure is 1.19 MPa to 1.21 MPa, corresponding to a second surface temperature rise of 176°C to 186°C; and the third shot peening pressure is 0.79 MPa to 0.81 MPa, corresponding to a third surface temperature rise of 126°C to 136°C.
[0011] Preferably, the projectile is steel wire cut shot with a diameter of 0.5mm to 0.6mm.
[0012] Preferably, during the hot shot peening process: the temperature data of the workpiece surface is monitored in real time by an infrared thermometer, and the ejection speed of the shot is dynamically adjusted according to the temperature data to keep the workpiece surface temperature within a preset range.
[0013] This invention also provides a kinetic energy conversion gradient thermal shot peening system, comprising: a shot supply module, a shot acceleration and injection module, and a speed control module. The shot supply module supplies shot to the system. The shot acceleration and injection module is connected to the shot supply module and is used to accelerate the shot to a critical ejection velocity and spray it onto different areas of the workpiece. The critical ejection velocity is the minimum velocity at which the kinetic energy of the shot impacting the workpiece is sufficient to be converted into thermal energy to bring the surface of the workpiece to the temperature required for thermal shot peening. The speed control module is connected to the shot acceleration and injection module and is used to control the shot acceleration and injection module so that the shot sprayed onto different areas of the workpiece has different ejection velocities, so that the kinetic energy carried by the shot when it impacts the workpiece is converted into plastic deformation energy and thermal energy of the workpiece surface material. The thermal energy causes different instantaneous temperature rises in different areas of the workpiece. Under the synergistic effect of the plastic deformation energy and thermal energy generated by the kinetic energy conversion, differentiated thermal shot peening is performed on different areas of the workpiece, thereby forming a gradient-distributed residual compressive stress layer in different areas of the workpiece.
[0014] Preferably, the system also includes a temperature monitoring module and a control module. The temperature monitoring module is located near the workpiece and is used to collect real-time temperature data of the workpiece surface. The control module is connected to both the projectile acceleration and injection module and the temperature monitoring module, and is used to adjust the output parameters of the projectile acceleration and injection module in real time based on the temperature data fed back by the temperature monitoring module. The control module includes a parameter storage unit, a feedback receiving unit, and an adjustment unit. The parameter storage unit is used to store preset surface temperature rise target values for different areas of the workpiece. The feedback receiving unit is connected to the temperature monitoring module and is used to receive real-time temperature data of the workpiece surface collected by the temperature monitoring module. The adjustment unit is connected to the feedback receiving unit and is used to dynamically adjust the output parameters of the projectile acceleration and injection module based on the comparison result between the real-time temperature data and the surface temperature rise target value, so as to change the projectile ejection speed.
[0015] Preferably, it also includes a shot recovery and recycling module, which includes a shot recovery unit and a screening unit. The shot recovery unit is used to recover the shot after shot peening, and the screening unit is connected to the shot recovery unit to screen the recovered shot according to the particle size. Shots that meet the particle size requirements are transported to the shot supply module for recycling, and shot that does not meet the particle size requirements are separated and discharged.
