A method for preparing cold-rolled high-quality carbon structural steel plate 25

By optimizing the processes of molten iron pretreatment, converter smelting, LF refining, continuous casting, and cold rolling, the problems of compositional fluctuation and microstructure inhomogeneity of 25 steel cold-rolled plates were solved, achieving a balance between high strength and good plasticity, and obtaining high-quality cold-rolled carbon structural steel 25 steel plates with high surface quality.

CN123108252APending Publication Date: 2026-11-17XINJIANG BAYI IRON & STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611260113.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-19
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

The existing production process for 25 steel cold-rolled plates has large fluctuations in composition and poor consistency in mechanical properties. Continuous casting billets are prone to center segregation and corner cracks. Hot rolling coiling temperature control is inaccurate, making it difficult to obtain both high strength and good plasticity at the same time.

Method used

By controlling the process steps of molten iron pretreatment, converter smelting, LF refining, continuous casting, hot rolling and cold rolling, including argon-protected casting throughout the process, constant casting speed, low-pressure sparse cooling, bell-type annealing and staged hydrogen blowing treatment, the chemical composition and microstructure uniformity are optimized. Combined with the cold rolling reduction and annealing process, a balance between high strength and good plasticity of the finished product is achieved.

Benefits of technology

It achieves narrow-range control of chemical composition, suppresses central segregation and corner cracks, obtains a uniform and fine microstructure, and the finished product has a tensile strength of ≥400MPa and an elongation at break of ≥24%, with excellent surface quality.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention belongs to the field of iron and steel metallurgy technology, specifically disclosing a method for preparing cold-rolled high-quality carbon structural steel 25 steel plates. The method includes hot metal pretreatment, converter smelting, LF refining, slab continuous casting, hot rolling, cold rolling, bell-type annealing, leveling, and recoiling with oil. The hot metal is subject to strict control of sulfur and phosphorus content; the converter limits the number of reblowing cycles and controls phosphorus return through slag blocking; the LF ensures sufficient soft blowing and white slag settling time; continuous casting is protected by argon gas throughout and uses low superheat constant casting speed; hot rolling controls heating, final rolling, and coiling temperatures and slab crown; cold rolling uses fixed raw material thickness to match the reduction amount; bell-type annealing involves segmented temperature control and staged hydrogen blowing to promote grain homogenization; leveling uses an elongation model; and finally, a light oil coating is applied for protection. This invention addresses the problems of large fluctuations in composition, numerous defects in cast slabs, and difficulty in matching strength and plasticity in existing processes. It narrowly controls harmful elements, improves the microstructure of the cast slab and hot-rolled slabs, and synergistically balances performance with the cold rolling and annealing process, resulting in improved tensile strength and elongation after fracture in the finished product.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of iron and steel metallurgy technology, specifically to a method for preparing cold-rolled high-quality carbon structural steel plate 25. Background Technology

[0002] 25 steel, a high-quality carbon structural steel, is a medium-carbon steel with high strength, good plasticity, and toughness. It is widely used in the manufacture of various structural components, mechanical parts, and stamped parts. Cold-rolled 25 steel sheets and strips are also widely used in automobile manufacturing, machining, and light industrial products due to their good surface quality, high dimensional accuracy, and stable mechanical properties.

[0003] However, in the existing production process of 25 steel cold-rolled sheet, on the one hand, the composition fluctuates greatly during the steelmaking process, especially the carbon and sulfur content is unstable, resulting in poor consistency of the mechanical properties of the product; on the other hand, the continuously cast billet is prone to center segregation and corner cracks, affecting the subsequent rolling yield; in addition, the hot rolling coiling temperature control precision is insufficient, resulting in poor uniformity of strip structure, large fluctuations in mechanical properties after cold rolling, and unreasonable matching of hot rolling annealing process parameters, making it difficult to achieve a balance between high strength and good plasticity at the same time. Summary of the Invention

[0004] The purpose of this invention is to provide a method for preparing high-quality cold-rolled carbon structural steel 25 steel plate, in order to solve the problems of large fluctuations in composition, poor performance consistency, easy occurrence of center segregation and corner cracks in cast billets, and insufficient control precision of hot rolling and hot rolling process parameters in existing processes.

