A self-constrained electromagnetic pulse-gradient directional remelting method for cold-sprayed iron-based porous reinforcing layers
By employing a self-constrained electromagnetic pulse-gradient directional remelting method, the problems of pore degassing, interface purification, and homogenization of the reinforcing phase in cold-sprayed Fe+Al2O3 porous reinforcing layers were solved, achieving coating densification and microstructure refinement, and improving the overall mechanical properties of the coating.
Patent Information
- Application Number
- CN202611636138.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-22
- Publication Date
- 2026-11-17
AI Technical Summary
Existing remelting technologies cannot effectively solve problems such as pore degassing and interface purification, electromagnetic stirring and homogenization of the reinforcing phase, temperature gradient and solidification process control in cold-sprayed Fe+Al2O3 porous reinforcing layers, resulting in insufficient uniformity and density of the coating's internal structure.
The self-constrained electromagnetic pulse-gradient directional remelting method is adopted. By setting a serrated magnetically conductive alloy block at the bottom of the sample, combined with alternating pulse preheating, back cooling and staged gradient cooling, the electromagnetic field, temperature field and solidification process are coordinated to achieve pore discharge, homogenization of reinforcing phase and refinement of solidification structure.
The remelting and densification of the cold-sprayed porous reinforcing layer, the homogenization of the reinforcing phase, and the refinement of the solidification structure were achieved, forming a dense columnar crystal-ultrafine crystal composite skeleton, which improved the overall mechanical properties of the coating.
Smart Images

Figure CN123108280A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of gradient remelting technology, and more specifically to a self-constrained electromagnetic pulse-gradient directional remelting method for cold-sprayed iron-based porous reinforcing layers. Background Technology
[0002] Cold spraying is a surface strengthening technology that utilizes high-speed solid powder particles to impact the substrate surface, achieving coating deposition through particle plastic deformation and interlocking. Because the powder particles remain in a solid state or at a lower temperature during cold spraying, it reduces problems such as high-temperature oxidation, phase transformation, and thermal effects encountered in traditional thermal spraying. Therefore, it is suitable for metal surface protection and the preparation of composite reinforcing layers. Iron-based materials possess good mechanical properties and a solid foundation for engineering applications. Introducing Al2O3 ceramic reinforcing phase into iron-based powders can utilize the high hardness and stability of Al2O3 to improve the wear resistance and overall mechanical properties of the reinforcing layer. Therefore, Fe+Al2O3 composite reinforcing layers have good application potential.
[0003] However, cold spraying is a high-speed, layer-by-layer particle deposition process, which inevitably leads to defects such as porosity, insufficiently bonded areas between particles, and localized agglomeration of the reinforcing phase within the coating. For Fe+Al2O3 composite reinforcing layers, due to differences in deformation capacity between iron-based particles and Al2O3 particles, there is still room for improvement in the uniformity and density of the microstructure within the deposited coating. Therefore, subsequent processing is needed to regulate the microstructure and densify the porous reinforcing layer formed by cold spraying.
[0004] Although existing remelting techniques can improve the porosity and bonding problems of cold-sprayed coatings to some extent, they still have the following shortcomings for Fe+Al2O3 porous reinforcement layers: (1) There is a lack of effective pore venting and interface purification processes before remelting. There are residual gases in the pores inside the cold spray coating. When the temperature is raised directly and rapidly for remelting, the pore gases are easily heated and expanded, forming secondary pores in the molten metal. At the same time, the oxides and insufficiently bonded areas at the particle interface are difficult to be effectively treated, affecting the metallurgical bonding of the remelted layer.
[0005] (2) Insufficient electromagnetic stirring and homogenization capabilities of the molten pool. Existing high-frequency induction remelting mainly utilizes electromagnetic fields for heating, but the stirring effect generated by the electromagnetic field is not fully utilized. The Al2O3 particles in the Fe+Al2O3 molten system may locally agglomerate, and the tiny pores inside the molten pool are difficult to expel in time, affecting the uniformity and density of the remelted layer.