[0016] Compared with the prior art, the beneficial effects of the present invention are as follows: The kinetic energy conversion gradient thermal shot peening method provided by the present invention first accelerates the projectile to a critical ejection velocity above the critical ejection velocity, so that the projectile acquires sufficient kinetic energy to generate a thermal effect upon impact. The setting of this critical ejection velocity fully considers the thermophysical parameters of different workpiece materials and the preset thermal shot peening temperature. Based on the correlation model between the projectile velocity and the adiabatic temperature rise of the workpiece surface, the ejection velocity of the projectile is made to just cross the threshold for generating effective thermal energy. Furthermore, the accelerated projectile is sprayed into different areas of the workpiece, and the projectiles sprayed into different areas have different ejection velocities, so that the kinetic energy carried by the projectile when it impacts the workpiece is converted into the plastic deformation energy and thermal energy of the workpiece surface material. This energy conversion occurs in the millisecond instant of the projectile impacting the workpiece, without any thermal inertia delay, and the generation of thermal energy is instantaneous. Simultaneous with plastic deformation, different instantaneous temperature rises can be generated in different areas of the workpiece without any external heat source. Finally, under the synergistic effect of plastic deformation energy and thermal energy generated by kinetic energy conversion, differentiated hot shot peening is carried out on different areas of the workpiece, forming a gradient-distributed residual compressive stress layer in different areas. This fundamentally eliminates the dependence on external heat sources and completely eliminates the problems caused by external heating equipment, such as structural complexity, high manufacturing costs, and temperature control lag due to thermal inertia. At the same time, since the heat is generated instantaneously at the shot impact point and acts on the shot-peened area, the non-shot-peened areas are completely unaffected by heat input, effectively avoiding thermal damage such as unexpected phase transformation and grain coarsening. This significantly improves the fatigue resistance and stress relaxation resistance of the parts, achieving a precise match between the strengthening effect and service requirements. Attached Figure Description
[0017] Figure 1 A flowchart illustrating a kinetic energy conversion gradient thermal shot peening method provided in an embodiment of the present invention; Figure 2 This is a schematic diagram of the thermodynamic synergistic process route of the intermediate shaft of the workpiece in a kinetic energy conversion gradient thermal shot peening method provided by an embodiment of the present invention; Figure 3 This is a schematic diagram of a kinetic energy conversion gradient thermal shot peening system provided in an embodiment of the present invention. Detailed Implementation
[0018] The following detailed description of a specific embodiment of the present invention is provided in conjunction with the accompanying drawings. However, it should be understood that the scope of protection of the present invention is not limited to the specific embodiment.
[0019] In the description of this invention, it should be understood that the terms "center," "longitudinal," "lateral," "length," "width," "thickness," "upper," "lower," "front," "rear," "left," "right," "vertical," "horizontal," "top," "bottom," "inner," "outer," "axial," "radial," and "circumferential" indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are only for the convenience of describing the technical solution of this invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this invention.
[0020] refer to Figure 1 This invention provides a kinetic energy conversion gradient thermal shot peening method, comprising the following steps: accelerating the projectile to a critical ejection velocity or higher, so that the projectile acquires sufficient kinetic energy to generate a thermal effect upon impact, wherein the critical ejection velocity is the minimum velocity at which the kinetic energy of the projectile upon impact with the workpiece is sufficient to be converted into thermal energy to bring the surface layer of the workpiece to the temperature required for thermal shot peening; spraying the accelerated projectile into different areas of the workpiece, wherein the projectiles sprayed into different areas have different ejection velocities, so that the kinetic energy carried by the projectile upon impact with the workpiece is converted into plastic deformation energy and thermal energy of the workpiece surface material, thereby utilizing the thermal energy to cause different instantaneous temperature rises in different areas of the workpiece; under the synergistic effect of the plastic deformation energy and thermal energy generated by the kinetic energy conversion, differential thermal shot peening is performed on different areas of the workpiece, forming a gradient-distributed residual compressive stress layer in different areas of the workpiece.