[0005] To achieve the above objectives, the basic solution provided by this invention is: a method for preparing cold-rolled high-quality carbon structural steel plate 25, comprising the following steps: S1. Hot metal pretreatment: Control the original hot metal composition: [Si]≤0.80%, [P]≤0.120%, [S]≤0.06%, hot metal temperature≥1280℃; when the hot metal [S]≥0.045%, desulfurization treatment is carried out, and the hot metal entering the converter [S] is controlled to ≤0.008%. The slag must be removed after the hot metal is desulfurized. S2. Converter smelting: A 120t converter is used for smelting. The number of converter reblowing times is controlled to not exceed 2. The tapping time is controlled to be 3.5-6 minutes. Slag-blocking tapping is adopted, and slag detection is combined with sliding plate slag blocking. Red-broom tapping is used to control the phosphorus return of molten steel in the ladle to ≤0.003%. S3, LF Refining: The molten steel is subjected to LF refining treatment, and the soft blowing time is controlled to be no less than 10 minutes, the calming time is no less than 5 minutes, and the white slag time is no less than 10 minutes. No aluminum or iron shall be added after the LF leaves the station. S4. Slab continuous casting: Argon gas is used for the entire casting process. The liquidus temperature is 1511℃ and the solidus temperature is 1457℃. The casting speed of the slab is controlled at 0.8~1.4m / min. Constant casting speed is used. The liquid level fluctuation in the crystallizer is controlled within ±5mm. The slab straightening temperature is not less than 900℃. The number of consecutive heats in the tundish is not more than 12. Slag is removed at least once every 4 to 5 heats. The segregation at the center of the slab is not greater than 2.5. S5. Hot rolling: The continuously cast slab is heated to 1150~1210℃ and rolled by a 1750mm hot continuous rolling mill. The final rolling temperature is controlled at 870±20℃. The front-end low-pressure sparse cooling mode is adopted, and the coiling temperature is controlled at 680±20℃. The descaling pressure is guaranteed to be above 18.5MPa. The crown is controlled according to the thickness of the hot-rolled raw material plate. S6. Cold rolling: After pickling, the hot-rolled raw material coil is rolled on a cold rolling mill. The raw material thickness is 3.5mm, the product thickness is 1.6~1.8mm, the reduction is 49%~52%, the necking is 1mm, the rolling speed is controlled at 100~300m / min, and the surface roughness of the No. 5 work roll of the last stand is required to be 1.5±5%μm. S7. Bell-type annealing: Annealing is carried out in a bell-type annealing furnace. The annealing temperature is controlled at 660±10℃, the heating time is 9~11h, the high temperature holding time is 8~9.5h, the waiting time is 4h, the furnace exit temperature is controlled at 100±5℃, and after the heating temperature rises to 430℃, the heating rate is controlled at 30~50℃ / h. The hydrogen blowing amount is controlled in stages during the annealing process. S8. Leveling: Leveling is performed using the elongation rate model. The target leveling rate is 1.0%, with a control range of 0.9% to 1.1%. The rolling pressure is controlled according to the thickness of the finished product. S9. Rewinding and Oiling: The leveled steel strip is rewinded and oiled, with a light oiling application of 0.6–1.1 g / m. 2 .

