A method for preparing titanium oxychloride solution by hydrochloric acid pressure leaching of ilmenite.

By reacting hydrochloric acid with ilmenite under high temperature and pressure, and adding hydrolysis inhibitors and TiO2 powder, the problem of easy hydrolysis of titanium oxychloride solution was solved, achieving efficient titanium leaching and stable preparation of titanium oxychloride solution, thus improving production efficiency and environmental performance.

CN123108293APending Publication Date: 2026-11-17SHANDONG CHUANGLING NEW MATERIAL TECH CO LTD +2
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611214443.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-11
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing technologies, titanium oxychloride solution is easily hydrolyzed to form TiO(OH)2 colloid, resulting in poor process stability, low titanium leaching rate, low reaction efficiency, large amount of waste acid, and high environmental treatment pressure.

Method used

Hydrochloric acid was used to react with ilmenite under high temperature and high pressure conditions. Hydrolysis inhibitors NH4Cl and oxalic acid were added to control the reaction temperature and acidity. Iron impurities were precipitated by adding TiO2 powder. High pressure was used to suppress the volatilization of hydrochloric acid, thereby improving the titanium leaching rate and stabilizing the titanium oxychloride solution.

Benefits of technology

It increased the titanium leaching rate to over 95%, reduced hydrochloric acid consumption by 40%, reduced wastewater treatment costs, improved production efficiency and product purity, and solved the problem of easy hydrolysis of titanium oxychloride solution.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention relates to a method for preparing titanium oxychloride solution by pressure leaching of ilmenite with hydrochloric acid, belonging to the technical field of hydrometallurgy. The invention uses ilmenite as raw material, reacting it with hydrochloric acid under high temperature and high pressure conditions; after the reaction, a hydrolysis inhibitor is added to obtain the titanium oxychloride solution. This invention solves the problem of easy hydrolysis of titanium oxychloride solution by adding a small amount of hydrolysis inhibitor. The high-pressure reaction increases the titanium leaching rate to over 95%, and the concentration of titanium oxychloride in the prepared solution is ≥150 g / L. Simultaneously, compared with the atmospheric pressure method, the hydrochloric acid consumption of this invention is reduced by 40%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the technical field of hydrometallurgy, specifically to a method for preparing titanium oxychloride solution by pressure leaching of ilmenite with hydrochloric acid. Background Technology

[0002] Titanium oxychloride (TiOCl2) is an inorganic compound composed of titanium (Ti), chlorine (Cl), and oxygen (O). It is commonly used as a precursor in the preparation of titanium-based catalysts or functional materials. For example, in the preparation of titanium dioxide, titanium oxychloride can be hydrolyzed in water to produce titanium hydroxide or hydrated oxides, which are then calcined to obtain high-purity titanium dioxide. Titanium oxychloride can also be used in the sol-gel method to prepare titanium oxide thin films or nanomaterials.

[0003] Titanium oxychloride is usually prepared industrially by high-temperature chlorination, using TiO2 or titanium tetrachloride as raw materials, reacting with chlorine (Cl2) or oxygen-containing gases (such as CO / CO2 or O2) at high temperatures of 600 ℃ to 1000 ℃. However, since titanium oxychloride is unstable at high temperatures and is prone to further chlorination or decomposition, the process conditions need to be strictly controlled. There is also a hydrochloric acid method for preparing titanium oxychloride, which involves partial hydrolysis of titanium tetrachloride or reaction of titanium dioxide with concentrated hydrochloric acid at high temperatures. However, the hydrochloric acid method has the following problems: (1) When titanium tetrachloride is hydrolyzed, the amount of water needs to be accurately measured to prevent excessive hydrolysis to generate TiO(OH)2 or titanium dioxide. The reaction of titanium dioxide with concentrated hydrochloric acid has low production efficiency and requires high temperature (reaction temperature ≥100℃) and concentrated hydrochloric acid (concentration ≥36%), and the by-product Cl2 needs to be treated. Furthermore, the hydrochloric acid method also has the problem that after obtaining titanium oxychloride, it is very easy to hydrolyze to form TiO(OH)2 colloid, resulting in poor overall process stability.