[0006] (3) The temperature gradient and solidification process after remelting are difficult to control effectively. Existing methods usually use natural cooling or a single cooling method, which makes it difficult to simultaneously achieve rapid solidification, grain refinement and thermal stress release. Cooling too quickly can easily generate large thermal stress and induce cracks, while cooling too slowly can easily cause grain coarsening and is not conducive to the formation of a stable directional solidification structure.
[0007] (4) Existing methods lack coordinated control over electromagnetic field, temperature field and solidification process. Adjusting remelting power or cooling parameters alone is insufficient to simultaneously address issues such as pore discharge, reinforcement phase dispersion, microstructure refinement and thermal stress control. Therefore, a process method capable of coordinated multi-field control of the remelting process is still needed. Summary of the Invention
[0008] The purpose of this invention is to provide a self-constrained electromagnetic pulse-gradient directional remelting method for cold-sprayed iron-based porous reinforcing layers. Based on high-frequency induction remelting, a magnetically conductive alloy block with a serrated microstructure is set at the bottom of the sample. Combined with alternating pulse preheating, back cooling, and staged gradient cooling after remelting, the electromagnetic field, temperature field, and solidification process during the remelting process are synergistically controlled, thereby achieving remelting densification, homogenization of the reinforcing phase, and refinement of the solidification structure of the cold-sprayed porous reinforcing layer.
[0009] The technical solution of this invention to solve the above-mentioned technical problems is as follows: A self-constrained electromagnetic pulse-gradient directional remelting method for cold-sprayed iron-based porous reinforcing layers is provided, comprising the following steps: S1. Cut the sample to prepare the reinforcement layer by cold spraying; S2. The sample is embedded into a non-magnetic insulating mold, and a magnetic alloy block with a serrated microstructure is embedded at the bottom. S3. Place the sample in an inert atmosphere, adjust the pressure to form a positive micro-pressure; S4. The cooling medium flows through the back of the sample to establish a temperature gradient between the sample surface and the back. Then, the sample is preheated by alternating pulses of the same frequency, followed by high-frequency induction remelting and electromagnetic stirring refining. S5. After high-frequency induction remelting, three-stage gradient cooling is performed.
[0010] Furthermore, in S1, the sample is a circular sample with a diameter of 30 mm, and the reinforcing layer material is Fe+Al2O3.
[0011] Furthermore, in S2, the non-magnetic insulating mold is made of 95% alumina ceramic, and the magnetic alloy block is made of 45# steel; the serration angle of the serrated microstructure matches the resonance angle of the high-frequency induction remelting frequency.
[0012] The surface of the magnetic alloy block is provided with isosceles right-angled triangular sawtooth microstructures with an apex angle of 90°, a tooth height of 0.5 mm, a tooth spacing of 1 mm, and the tips of the sawtooths pointing towards the induction coil of the high-frequency induction remelting.
[0013] Furthermore, in S3, the pressure is 0.01-0.03 MPa.
[0014] Furthermore, in S4, the cooling medium is water; When preheating with alternating pulses at the same frequency, heat for 3-5 seconds under conditions of 0.6-1 kW; During high-frequency induction remelting, heating is performed for 8-12 seconds at 1.2-2.2 kW and 170-180 kHz, with a heating temperature of 510℃.
[0015] Furthermore, in S5, a three-stage gradient cooling process is employed: First stage: Water cooling is performed on the back of the sample for 3-5 seconds to cool the surface temperature of the remelted layer to 500 ℃; Second stage: The sample is cooled to 350 ℃ at a cooling rate of 10-15 ℃ / min and held at that temperature for 10-15 min; Third stage: Water cooling is stopped, and the sample is allowed to cool naturally to room temperature with the furnace.