[0006] The beneficial effects of this invention are as follows: By controlling the pretreatment of molten iron, the endpoint control of the converter, and the LF refining process, a narrow range of control over the chemical composition of 25 steel is achieved, especially controlling the S content to ≤0.005% and the P content to ≤0.015%, effectively reducing the adverse effects of harmful elements on mechanical properties; argon-protected casting throughout the continuous casting process, carbon-free protective slag, strict superheat control, and constant casting speed (0.8~1.4m / min) effectively suppress the generation of slab center segregation and corner cracks, with slab center segregation controlled within 2.5 grade; hot rolling adopts a low-pressure sparse cooling mode in the front stage, combined with a final rolling temperature of 870±20℃ and a coiling temperature of 680±20℃. By controlling the temperature, a uniform and fine hot-rolled microstructure was obtained, providing a good raw material microstructure basis for subsequent cold rolling. The cold rolling annealing process, through the synergistic combination of controlling the cold rolling reduction (49%~52%) and the bell-type annealing process (660±10℃, holding for 9~10h), combined with a staged hydrogen blowing system, effectively promoted recrystallization and grain homogenization, enabling the finished product to simultaneously obtain a tensile strength of ≥400MPa and an elongation at break of ≥24%, achieving a balance between high strength and good plasticity. By controlling the emulsion parameters, rolling speed, annealing atmosphere, and leveling process, the surface reflectivity of the finished product is ≥60%, and the surface roughness is controlled within 0.7~1.1μm, meeting the requirements for high surface quality.

[0007] Option 2, which is the preferred option of the basic option, in S2, the endpoint components are controlled as follows: [C]≥0.06%, [P]≤0.018%, [S]≤0.030%.

[0008] Option 3, which is the preferred option of the basic option, involves deoxidizing and alloying a composite deoxidizer, aluminum-iron, and silicon-manganese alloy, which are added in order of increasing deoxidation capacity. The silicon-manganese alloy and aluminum-iron are added when the steel is 1 / 3 to 1 / 2 of the way through the tapping process.

[0009] Option 4 is the preferred option of the basic option. In S4, carbon-free protective slag and carbon-free ladle covering agent are used. The water content (H2O) of the protective slag and covering agent is ≤0.5%. The superheat of the tundish in the first continuous casting furnace is controlled to be ≤40℃, and the superheat of the tundish in the continuous casting furnace is ≤30℃.

[0010] Option 5, which is the preferred option of the basic option, is as follows: when the thickness of the hot-rolled raw material plate is ≤2.2mm, the crown is ≤50μm; when the thickness of the raw material plate is >2.2mm, the crown is ≤60μm; and the wedge shape shall not exceed the crown.

[0011] Option 6, which is the preferred option of the basic option, involves controlling the hydrogen blowing rate in stages during the annealing process in S7 as follows: First stage: heating time 1 hour, hydrogen blowing flow rate 10 m³ / h. 3 / h; Second stage: Heating time is 4-6 hours, hydrogen blowing flow rate is 20-25 m³ / h; 3 / h; Third stage: heating time 3h, hydrogen blowing flow rate 10-20m³ / h; 3 / h; Fourth stage: Heating time 2h, hydrogen blowing flow rate 8m 3 / h.

[0012] Option 7 is the preferred option of the basic option. In S8, the rolling pressure is controlled according to the specific control method of the finished product thickness as follows: when the finished product thickness is 1.6 to 1.7 mm, the rolling force is set to 2000 kN with fluctuation of less than 500 kN; when the finished product thickness is 1.6 to 1.7 mm, the rolling force is set to 2300 kN with fluctuation of less than 500 kN; and the surface roughness is 0.7-1.1 μm.

[0013] Option 8 is an optimal choice of the basic option, which controls the tensile strength of the finished 25 steel plate to be ≥400MPa and the elongation after fracture to be ≥24%. Detailed Implementation

[0014] The present invention will be further described in detail below through specific embodiments: Example 1