[0004] The existing methods for preparing titanium oxychloride solution using ilmenite powder and hydrochloric acid have the following problems: (1) Severe volatilization of hydrochloric acid and easy decrease in system acidity: Under normal pressure and heating, a large amount of HCl volatilizes, and the acidity of the reaction system continues to decrease, which directly leads to low titanium dissolution rate and poor reaction efficiency. In addition, the volatilized HCl corrodes equipment and pollutes the environment. (2) Titanium oxychloride is prone to premature hydrolysis: When the acidity is insufficient, the generated TiOCl2 is rapidly hydrolyzed to form TiO2 precipitate, the titanium recovery rate decreases and the product purity is low; in order to inhibit hydrolysis, HCl needs to be continuously introduced, which further increases acid consumption and wastewater volume. For example, patent CN101723448A discloses a method for preparing titanium oxychloride, which discloses the preparation of titanium oxychloride by reacting ilmenite powder and hydrochloric acid under normal pressure and heating conditions. After obtaining titanium oxychloride, hydrogen chloride gas is introduced into the reaction system to inhibit the hydrolysis of titanium oxychloride. However, the above method uses too much hydrogen chloride, which puts great pressure on subsequent wastewater treatment. (3) Difficult separation of ilmenite and large interference from impurities: Iron oxides in ilmenite react with hydrochloric acid to generate FeCl2 / FeCl3, and a large amount of iron impurities are mixed into the titanium solution, resulting in a high load for subsequent impurity removal; the hydrolysis of iron salt also consumes acid and aggravates titanium hydrolysis. (4) Limited reaction temperature and low leaching efficiency: The boiling point of the hydrochloric acid system is low at normal pressure (about 108℃), and it is difficult to increase the reaction temperature. The ilmenite lattice is not sufficiently destroyed, and the leaching rate of titanium is usually less than 80%, resulting in low resource utilization. (5) Large amount of waste acid and high treatment cost: In order to maintain acidity and inhibit hydrolysis, excess hydrochloric acid and HCl gas are required. The subsequent waste acid concentration is high and the total amount is large. The neutralization treatment consumes a lot of alkali and contains a high concentration of Cl. - Compared to iron salts, environmental disposal faces significant challenges. Summary of the Invention

[0005] To address the technical problem that the titanium oxychloride solution is easily hydrolyzed to form TiO(OH)2 colloid during the preparation of titanium oxychloride, resulting in poor process stability, this invention provides a method for preparing titanium oxychloride solution by hydrochloric acid pressure leaching of ilmenite, thereby solving the above-mentioned problem.

[0006] The technical solution of this invention is as follows: A method for preparing titanium oxychloride solution by hydrochloric acid pressure leaching of ilmenite involves using ilmenite as raw material and reacting it with hydrochloric acid under high temperature and high pressure conditions; after the reaction is completed, a hydrolysis inhibitor is added to obtain the titanium oxychloride solution.

[0007] Furthermore, ilmenite reacts with hydrochloric acid under conditions of 0.3–0.8 MPa. Existing technologies typically use atmospheric pressure heating to prepare titanium oxychloride, relying on the introduction of large amounts of hydrogen chloride to suppress product hydrolysis. However, hydrochloric acid is volatile under atmospheric pressure, resulting in insufficient acidity in the system. This leads to low titanium leaching rates and easy hydrolysis of titanium oxychloride, causing raw material losses. It also consumes large amounts of hydrogen chloride, resulting in high chloride and residual acid content in subsequent wastewater, putting significant pressure on environmental treatment. Additionally, it causes significant iron impurity leaching, making product purification difficult. By using high-pressure conditions of 0.3–0.8 MPa, hydrochloric acid volatilization is suppressed, stabilizing the system's high acidity and inhibiting titanium oxychloride hydrolysis at its source, eliminating the need for the large-scale introduction of hydrogen chloride. Furthermore, it increases the reaction temperature, fully disrupting the mineral lattice, effectively improving titanium leaching rates, and reducing impurity leaching. This improves product quality and production efficiency while significantly reducing acid consumption and subsequent wastewater treatment costs, making it more suitable for industrial production.

[0008] Furthermore, the reaction temperature of ilmenite with hydrochloric acid is controlled at 110 ℃~120 ℃.

[0009] Furthermore, the hydrolysis inhibitor includes NH4Cl and oxalic acid, with a total concentration of NH4Cl and oxalic acid of 0.15~0.35 mol / L. Testing showed that the hydrolysis inhibitor can ensure that the titanium dichloride solution remains stable at 60 °C for 24 hours without hydrolysis.

[0010] Furthermore, in the hydrolysis inhibitor, the concentration of NH4Cl is 0.1~0.3 mol / L, and the concentration of oxalic acid is 0.05 mol / L.

[0011] Furthermore, the concentration of the hydrochloric acid is 20 wt% to 25 wt%.

[0012] Furthermore, after ilmenite reacts with hydrochloric acid under high temperature and high pressure conditions, TiO2 powder is added to the reaction solution to adjust the pH of the reaction system to 1.5~2.0. The addition of TiO2 powder selectively precipitates Fe. 3+ This ensures that the Fe residue in the reaction system is <0.5g / L, which meets the requirements for direct production of titanium powder by electrolysis.