[0021] In the above embodiments, the kinetic energy conversion gradient thermal shot peening method provided by the present invention first accelerates the projectile to a critical ejection velocity above the critical ejection velocity, enabling the projectile to acquire sufficient kinetic energy to generate a thermal effect upon impact. The setting of this critical ejection velocity fully considers the thermophysical parameters of different workpiece materials and the preset thermal shot peening temperature. Based on the correlation model between the projectile velocity and the adiabatic temperature rise of the workpiece surface, the projectile's ejection velocity is precisely above the threshold for generating effective thermal energy. Furthermore, the accelerated projectile is sprayed into different areas of the workpiece, with projectiles sprayed into different areas having different ejection velocities. This allows the kinetic energy carried by the projectile upon impact to be converted into plastic deformation energy and thermal energy of the workpiece surface material. This energy conversion occurs instantaneously within milliseconds of the projectile impacting the workpiece, without any thermal inertia delay. The generation of thermal energy is simultaneous with plastic deformation. The process is completed in one step, without any external heat source assistance, so that different areas of the workpiece can generate different instantaneous temperature rises. Finally, under the synergistic effect of plastic deformation energy and thermal energy generated by kinetic energy conversion, differentiated hot shot peening is carried out on different areas of the workpiece, forming a gradient-distributed residual compressive stress layer in different areas. This fundamentally eliminates the dependence on external heat sources and completely eliminates the problems caused by external heating equipment, such as structural complexity, high manufacturing costs, and temperature control lag due to thermal inertia. At the same time, since the heat is only generated instantaneously at the shot impact point and acts on the shot-peened area, the non-shot-peened areas are completely unaffected by the heat input, effectively avoiding thermal damage such as unexpected phase transformation and grain coarsening, significantly improving the fatigue resistance and stress relaxation resistance of the parts, and achieving a precise match between the strengthening effect and service requirements.
[0022] Specifically, in this embodiment, the target of shot peening is mainly a hollow, central shaft-shaped workpiece.
[0023] Furthermore, the projectile is accelerated to a critical shot peening velocity of 100 m / s to 250 m / s.
[0024] In the above embodiments, the velocity at which the projectile is accelerated to the critical shot peening point is limited to 100 m / s to 250 m / s. This velocity range is calculated based on the constraint of the tempering temperature of gear parts after heat treatment (150°C to 220°C) and the positive correlation between the kinetic energy of the projectile and the adiabatic temperature rise of the workpiece surface in the principle of energy conservation. Within this velocity range, the heat energy generated when the projectile impacts is just enough to raise the temperature of the workpiece surface to the temperature range required for thermal shot peening. At the same time, it avoids excessive velocity that would cause the temperature rise to exceed the tempering temperature and damage the material matrix properties, thereby ensuring the structural stability of the workpiece material while ensuring the strengthening effect.
[0025] Furthermore, the step of spraying accelerated projectiles into different areas of the workpiece, with the projectiles sprayed into different areas having different ejection velocities, specifically includes: presetting corresponding surface temperature rise target values for different areas of the workpiece; adjusting the shot peening pressure according to the preset surface temperature rise target values to change the ejection velocity of the projectiles, so that the projectiles sprayed into different areas have different impact velocities.
[0026] In the above embodiments, the step of spraying accelerated projectiles into different areas of the workpiece with different ejection velocities is specified as follows: preset corresponding surface temperature rise target values for different areas of the workpiece, and adjust the shot peening pressure according to the preset surface temperature rise target values to change the ejection velocity of the projectiles, so that the projectiles sprayed into different areas have different impact velocities. Thus, the shot peening pressure is used as a control variable to achieve precise control of the projectile ejection velocity and surface temperature rise, providing a quantifiable process adjustment means for the subsequent formation of gradient residual compressive stress layer.
[0027] Table 1. Relationship between shot velocity and surface temperature rise under different shot peening pressures. Shot peening pressure (MPa) Projectile velocity (m / s) Surface temperature rise (°C) 0.8 199 131 0.9 211 142 1.0 223 157 1.1 234 170 1.2 244 181 1.3 254 194 1.4 264 210 1.5 273 221 1.6 282 234 Furthermore, in the gradient control step: a first shot peening zone, a second shot peening zone, and a third shot peening zone are sequentially set along the axial direction of the workpiece; the spray gun is controlled to perform shot peening in the first shot peening zone at a first shot peening pressure to obtain a first surface temperature rise and a first residual compressive stress layer; the spray gun is controlled to perform shot peening in the second shot peening zone at a second shot peening pressure to obtain a second surface temperature rise and a second residual compressive stress layer; the spray gun is controlled to perform shot peening in the third shot peening zone at a third shot peening pressure to obtain a third surface temperature rise and a third residual compressive stress layer; wherein, the first shot peening pressure, the second shot peening pressure, and the third shot peening pressure are different from each other, and the first surface temperature rise, the second surface temperature rise, and the third surface temperature rise correspond to different thermal shot peening temperature ranges.