[0015] A method for preparing cold-rolled high-quality carbon structural steel plate 25 includes the following steps: S1. Hot metal pretreatment: Control the original hot metal composition: [Si]≤0.80%, [P]≤0.120%, [S]≤0.06%, hot metal temperature≥1280℃; when the hot metal [S]≥0.045%, desulfurization treatment is carried out, and the hot metal entering the converter [S] is controlled to ≤0.008%. The slag must be removed after the hot metal is desulfurized. S2. Converter smelting: A 120t converter is used for smelting. The number of converter reblowing times is controlled to be no more than 2. The final composition is controlled as follows: [C]≥0.06%, [P]≤0.018%, [S]≤0.030%. The tapping time is controlled to be 3.5-6min. Slag-blocking tapping is adopted, and slag detection is combined with sliding plate slag blocking. Red-bomb tapping is used to control the phosphorus return of molten steel in the ladle to be ≤0.003%. Deoxidation and alloying are carried out using composite deoxidizer, aluminum-iron, and silicon-manganese alloy, which are added in order of deoxidation capacity from weakest to strongest. Silicon-manganese alloy and aluminum-iron are added when the steel is 1 / 3 to 1 / 2 tapped. S3, LF Refining: The molten steel is subjected to LF refining treatment, and the soft blowing time is controlled to be no less than 10 minutes, the calming time is no less than 5 minutes, and the white slag time is no less than 10 minutes. No aluminum or iron shall be added after the LF leaves the station. S4. Slab continuous casting: Argon gas is used for the entire casting process. The liquidus temperature is 1511℃ and the solidus temperature is 1457℃. The slab casting speed is controlled at 0.8~1.4m / min. Constant casting speed is used. The liquid level fluctuation in the crystallizer is controlled within ±5mm. The slab straightening temperature is not less than 900℃. The number of tundish heats cast in the tundish is not more than 12. Slag is removed at least once every 4 to 5 heats. The center segregation of the slab is not greater than 2.5 grade. Carbon-free protective slag and carbon-free ladle covering agent are used. The water content (H2O) of the protective slag and covering agent is ≤0.5%. The superheat of the tundish in the first heat of continuous casting is controlled at ≤40℃, and the superheat of the tundish in the continuous casting furnace is controlled at ≤30℃. S5. Hot Rolling: The continuously cast slab is heated to 1150~1210℃ and rolled by a 1750mm hot continuous rolling mill. The final rolling temperature is controlled at 870±20℃. A low-pressure sparse cooling mode is adopted in the front section, and the coiling temperature is controlled at 680±20℃. The descaling pressure is guaranteed to be above 18.5MPa. The crown is controlled according to the thickness of the hot-rolled raw material plate. The specific crown control method according to the thickness of the hot-rolled raw material plate is as follows: when the thickness of the raw material plate is ≤2.2mm, the crown is ≤50μm; when the thickness of the raw material plate is >2.2mm, the crown is ≤60μm. The wedge shape shall not be greater than the crown. S6. Cold rolling: After pickling, the hot-rolled raw material coil is rolled on a cold rolling mill. The raw material thickness is 3.5mm, the product thickness is 1.6~1.8mm, the reduction is 49%~52%, the necking is 1mm, the rolling speed is controlled at 100~300m / min, and the surface roughness of the No. 5 work roll of the last stand is required to be 1.5±5%μm. S7. Bell-type annealing: Annealing is performed using a bell-type annealing furnace. The annealing temperature is controlled at 660±10℃, the heating time is 9-11 hours, the high-temperature holding time is 8-9.5 hours, the waiting time under the bell is 4 hours, and the furnace exit temperature is controlled at 100±5℃. After the heating temperature reaches 430℃, the heating rate is controlled at 30-50℃ / h. The hydrogen blowing rate is controlled in stages during the annealing process. The specific method for controlling the hydrogen blowing rate in stages during the annealing process is as follows: First stage: heating time 1 hour, hydrogen blowing flow rate 10 m³ / h. 3 / h; Second stage: Heating time is 4-6 hours, hydrogen blowing flow rate is 20-25 m³ / h; 3 / h; Third stage: heating time 3h, hydrogen blowing flow rate 10-20m³ / h; 3 / h; Fourth stage: Heating time 2h, hydrogen blowing flow rate 8m 3 / h; S8. Leveling: Leveling is performed using the elongation rate mode. The target leveling rate is 1.0%, with a control range of 0.9% to 1.1%. The rolling pressure is controlled according to the finished product thickness. The specific control method for the rolling pressure based on the finished product thickness is as follows: when the finished product thickness is 1.6 to 1.7 mm, the rolling force is set at 2000 kN with a fluctuation of less than 500 kN; when the finished product thickness is 1.6 to 1.7 mm, the rolling force is set at 2300 kN with a fluctuation of less than 500 kN; and the surface roughness is 0.7-1.1 μm. S9. Rewinding and Oiling: The leveled steel strip is rewinded and oiled, with a light oiling application of 0.6–1.1 g / m. 2 The tensile strength of the finished 25 steel plate should be ≥400MPa and the elongation after fracture should be ≥24%.