[0016] In the self-constrained electromagnetic pulse-gradient directional remelting process, a circular sample is first prepared by wire cutting. A pristine Fe+Al2O3 reinforcement layer with a porosity gradient and high interfacial resistivity is then prepared using a cold spraying process. The sample is embedded in a non-magnetic insulating mold, with a magnetically conductive alloy block featuring a serrated microstructure embedded at the bottom. The serration angle of the serrated microstructure matches the resonant angle of the high-frequency induction remelting frequency, generating a magnetostrictive effect under an alternating magnetic field to transmit high-frequency micro-vibrations into the coating. The sample is placed in an inert atmosphere with a positive micro-pressure, which works synergistically with the microwaves during high-frequency induction remelting. This allows residual gas within the pores of the reinforcement layer to be actively expelled by a pressure pump during the preheating stage, while preventing external oxygen infiltration. During preheating with a synchronous alternating pulse, the high resistivity of the original particle interface from the cold spraying induces localized micro-arc discharges during low-power preheating. The instantaneous high temperature generated by the micro-arc reduces and removes oxide inclusions from the particle surface, providing a clean interface for metallurgical bonding. During high-frequency induction remelting, the high-frequency electromagnetic field interacts with the bottom magnetic block, generating strong Lorentz forces and electromagnetic stirring forces within the molten pool. The stirring force uniformly disperses the hard particles (such as Al2O3) that agglomerate during cold spraying, and forces the tiny pores inside the molten pool to float upwards and be expelled through magnetostrictive waves. Before heating, the cooling medium (water cooling) flows across the back of the sample, pre-establishing a temperature gradient between the sample surface and the back. At the moment heating stops, the surface molten pool forms a large temperature gradient (G) under the strong quenching of the bottom water cooling. The perfect match between the high G value and the low growth rate (V) forces the melt to undergo directional solidification along the heat flow direction, forming a dense columnar crystal-ultrafine crystal composite framework. At the same time, due to the drastic change in the temperature gradient, a residual compressive stress field is reconstructed in situ on the coating surface, offsetting the tensile stress caused by thermal expansion and contraction. During the three-stage gradient cooling process, the first stage (self-excited cooling stage) involves maintaining forced water cooling at the back to cool the surface temperature of the remelted layer to 500°C; the second stage (gradient slow cooling stage) involves reducing the flow rate of the back cooling water to slowly cool to 350°C at a cooling rate of 10-15°C / min; and the third stage (natural cooling stage) involves shutting off the back cooling water and allowing the furnace to cool naturally to room temperature in an inert protective atmosphere to obtain a remelted, dense, and finely grained iron-based alloy reinforcement layer.
[0017] The present invention has the following beneficial effects: This invention utilizes the anomalous resistivity of a cold-sprayed porous layer and the deep coupling with a high-frequency induced electromagnetic field. By setting up a resonant structure for the magnetically conductive alloy block, it is not merely a simple heating component, but rather constitutes a complete electromagnetic refining system together with micro-arc excitation and Lorentz force stirring. Gradient cooling is not just for temperature reduction, but also to cooperate with electromagnetic stirring to achieve directional solidification and residual compressive stress reconstruction. These four characteristics are inseparable; the absence of any one step will lead to the complete failure of the core mechanism of electromagnetic pulse-micro-arc purification-directional solidification. They work together to obtain an ultrafine-grained directional microstructure on an extremely cold matrix. Attached Figure Description
[0018] Figure 1 This is a schematic diagram of a magnetically conductive alloy block; Figure 2 for Figure 1 Enlarged view of section AA; Figure 3 The images shown are surface micrographs of the products obtained in Example 1 and Comparative Examples 1-3; Figure a is Example 1, Figure b is Comparative Example 1, Figure c is Comparative Example 2, and Figure d is Comparative Example 3. Figure 4 The images shown are light micrographs of the products obtained in Example 1 and Comparative Examples 1-3; Figure a is Example 1, Figure b is Comparative Example 1, Figure c is Comparative Example 2, and Figure d is Comparative Example 3. Detailed Implementation
[0019] The present invention will be further illustrated below with reference to specific embodiments, but the embodiments do not limit the present invention in any way. Unless otherwise specified, the reagents, methods, and equipment used in the present invention are conventional reagents, methods, and equipment in this technical field.