[0028] In the above embodiments, by sequentially setting the first shot peening zone, the second shot peening zone, and the third shot peening zone along the axial direction of the workpiece, and controlling the shot gun to perform shot peening with different shot peening pressures in each shot peening zone, different surface temperature rises and residual compressive stress layers of different depths are obtained. Thus, a stepped composite reinforcement layer distributed along the axial direction is realized on a single workpiece. The reinforcement degree of each region is precisely matched with the service stress state, which not only avoids the energy waste caused by uniform parameter reinforcement of the whole part, but also prevents negative effects such as stress concentration or surface microcracks that may be caused by over-strengthening.
[0029] Specifically, in this embodiment, the total length of the intermediate shaft is L, and it is divided into three shot peening zones from top to bottom along the axial direction: Stage I, Stage II, and Stage III. The lengths of each zone are L1, L2, and L3, respectively. In this embodiment, L1:L2:L3 = 1:1:1. The division ratio of the three shot peening zones is determined based on the geometry of the workpiece and the stress distribution during service. For shaft parts subjected to combined bending and torsional loads, the stress peak region is usually located in the middle section of the shaft, corresponding to Stage II, where the highest shot peening pressure and temperature rise are applied. The stress lower regions are located at both ends of the shaft, corresponding to Stage I and Stage III, where lower shot peening pressure and temperature rise are applied. The specific length of each zone can be adjusted according to the stress distribution curve of the actual workpiece.
[0030] As shown in Table 1, during the shot peening process, the central controller dynamically adjusts the shot peening pressure and controls the shot injection speed based on the workpiece surface temperature feedback signal, ensuring that the workpiece surface temperature remains within the set range. Figure 2 As shown, the spray gun first moves to the position to perform the thermal shot peening process in stage I, referring to... Figure 2 The first shot peening pressure is 0.09MPa~1.01MPa, and the corresponding first surface temperature rise is 152℃~162℃; the second shot peening pressure is 1.19MPa~1.21MPa, and the corresponding second surface temperature rise is 176℃~186℃; the third shot peening pressure is 0.79MPa~0.81MPa, and the corresponding third surface temperature rise is 126℃~136℃.
[0031] In the above embodiments, by limiting the first shot peening pressure to 0.99MPa~1.01MPa with a corresponding surface temperature rise of 152℃~162℃, the second shot peening pressure to 1.19MPa~1.21MPa with a corresponding surface temperature rise of 176℃~186℃, and the third shot peening pressure to 0.79MPa~0.81MPa with a corresponding surface temperature rise of 126℃~136℃, these three sets of pressure and temperature parameters are optimized process windows obtained through calibration tests based on steel wire shot with a diameter of 0.6mm. The second shot peening zone corresponds to the stress peak area of shaft parts and adopts the highest temperature rise and the deepest strengthening layer, followed by the first shot peening zone, and the third shot peening zone corresponds to the area with lower stress and adopts the lowest temperature rise. This forms an asymmetric gradient distribution that matches the service stress state, and the depth and amplitude of the residual compressive stress layer in each region are controlled within the optimal range.
[0032] Furthermore, the projectile is steel wire cut shot with a diameter of 0.5mm to 0.6mm.
[0033] In the above embodiments, by limiting the projectile to wire cut shot with a diameter of 0.5mm to 0.6mm, this material and diameter range ensure that the projectile has sufficient mass and hardness to generate sufficient plastic deformation energy and heat energy upon impact, while avoiding the deterioration of workpiece surface roughness due to excessively large projectiles or the insufficient kinetic energy due to excessively small projectiles, which would prevent the critical ejection speed requirement from being reached. At the same time, the long cycle life of wire cut shot is beneficial to reducing process costs.