[0016] Example 2

[0017] A method for preparing cold-rolled high-quality carbon structural steel plate 25 includes the following steps: S1. Hot metal pretreatment: Original hot metal [Si]: 0.65%, [P]: 0.085%, [S]: 0.052%, hot metal temperature 1310℃, after desulfurization treatment, hot metal entering the converter [S]: 0.006%; S2, Converter smelting: Endpoint [C]: 0.08%, [P]: 0.012%, [S]: 0.018%, tapping time 4.5 min, phosphorus recovery 0.002%; S3, LF refining: Soft blowing time 12min, calming time 6min, white residue time 12min; S4, Continuous casting: First furnace tundish superheat 38℃, continuous casting furnace tundish superheat 28℃, casting speed 1.2m / min, crystallizer liquid level fluctuation ±3mm, slab straightening temperature 950℃; S5. Hot rolling: heating temperature 1180℃, final rolling temperature 875℃, coiling temperature 685℃, descaling pressure 19.5MPa; S6, Cold Rolling: Raw material plate thickness 3.5mm, finished plate thickness 1.7mm, reduction 51.4%, rolling speed 180m / min; S7. Bell-type annealing: Annealing temperature 660℃, heating time 10h, holding time 8.5h, furnace exit temperature 100℃. S8. Leveling: Leveling rate 1.0%, rolling pressure 2500kN; S9. Finished product mechanical properties: tensile strength 425MPa, elongation after fracture 36%.

[0018] Example 3

[0019] A method for preparing cold-rolled high-quality carbon structural steel plate 25 includes the following steps: S1. Hot metal pretreatment: Original hot metal [Si]: 0.72%, [P]: 0.098%, [S]: 0.048%, hot metal temperature 1295℃, after desulfurization treatment, hot metal entering the converter [S]: 0.005%; S2, Converter smelting: Endpoint [C]: 0.07%, [P]: 0.015%, [S]: 0.020%, tapping time 5.0 min, phosphorus recovery 0.002%; S3, LF refining: soft blowing time 15min, calming time 8min, white residue time 14min; S4, Continuous casting: First furnace tundish superheat 36℃, continuous casting furnace tundish superheat 26℃, casting speed 1.1m / min, crystallizer liquid level fluctuation ±4mm, slab straightening temperature 920℃; S5. Hot rolling: Heating temperature 1190℃, final rolling temperature 868℃, coiling temperature 672℃, descaling pressure 19.2MPa; S6, Cold rolling: Raw material plate thickness 3.5mm, finished plate thickness 1.6mm, reduction 54.3%, rolling speed 200m / min; S7. Bell-type annealing: annealing temperature 655℃, heating time 10.5h, holding time 9h, furnace exit temperature 98℃; S8, Leveling: Leveling rate 1.1%, rolling pressure 2800kN; S9. Finished product mechanical properties: tensile strength 438MPa, elongation after fracture 35%.