[0020] Example 1:
[0021] A self-constrained electromagnetic pulse-gradient directional remelting method for cold-spraying iron-based porous reinforcing layers includes the following steps: S1. A circular sample with a diameter of 30 mm and a thickness of 10 mm was prepared by wire cutting, and then a ferrous alloy reinforcing layer (Fe+Al2O3) was prepared by cold spraying. S2. Embed the sample into a non-magnetic insulating mold (95% alumina ceramic), and embed a magnetically conductive alloy block (45# steel) with a serrated microstructure at the bottom; For example... Figure 1 and Figure 2 As shown, the surface of the magnetic alloy block is provided with isosceles right-angled triangular sawtooth microstructures with an apex angle of 90°, a tooth height of 0.5 mm, a tooth spacing of 1 mm, and the tips of the sawtooths pointing towards the induction coil of the high-frequency induction remelting. S3. Place the sample in a high-purity argon atmosphere, adjust the pressure to 0.02 MPa and form a positive micro-pressure, adjust the height of the support so that the distance between the sample surface to be remelted and the planar induction coil is 10 mm. S4. The cooling medium flows through the back of the sample to establish a temperature gradient between the sample surface and the back. Then, it is preheated by alternating pulses at the same frequency (power 0.8 kW, time 4 s), followed by high-frequency induction remelting (power 1.8 kW, frequency 175 kHz, time 10 s, heating temperature 510 ℃). During preheating, micro-arc discharge is induced to clean the particle interface. The high-frequency magnetic field of the heating and remelting interacts with the 90° sawtooth, generating a magnetostrictive effect at the tip, which excites a strong Lorentz stirring force into the molten pool, breaking up the agglomerated particles and forcibly expelling the pores. S5. After high-frequency induction remelting, a three-stage gradient cooling process is performed. In the first stage, water cooling is maintained for 3-5 seconds to reduce the temperature to 500 ℃. In the second stage, the water flow rate is reduced to 12 ℃ / min to cool down to 350 ℃ and held for 12 min. In the third stage, water cooling is turned off and the furnace is allowed to cool naturally to room temperature.
[0022] Comparative Example 1: A self-constrained electromagnetic pulse-gradient directional remelting method for cold-spraying iron-based porous reinforcing layers includes the following steps: S1. A circular sample with a diameter of 30 mm and a thickness of 10 mm was prepared by wire cutting, and then a ferrous alloy reinforcing layer (Fe+Al2O3) was prepared by cold spraying. S2. The sample is embedded in a non-magnetic insulating mold (95% alumina ceramic), and a magnetic alloy block (45# steel) with a serrated microstructure is embedded at the bottom; the surface of the magnetic alloy block is flat and has no 90° serrated microstructure. S3. Place the sample in a high-purity argon atmosphere, adjust the pressure to 0.02 MPa and form a positive micro-pressure, adjust the height of the support so that the distance between the sample surface to be remelted and the planar induction coil is 10 mm. S4. The cooling medium flows through the back of the sample to establish a temperature gradient between the sample surface and the back. Then, it is preheated by alternating pulses at the same frequency (power 0.8 kW, time 4 s), followed by high-frequency induction remelting (power 1.8 kW, frequency 175 kHz, time 10 s, heating temperature 510 ℃). During preheating, micro-arc discharge is induced to clean the particle interface. The high-frequency magnetic field of the heating and remelting interacts with the 90° sawtooth, generating a magnetostrictive effect at the tip, which excites a strong Lorentz stirring force into the molten pool, breaking up the agglomerated particles and forcibly expelling the pores. S5. After high-frequency induction remelting, a three-stage gradient cooling process is performed. In the first stage, water cooling is maintained for 3-5 seconds to reduce the temperature to 500 ℃. In the second stage, the water flow rate is reduced to 12 ℃ / min to cool down to 350 ℃ and held for 12 min. In the third stage, water cooling is turned off and the furnace is allowed to cool naturally to room temperature.