[0034] Furthermore, during the hot shot peening process: the temperature data of the workpiece surface is monitored in real time by an infrared thermometer, and the ejection speed of the shot is dynamically adjusted according to the temperature data to keep the workpiece surface temperature within a preset range.
[0035] In the above embodiments, by using an infrared thermometer to monitor the temperature data of the workpiece surface in real time during the hot shot peening process, and dynamically adjusting the ejection speed of the shot according to the temperature data, the surface temperature of the workpiece is maintained within a preset range. The non-contact measurement characteristics of the infrared thermometer avoid interference with the shot peening process. Combined with millisecond-level pressure regulation, real-time temperature control is achieved, effectively offsetting the temperature rise deviation caused by external factors such as ambient temperature fluctuations, workpiece material differences, or gas source pressure drift. This ensures that the actual temperature of each shot peening area is always within the preset process window, significantly improving the repeatability of the process and the consistency of products during mass production.
[0036] Specifically, the infrared thermometer has a sampling frequency of no less than 100Hz, and the measurement point is focused on the center of the shot impact area to ensure that the measured temperature accurately reflects the instantaneous temperature rise of the shot peening area. The central controller has a preset temperature threshold range (preset value ± 5℃). When the temperature signal fed back by the infrared thermometer is lower than the lower limit of the preset value, the central controller increases the output pressure of the high-pressure gas station through the pressure controller, increasing the shot ejection velocity and increasing the impact heat generation; when the temperature signal is higher than the upper limit of the preset value, the central controller decreases the output pressure of the high-pressure gas station, decreasing the shot ejection velocity and reducing the impact heat generation. The entire control process is completed within milliseconds, ensuring that the temperature of the shot peening area is always maintained within the preset range.
[0037] refer to Figure 3The present invention also provides a kinetic energy conversion gradient thermal shot peening system, comprising: a shot supply module, a shot acceleration and injection module, and a speed control module. The shot supply module is used to supply shot to the system. The shot acceleration and injection module is connected to the shot supply module and is used to accelerate the shot to a critical ejection velocity and spray it to different areas of the workpiece. The critical ejection velocity is the minimum velocity at which the kinetic energy of the shot when it impacts the workpiece is sufficient to be converted into thermal energy to bring the surface of the workpiece to the temperature required for thermal shot peening. The speed control module is connected to the shot acceleration and injection module and is used to control the shot acceleration and injection module so that the shot sprayed to different areas of the workpiece has different ejection velocities, so that the kinetic energy carried by the shot when it impacts the workpiece is converted into plastic deformation energy and thermal energy of the surface material of the workpiece. The thermal energy causes different instantaneous temperature rises in different areas of the workpiece. Under the synergistic effect of the plastic deformation energy and thermal energy generated by the kinetic energy conversion, differentiated thermal shot peening is performed on different areas of the workpiece, thereby forming a gradient-distributed residual compressive stress layer in different areas of the workpiece.
[0038] In the above embodiments, a shot supply module continuously supplies shot to the system, ensuring a sufficient supply of shot during shot peening, thus providing a material basis for continuous operation. A shot acceleration and injection module accelerates the shot to above the critical ejection velocity and injects it into different areas of the workpiece. This critical ejection velocity is the minimum speed at which the kinetic energy of the shot impacting the workpiece is sufficient to be converted into thermal energy to bring the workpiece surface to the temperature required for thermal peening. This ensures that the shot just exceeds the energy threshold for generating effective thermal energy at the moment of impact. A speed control module controls the shot acceleration and injection module, allowing shot to be injected into different areas of the workpiece with different ejection velocities. This converts the kinetic energy carried by the shot upon impact into the plastic deformation energy and thermal energy of the workpiece surface material. This thermal energy causes different instantaneous temperature rises in different areas of the workpiece. The synergistic effect of the plastic deformation energy and thermal energy generated by the kinetic energy conversion... Differential hot shot peening is applied to different areas of the workpiece to form a gradient residual compressive stress layer in different areas of the workpiece. The three functional modules mentioned above are connected in sequence and work together to realize a complete process chain of shot supply, ultra-high speed acceleration spraying, speed differentiation control and gradient hot shot peening without relying on any external heat source. Since the heat is only generated instantaneously at the shot impact point and acts on the shot-peened area, the non-shot-peened area is completely unaffected by the heat input, which fundamentally eliminates the defects of complex structure and high manufacturing cost caused by external heating equipment. At the same time, the speed control module directly controls the shot acceleration spraying module to differentiate the ejection speed. The controllable distribution of gradient residual compressive stress layer can be achieved without complex multi-actuator collaborative control. The structure is simple and compact and is suitable for surface strengthening treatment of various metal parts such as gears, shafts, and blades that are subjected to alternating loads.