[0020] Example 4

[0021] A method for preparing cold-rolled high-quality carbon structural steel plate 25 includes the following steps: S1. Hot metal pretreatment: Original hot metal [Si]: 0.58%, [P]: 0.076%, [S]: 0.055%, hot metal temperature 1320℃, after desulfurization treatment, hot metal entering the converter [S]: 0.007%; S2, Converter smelting: Endpoint [C]: 0.09%, [P]: 0.010%, [S]: 0.015%, tapping time 4.0 min, phosphorus recovery 0.0015%; S3, LF refining: Soft blowing time 11min, calming time 7min, white residue time 11min; S4, Continuous casting: First furnace tundish superheat 39℃, continuous casting furnace tundish superheat 27℃, casting speed 1.3m / min, crystallizer liquid level fluctuation ±2mm, slab straightening temperature 960℃; S5. Hot rolling: heating temperature 1170℃, final rolling temperature 882℃, coiling temperature 690℃, descaling pressure 20.0MPa; S6, Cold Rolling: Raw material plate thickness 3.5mm, finished plate thickness 1.8mm, reduction 48.6%, rolling speed 160m / min; S7. Bell-type annealing: Annealing temperature 665℃, heating time 9.5h, holding time 10h, furnace exit temperature 102℃; S8, Leveling: Leveling rate 1.05%, rolling pressure 2200kN; S9. Finished product mechanical properties: tensile strength 412MPa, elongation after fracture 37%.

[0022] The above descriptions are merely embodiments of the present invention, and common knowledge regarding specific structures and characteristics is not elaborated upon here. It should be noted that those skilled in the art can make various modifications and improvements without departing from the structure of the present invention, and these should also be considered within the scope of protection of the present invention. These modifications and improvements will not affect the effectiveness of the present invention or the practicality of the patent. The scope of protection claimed in this application should be determined by the content of its claims, and the specific embodiments described in the specification can be used to interpret the content of the claims.

Claims

1. A method for preparing cold-rolled high-quality carbon structural steel plate 25, characterized in that, Includes the following steps: S1. Hot metal pretreatment: Control the original hot metal composition: [Si]≤0.80%, [P]≤0.120%, [S]≤0.06%, hot metal temperature≥1280℃; when the hot metal [S]≥0.045%, desulfurization treatment is carried out, and the hot metal entering the converter [S] is controlled to ≤0.008%. The slag must be removed after the hot metal is desulfurized. S2. Converter smelting: A 120t converter is used for smelting. The number of converter reblowing times is controlled to not exceed 2. The tapping time is controlled to be 3.5-6 minutes. Slag-blocking tapping is adopted, and slag detection is combined with sliding plate slag blocking. Red-broom tapping is used to control the phosphorus return of molten steel in the ladle to ≤0.003%. S3, LF Refining: The molten steel is subjected to LF refining treatment, and the soft blowing time is controlled to be no less than 10 minutes, the calming time is no less than 5 minutes, and the white slag time is no less than 10 minutes. No aluminum or iron shall be added after the LF leaves the station. S4. Slab continuous casting: Argon gas is used for the entire casting process. The liquidus temperature is 1511℃ and the solidus temperature is 1457℃. The casting speed of the slab is controlled at 0.8~1.4m / min. Constant casting speed is used. The liquid level fluctuation in the crystallizer is controlled within ±5mm. The slab straightening temperature is not less than 900℃. The number of consecutive heats in the tundish is not more than 12. Slag is removed at least once every 4 to 5 heats. The segregation at the center of the slab is not greater than 2.