[0013] Furthermore, when adding TiO2 powder to purify the reaction system, the reaction is carried out under normal pressure.

[0014] Furthermore, before reacting with hydrochloric acid, the ilmenite is crushed to a particle size of 200 mesh.

[0015] Furthermore, the waste gas generated from the reaction of ilmenite and hydrochloric acid enters the absorption device, where it reacts with H2O2 to generate hydrochloric acid for recycling, increasing the utilization rate of hydrochloric acid to over 90%.

[0016] The beneficial effects of this invention are as follows: This invention provides a method for preparing titanium oxychloride solution by pressure leaching of ilmenite with hydrochloric acid. By adding a small amount of hydrolysis inhibitor, the problem of easy hydrolysis of titanium oxychloride solution is solved. A high-pressure reaction is employed, increasing the titanium leaching rate to over 95%, and the concentration of titanium oxychloride in the prepared solution is ≥150 g / L. Simultaneously, compared with the atmospheric pressure method, this invention reduces hydrochloric acid consumption by 40%. Detailed Implementation

[0017] To enable those skilled in the art to better understand the technical solutions of this invention, the technical solutions in the embodiments of this invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of this invention, and not all embodiments. Based on the embodiments of this invention, all other embodiments obtained by those skilled in the art without creative effort should fall within the scope of protection of this invention.

[0018] Example 1 A method for preparing titanium oxychloride solution by pressure leaching of ilmenite with hydrochloric acid, the specific steps of which are as follows: (1) Use 1 kg of ilmenite with a particle size of 200 mesh as raw material, wherein the TiO2 content in the ilmenite is 48%; add 4L of hydrochloric acid with a concentration of 25%, mix and add to a high-pressure reactor; (2) The pressure vessel was controlled to react at 0.4 MPa and 115 ℃ for 3 h. After cooling, the mixture was filtered to obtain the leachate. The concentration of TiOCl2 in the leachate was measured to be 152 g / L, and the concentration of Fe was 152 g / L. 2+ The concentration was 12.3 g / L; (3) Add TiO2 powder to the leachate to adjust the pH of the leachate to 1.5~2.0. The amount added is approximately 1.2 times the theoretical amount. The theoretical amount mentioned here refers to the total amount of Fe²⁺ in the leachate. + Oxidized to Fe³ + The required stoichiometric amount of TiO2 for hydrolysis and precipitation was determined. The mixture was then stirred at 80 °C for 1 h and filtered. The Fe content in the filtrate was then measured. 3+ Reduced to 0.4 g / L; (4) Add a hydrolysis inhibitor to the filtrate. The concentration of NH4Cl in the hydrolysis inhibitor is 0.2 mol / L and the concentration of oxalic acid is 0.05 mol / L. Titanium dichloride solution is obtained.

[0019] The transmittance (450 nm) of the titanium oxychloride solution was >90%. Simultaneously, tests on solution turbidity, pH stability, chloride / titanium molar ratio, and accelerated storage demonstrated that the solution exhibited excellent stability with no significant hydrolysis precipitation during storage; the titanium leaching rate was ≥98%. Raman spectroscopy, infrared spectroscopy, and X-ray photoelectron spectroscopy were used to characterize the form of titanium in the solution, indicating that titanium mainly exists as TiO₂.2+ The presence of TiOCl2 in the form of (titanium dichloride) with significant Ti=O bond characteristic peaks and no obvious Ti-O-Ti hydrolysis product signal proves that TiOCl2 exists stably in solution.

[0020] Example 2 A method for preparing titanium oxychloride solution by pressure leaching of ilmenite with hydrochloric acid, the specific steps of which are as follows: (1) Use 100 kg of ilmenite with a particle size of 200 mesh as raw material, wherein the TiO2 content in the ilmenite is 48%; add 400 L of hydrochloric acid with a concentration of 25%, mix and add to a high-pressure reactor; the mineral-acid ratio (mass / volume) is 1:4 kg / L; (2) The pressure vessel was controlled to react at 0.5 MPa and 115 ℃ for 3 h; after the reaction, the pressure inside the vessel was reduced to atmospheric pressure, and a pipe was installed at the exhaust port of the high-pressure vessel to introduce the depressurized waste gas into the absorption tower. The absorption tower was filled with hydrogen peroxide, which could convert the waste gas (mainly HCl and Cl2) into hydrochloric acid for recycling; after cooling, the solution was filtered to obtain the leachate; after testing, the concentration of TiOCl2 in the leachate was 152 g / L, and the Fe... 2+ The concentration was 22.7 g / L; The amount of HCl recovered is calculated by detecting the volume and concentration of hydrochloric acid recovered in the absorption tower. This amount is then divided by the theoretical amount of HCl lost through volatilization during the reaction process to obtain the hydrochloric acid recovery rate, specifically: (Amount of recovered HCl / Amount of theoretically lost HCl through volatilization) × 100% = 91.2% (3) Add TiO2 powder to the leachate, the amount of which is approximately 1.2 times the theoretical amount. Adjust the pH of the leachate to 1.5~2.0, then stir at 80 ℃ for 1 h and filter. Detect the Fe content in the filtrate. 3+ Reduced to 0.4 g / L; (4) Add a hydrolysis inhibitor to the filtrate. The concentration of NH4Cl in the hydrolysis inhibitor is 0.2 mol / L and the concentration of oxalic acid is 0.05 mol / L. Titanium dichloride solution is obtained.