[0039] Further, refer to Figure 3It also includes a temperature monitoring module and a control module. The temperature monitoring module is located near the workpiece and is used to collect the temperature data of the workpiece surface in real time. The control module is connected to both the shot acceleration and injection module and the temperature monitoring module. It is used to adjust the output parameters of the shot acceleration and injection module in real time based on the temperature data fed back by the temperature monitoring module. The control module includes a parameter storage unit, a feedback receiving unit, and an adjustment unit. The parameter storage unit is used to store preset surface temperature rise target values for different areas of the workpiece. The feedback receiving unit is connected to the temperature monitoring module and is used to receive the real-time temperature data of the workpiece surface collected by the temperature monitoring module. The adjustment unit is connected to the feedback receiving unit and is used to dynamically adjust the output parameters of the shot acceleration and injection module to change the ejection speed of the shot based on the comparison result between the real-time temperature data and the surface temperature rise target value.
[0040] In the above embodiments, a temperature monitoring module is set to collect the temperature data of the workpiece surface in real time, and a control module is set to adjust the output parameters of the projectile acceleration and injection module in real time based on the temperature data fed back by the temperature monitoring module. The control module specifically includes a parameter storage unit, a feedback receiving unit, and an adjustment unit. The parameter storage unit stores preset surface temperature rise target values for different areas of the workpiece. The feedback receiving unit receives the real-time temperature data of the workpiece surface collected by the temperature monitoring module. The adjustment unit dynamically adjusts the output parameters of the projectile acceleration and injection module to change the projectile's ejection velocity based on the comparison between the real-time temperature data and the surface temperature rise target values. Thus, based on the speed differentiation control achieved in embodiment 8... Furthermore, a complete closed-loop control loop of "preset target value storage - real-time temperature feedback - dynamic deviation comparison - execution parameter adjustment" was constructed, enabling the shot ejection velocity of each shot peening area to be autonomously adjusted in real time according to the actual temperature rise. This effectively offsets the temperature rise deviation caused by external factors such as ambient temperature fluctuations, gas source pressure drift, or changes in equipment status during continuous operation, ensuring that the actual temperature of each area is always within the preset process window. This significantly improves the repeatability of the gradient thermal shot peening process and the product consistency during mass production. At the same time, this closed-loop control does not require additional complex hardware structures and can be achieved simply through the collaborative work of the units within the control module, reducing the overall manufacturing cost and control complexity of the equipment.
[0041] Further, refer to Figure 3 It also includes a shot recovery and recycling module, which includes a shot recovery unit and a screening unit. The shot recovery unit is used to recover the shot after shot peening. The screening unit is connected to the shot recovery unit and is used to screen the recovered shot according to the particle size. Shots that meet the particle size requirements are transported to the shot supply module for recycling, and shot that does not meet the particle size requirements are separated and discharged.