5. S5. Hot rolling: The continuously cast slab is heated to 1150~1210℃ and rolled by a 1750mm hot continuous rolling mill. The final rolling temperature is controlled at 870±20℃. The front-end low-pressure sparse cooling mode is adopted, and the coiling temperature is controlled at 680±20℃. The descaling pressure is guaranteed to be above 18.5MPa. The crown is controlled according to the thickness of the hot-rolled raw material plate. S6. Cold rolling: After pickling, the hot-rolled raw material coil is rolled on a cold rolling mill. The raw material thickness is 3.5mm, the product thickness is 1.6~1.8mm, the reduction is 49%~52%, the necking is 1mm, the rolling speed is controlled at 100~300m / min, and the surface roughness of the No. 5 work roll of the last stand is required to be 1.5±5%μm. S7. Bell-type annealing: Annealing is carried out in a bell-type annealing furnace. The annealing temperature is controlled at 660±10℃, the heating time is 9~11h, the high temperature holding time is 8~9.5h, the waiting time is 4h, the furnace exit temperature is controlled at 100±5℃, and after the heating temperature rises to 430℃, the heating rate is controlled at 30~50℃ / h. The hydrogen blowing amount is controlled in stages during the annealing process. S8. Leveling: Leveling is performed using the elongation rate model. The target leveling rate is 1.0%, with a control range of 0.9% to 1.1%. The rolling pressure is controlled according to the thickness of the finished product. S9. Rewinding and Oiling: The leveled steel strip is rewinded and oiled, with a light oiling application of 0.6–1.1 g / m. 2 .

2. The method for preparing a cold-rolled high-quality carbon structural steel plate (25) according to claim 1, characterized in that, In S2, the endpoint component control is: [C] ≥ 0.06%, [P] ≤ 0.018%, [S] ≤ 0.030%.

3. The method for preparing a cold-rolled high-quality carbon structural steel plate (25) according to claim 1, characterized in that, In S2, deoxidation alloying uses a composite deoxidizer, aluminum-iron, and silicon-manganese alloy, which are added in order of increasing deoxidation capacity. The silicon-manganese alloy and aluminum-iron are added when the steel is 1 / 3 to 1 / 2 tapped.

4. The method for preparing a cold-rolled high-quality carbon structural steel plate 25 according to claim 1, characterized in that, In S4, carbon-free protective slag and carbon-free ladle covering agent are used. The water content (H2O) of the protective slag and covering agent is ≤0.5%. The superheat of the tundish in the first continuous casting furnace is controlled to be ≤40℃, and the superheat of the tundish in the continuous casting furnace is ≤30℃.

5. The method for preparing a cold-rolled high-quality carbon structural steel plate 25 according to claim 1, characterized in that, In S5, the specific control method for crowning based on the thickness of the hot-rolled raw material plate is as follows: when the thickness of the raw material plate is ≤2.2mm, the crowning is ≤50μm; when the thickness of the raw material plate is >2.2mm, the crowning is ≤60μm; and the wedge shape shall not exceed the crowning.

6. The method for preparing a cold-rolled high-quality carbon structural steel plate 25 according to claim 1, characterized in that, In S7, the specific method for controlling the hydrogen blowing rate in stages during the annealing process is as follows: First stage: heating time 1 hour, hydrogen blowing flow rate 10 m³ / h. 3 / h; Second stage: Heating time is 4-6 hours, hydrogen blowing flow rate is 20-25 m³ / h; 3 / h; Third stage: heating time 3h, hydrogen blowing flow rate 10-20m³ / h; 3 / h; Fourth stage: Heating time 2h, hydrogen blowing flow rate 8m 3 / h.

7. The method for preparing a cold-rolled high-quality carbon structural steel plate 25 according to claim 1, characterized in that, In S8, the rolling pressure is controlled according to the thickness of the finished product as follows: when the thickness of the finished product is 1.6 to 1.7 mm, the rolling force is set to 2000 kN with a fluctuation of less than 500 kN; when the thickness of the finished product is 1.6 to 1.7 mm, the rolling force is set to 2300 kN with a fluctuation of less than 500 kN; and the surface roughness is 0.7-1.1 μm.

8. The method for preparing a cold-rolled high-quality carbon structural steel plate 25 according to claim 1, characterized in that, The tensile strength of the finished 25 steel plate should be ≥400MPa and the elongation after fracture should be ≥24%.