[0023] Comparative Example 2: A self-constrained electromagnetic pulse-gradient directional remelting method for cold-spraying iron-based porous reinforcing layers includes the following steps: S1. A circular sample with a diameter of 30 mm and a thickness of 10 mm was prepared by wire cutting, and then a ferrous alloy reinforcing layer (Fe+Al2O3) was prepared by cold spraying. S2. The sample is embedded in a non-magnetic insulating mold (95% alumina ceramic), and a magnetic alloy block (45# steel) with a serrated microstructure is embedded at the bottom. The surface of the magnetic alloy block is provided with an isosceles right-angled triangular serrated microstructure with a vertex angle of 90°, a tooth height of 0.5 mm, a tooth spacing of 1 mm, and the serrated tips pointing towards the induction coil of the high-frequency induction remelting. S3. Place the sample in a high-purity argon atmosphere, adjust the pressure to 0.02 MPa and form a positive micro-pressure, adjust the height of the support so that the distance between the sample surface to be remelted and the planar induction coil is 10 mm. S4. The cooling medium flows through the back of the sample to establish a temperature gradient between the sample surface and the back. Then, it is preheated by alternating pulses at the same frequency (power 0.8 kW, time 4 s), followed by high-frequency induction remelting (power 1.8 kW, frequency 175 kHz, time 10 s, heating temperature 510 ℃). During preheating, micro-arc discharge is induced to clean the particle interface. The high-frequency magnetic field of the heating and remelting interacts with the 90° sawtooth, generating a magnetostrictive effect at the tip, which excites a strong Lorentz stirring force into the molten pool, breaking up the agglomerated particles and forcibly expelling the pores. S5. After high-frequency induction remelting, the furnace is naturally cooled to room temperature in an inert atmosphere.
[0024] Due to the lack of segmented temperature control, the cooling rate of the molten layer surface is completely uncontrollable after heating is completely stopped, influenced by the residual heat of the substrate and heat dissipation from the air. The surface layer generates enormous thermal stress instantaneously during rapid cooling, which mismatches with the thermal expansion caused by uneven internal temperature. This results in dense, macroscopic, penetrating cracks on the remelted layer surface, and the coating exhibits a tendency to peel over large areas.
[0025] Comparative Example 3: A self-constrained electromagnetic pulse-gradient directional remelting method for cold-spraying iron-based porous reinforcing layers includes the following steps: S1. A circular sample with a diameter of 30 mm and a thickness of 10 mm was prepared by wire cutting, and then a ferrous alloy reinforcing layer (Fe+Al2O3) was prepared by cold spraying. S2. The sample is embedded in a non-magnetic insulating mold (95% alumina ceramic), and a magnetic alloy block (45# steel) with a serrated microstructure is embedded at the bottom. The surface of the magnetic alloy block is provided with an isosceles right-angled triangular serrated microstructure with a vertex angle of 90°, a tooth height of 0.5 mm, a tooth spacing of 1 mm, and the serrated tips pointing towards the induction coil of the high-frequency induction remelting. S3. Place the sample in a high-purity argon atmosphere, adjust the pressure to 0.02 MPa and form a positive micro-pressure, adjust the height of the support so that the distance between the sample surface to be remelted and the planar induction coil is 10 mm. S4. Directly heat at 1.8 kW and 175 kHz for 10 s, heating temperature 510 s; Because no preheating step was performed, the gas that should have been steadily escaping from the pores of the cold-sprayed coating surface at low temperatures encountered a sudden high temperature, resulting in violent instantaneous expansion and the formation of huge internal stress. This caused large-scale cracking and peeling of the coating surface. At the same time, due to the lack of forced back cooling, a large amount of heat was conducted to the substrate, resulting in a severe expansion of the heat-affected zone of the substrate. The temperature difference between the surface and the substrate was extremely small, making it impossible to establish an effective temperature gradient. As a result, the natural cooling of the molten pool was extremely slow, and directional solidification and self-cooling effects failed to form. The gas in the molten pool could not also rise and be discharged quickly with the help of the thermal gradient.