[0042] In the above embodiments, the shot recovery and circulation module includes a shot recovery unit and a screening unit. The shot recovery unit recovers the shot after shot peening and transports it to the screening unit. The screening unit screens the recovered shot according to its particle size, transports the shot that meets the particle size requirements to the shot supply module for recycling, and separates and discharges the shot that does not meet the particle size requirements. This realizes the automatic recovery, screening and circulation supply of shot, ensuring the consistency of shot size and the stability of impact kinetic energy during shot peening. At the same time, it avoids broken shot from being mixed into the shot peening flow and causing damage to the workpiece surface, thus ensuring the continuous and stable operation of the gradient thermal shot peening process.
[0043] After shot peening, the shot, along with broken shot fragments and metal dust detached from the workpiece surface, falls into the bottom hopper of the equipment. A shot recovery pipe connects to the bottom of the hopper, and the recovery pipe contains an lifting device (such as a bucket elevator or pneumatic conveyor) to transport the recovered mixture to the shot screening screen. The shot screening screen uses a graded screen structure with a mesh size smaller than the shot diameter (0.50mm in this embodiment). The oversize material (shot with a particle size ≥ 0.50mm) falls into the shot chamber for recycling, while the undersize material (broken shot fragments and metal dust) enters the waste hopper for periodic discharge.
[0044] Regarding increasing the projectile ejection velocity, this embodiment proposes that, firstly, due to the influence of gear tempering stability, the surface heating temperature of the workpiece should not exceed the gear heat treatment tempering temperature, generally 150℃~220℃. Within this temperature range, the required projectile ejection velocity is relatively low, at 100m / s~250m / s. Secondly, the air compressor station used in this system has an upper pressure output limit of 1.6MPa, higher than conventional air compressor stations, to increase the projectile ejection velocity. The spray gun nozzle at the projectile ejection position is a high-pressure nozzle, and its unique internal structure further enhances the projectile ejection velocity. Through these designs, the critical ejection velocity required by the system is met.
[0045] The above-disclosed embodiments are merely a few specific examples of the present invention. However, the embodiments of the present invention are not limited thereto, and any variations that can be conceived by those skilled in the art should fall within the protection scope of the present invention.
Claims
1. A kinetic energy conversion gradient thermal shot peening method, characterized in that, Includes the following steps: The projectile is accelerated to a critical ejection velocity or higher, so that the projectile has enough kinetic energy to produce a thermal effect upon impact. The critical ejection velocity is the minimum velocity at which the kinetic energy of the projectile is sufficient to be converted into thermal energy to bring the surface of the workpiece to the temperature required for shot peening. The accelerated projectile is sprayed into different areas of the workpiece, and the projectiles sprayed into the different areas have different ejection velocities. When the projectile hits the workpiece, the kinetic energy it carries is converted into the plastic deformation energy and thermal energy of the workpiece surface material. The thermal energy is used to cause different instantaneous temperature rises in different areas of the workpiece. Under the synergistic effect of the plastic deformation energy and thermal energy generated by the kinetic energy conversion, differentiated hot shot peening is performed on different regions of the workpiece to form a gradient-distributed residual compressive stress layer in different regions of the workpiece.
2. The kinetic energy conversion gradient thermal shot peening method as described in claim 1, characterized in that, The projectile is accelerated to the critical velocity for shot peening, which is 100 m / s to 250 m / s.
3. The kinetic energy conversion gradient thermal shot peening method as described in claim 1, characterized in that, The step of propelling the accelerated projectile into different areas of the workpiece, wherein the projectiles propelled into the different areas have different ejection velocities, specifically includes: Preset corresponding surface temperature rise target values for different areas of the workpiece; Based on the preset target surface temperature rise value, the shot peening pressure is adjusted to change the ejection velocity of the projectile, so that the projectiles ejected into the different areas have different impact velocities.
4. The kinetic energy conversion gradient thermal shot peening method as described in claim 3, characterized in that, In the gradient control step: A first shot peening zone, a second shot peening zone, and a third shot peening zone are sequentially set along the axial direction of the workpiece; The spray gun is controlled to perform shot peening in the first shot peening area at the first shot peening pressure to obtain the first surface temperature rise and the first residual compressive stress layer. The spray gun is controlled to perform shot peening in the second shot peening zone at the second shot peening pressure to obtain a second surface temperature rise and a second residual compressive stress layer. The spray gun is controlled to perform shot peening in the third shot peening zone at a third shot peening pressure to obtain a third surface temperature rise and a third residual compressive stress layer. The first shot peening pressure, the second shot peening pressure, and the third shot peening pressure are different from each other, and the first surface temperature rise, the second surface temperature rise, and the third surface temperature rise correspond to different thermal shot peening temperature ranges.
5. The kinetic energy conversion gradient thermal shot peening method as described in claim 4, characterized in that, The first shot peening pressure is 0.09MPa~1.01MPa, and the corresponding temperature rise of the first surface is 152℃~162℃; The second shot peening pressure is 1.19 MPa to 1.21 MPa, and the corresponding temperature rise of the second surface is 176°C to 186°C. The third shot peening pressure is 0.79MPa~0.81MPa, and the corresponding temperature rise of the third surface is 126℃~136℃.
6. The kinetic energy conversion gradient thermal shot peening method as described in claim 5, characterized in that, The projectile is steel wire cut shot with a diameter of 0.5mm to 0.6mm.
7. The kinetic energy conversion gradient thermal shot peening method as described in claim 5, characterized in that, During hot shot peening: The surface temperature of the workpiece is monitored in real time by an infrared thermometer, and the ejection speed of the projectile is dynamically adjusted according to the temperature data to keep the surface temperature of the workpiece within a preset range.
8. A kinetic energy conversion gradient thermal shot peening system, characterized in that, include: The projectile supply module is used to supply projectiles to the system; The projectile acceleration and injection module is connected to the projectile supply module and is used to accelerate the projectile to a critical ejection speed and eject it to different areas of the workpiece. The critical ejection speed is the minimum speed at which the kinetic energy of the projectile when it hits the workpiece is sufficient to be converted into thermal energy that brings the surface of the workpiece to the temperature required for thermal peening. A speed control module, connected to the projectile acceleration and spraying module, is used to control the projectile acceleration and spraying module so that the projectiles sprayed into different areas of the workpiece have different ejection velocities. This allows the kinetic energy carried by the projectiles when they impact the workpiece to be converted into plastic deformation energy and thermal energy of the workpiece surface material. The thermal energy causes different instantaneous temperature rises in different areas of the workpiece. Under the synergistic effect of the plastic deformation energy and thermal energy generated by the kinetic energy conversion, differentiated hot shot peening is performed on different areas of the workpiece, thereby forming a gradient-distributed residual compressive stress layer in different areas of the workpiece.
9. The kinetic energy conversion gradient thermal shot peening method and system as described in claim 8, characterized in that, It also includes a temperature monitoring module and a control module. The temperature monitoring module is located near the workpiece and is used to collect the temperature data of the workpiece surface in real time. The control module is connected to both the projectile acceleration and injection module and the temperature monitoring module, and is used to adjust the output parameters of the projectile acceleration and injection module in real time based on the temperature data fed back by the temperature monitoring module. The control module includes: A parameter storage unit is used to store preset surface temperature rise target values for different areas of the workpiece; A feedback receiving unit is connected to the temperature monitoring module and is used to receive real-time temperature data of the workpiece surface collected by the temperature monitoring module. An adjustment unit, connected to the feedback receiving unit, is used to dynamically adjust the output parameters of the projectile acceleration injection module based on the comparison result between the real-time temperature data and the target value of the surface temperature rise, so as to change the ejection velocity of the projectile.
10. The kinetic energy conversion gradient thermal shot peening method and system as described in claim 8, characterized in that, It also includes a projectile recovery and recycling module, which includes: The shot recovery unit is used to recover the shot after shot peening; The screening unit, connected to the shot recovery unit, is used to screen the recovered shot according to its particle size, transport the shot that meets the particle size requirements to the shot supply module for recycling, and separate and discharge the shot that does not meet the particle size requirements.