[0026] S5. After high-frequency induction remelting, a three-stage gradient cooling process is performed. In the first stage, water cooling is maintained for 3-5 seconds to reduce the temperature to 500 ℃. In the second stage, the water flow rate is reduced to 12 ℃ / min to cool down to 350 ℃ and held for 12 min. In the third stage, water cooling is turned off and the furnace is allowed to cool naturally to room temperature.
[0027] The products obtained in Example 1 and Comparative Examples 1-3 were subjected to performance tests, and the results are shown in Table 1; the surface micrographs and micrographs of the samples are shown in Table 1. Figure 3 and Figure 4 As shown.
[0028] Table 1 Performance Test Results
[0029] Table 1 shows that the remelted layer of Comparative Example 1 contains a significant pore aggregation area, indicating that the 90° resonant sawtooth pattern is an indispensable core feature for generating electromagnetic stirring and forced venting. The results of Example 1 demonstrate that three-stage gradient slow cooling is a core feature for smoothly releasing thermal stress, preventing cracking of the remelted layer, and ensuring coating integrity. In Comparative Example 3, due to spalling and lack of densification, the sample surface was essentially unusable, and a complete remelted layer could not be formed. Measurements of the residual area with severe defects showed a porosity exceeding 10%, an average grain size as large as 15 μm (due to the lack of self-cooling, the grains grew significantly), a severe decrease in microhardness to 250 HV, and an interface bonding strength reduced to below 20 MPa due to spalling. This indicates that synchronous alternating pulse preheating and gradient cooling are indispensable synergistic features for ensuring stable gas release, establishing an extreme gradient field, achieving high-speed directional solidification, and preventing coating spalling.
[0030] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A self-constrained electromagnetic pulse-graded directional remelting method of cold sprayed iron-based porous reinforced layer, characterized in that, The method comprises the following steps: S1, cutting a sample and preparing a reinforcing layer by cold spraying; S2, embedding the sample into a non-magnetic insulation mold and embedding a magnetic alloy block with a jagged microstructure at the bottom; S3, placing the sample in an inert atmosphere, adjusting the pressure and forming a positive micro-pressure; S4, flowing a cooling medium through the back of the sample to build a temperature gradient on the surface and back of the sample, then preheating through the same frequency alternating pulse, and then high-frequency induction remelting and electromagnetic stirring refining; S5, three-stage gradient cooling after high-frequency induction remelting.
2. The self-constrained electromagnetic pulse-graded directional remelting method of cold sprayed iron-based porous reinforcing layer according to claim 1, characterized in that, In S1, the sample is a φ30 mm circular sample, and the reinforcing layer material is Fe+Al2O3.
3. The self-constrained electromagnetic pulse-graded directional remelting method of cold sprayed iron-based porous reinforcing layer according to claim 1, characterized in that, In S2, the non-magnetic insulation mold material is 95% alumina ceramic.
4. The self-constrained electromagnetic pulse-graded directional remelting method of cold sprayed iron-based porous reinforcing layer according to claim 1, characterized in that, In S3, the pressure is 0.01-0.03 Mpa.
5. The self-constrained electromagnetic pulse-graded directional re- melting method of cold sprayed iron-based porous reinforced layers according to claim 1, characterized in that, In S4, the cooling medium is water; When preheating through the same frequency alternating pulse, heat for 3-5 s under the condition of 0.6-1 kW; When high-frequency induction remelting, heat for 8-12 s under the condition of 1.2-2.2 kW and 170-180 kHz.
6. The self-constrained electromagnetic pulse-graded directional re- melting method of cold sprayed iron-based porous reinforced layers according to claim 1, characterized in that, In S5, three-stage gradient cooling: first stage: cool the remelted layer surface temperature to 500 ℃ by water cooling through the back of the sample for 3-5 s; second stage: cool to 350 ℃ at a cooling rate of 10-15 ℃ / min and keep for 10-15 min; third stage: stop water cooling and cool to room temperature naturally with the furnace.