[0021] The transmittance of the titanium oxychloride solution (450 nm) was >90%. Furthermore, indicators such as solution turbidity, pH stability, chloride / titanium molar ratio, and accelerated storage tests confirmed that the solution exhibited excellent stability with no significant hydrolysis precipitation during storage; the titanium leaching rate was 98.5%. Raman spectroscopy, infrared spectroscopy, and X-ray photoelectron spectroscopy were used to characterize the form of titanium in the solution, indicating that titanium mainly exists as TiO2. 2+ The presence of TiOCl2 in the form of (titanium dichloride) with significant characteristic peaks of Ti=O bonds and no obvious signals of Ti-O-Ti hydrolysis products proves that TiOCl2 exists stably in solution.

[0022] Comparative Example 1 A method for preparing titanium oxychloride solution by leaching ilmenite with hydrochloric acid, the specific steps of which are as follows: (1) Use 1 kg of ilmenite with a particle size of 200 mesh as raw material, wherein the TiO2 content in the ilmenite is 48%; add 4 L of 25% hydrochloric acid, mix and add to the reactor; the mineral-acid ratio (mass / volume) is 1:4 kg / L; (2) The reaction was carried out at 115 °C under normal pressure for 6 h. After cooling, the solution was filtered to obtain the leachate. The concentration of TiOCl2 in the leachate was found to be 85 g / L, and the concentration of Fe was 85 g / L. 2+ The concentration was 15.6 g / L; (3) Add TiO2 powder to the leachate, the amount of which is about 1.2 times the theoretical amount. Adjust the pH of the leachate to 1.5~2.0, then stir at 80℃ for 1 h and filter. The transmittance (450 nm) of the titanium oxychloride solution was 72%. Numerous Ti-O-Ti hydrolysis signals were observed through tests on solution turbidity, pH stability, chloride / titanium molar ratio, and accelerated storage. The titanium leaching rate was 55%.

[0023] Comparative Example 2 A method for preparing titanium oxychloride solution by pressure leaching of ilmenite with hydrochloric acid, the specific steps of which are as follows: (1) Use 1 kg of ilmenite with a particle size of 200 mesh as raw material, wherein the TiO2 content in the ilmenite is 48%; add 4 L of hydrochloric acid with a concentration of 25%, mix and then add to a high-pressure reactor; (2) The reaction was carried out at 115 °C under normal pressure for 6 h. During the reaction, 3.2 L of 25% hydrochloric acid was added. After cooling, the solution was filtered to obtain the leachate. The concentration of TiOCl2 in the leachate was found to be 102 g / L, and the concentration of Fe was 102 g / L. 2+ The concentration was 18.3 g / L; (3) Add TiO2 powder to the leachate, the amount of which is approximately 1.2 times the theoretical amount. Adjust the pH of the leachate to 1.5~2.0, then stir at 80 ℃ for 1 h and filter to obtain a titanium oxychloride solution. Detect the Fe content in the filtrate. 3+ The concentration is 1.2 g / L; The transmittance (450nm) of the titanium oxychloride solution was >90%. (Small amounts of Ti-O-Ti hydrolysis signals were observed through tests on solution turbidity, pH stability, chloride / titanium molar ratio, and accelerated storage. The titanium leaching rate was 66%.)

[0024] The results of Examples 1-2 and Comparative Examples 1-2 show that high pressure conditions effectively suppress hydrochloric acid volatilization, stabilize the acidity of the system and increase the reaction temperature. The titanium leaching rate is increased from 55%-66% in the normal pressure process to ≥98%, and the TiOCl2 concentration is significantly increased, which greatly improves the raw material utilization rate and production efficiency.

[0025] In addition, this invention eliminates the need for intermediate acid replenishment, achieving a hydrochloric acid reuse rate of up to 91.2%, thus avoiding the problems of high acid consumption and large wastewater volume in traditional atmospheric pressure processes, and significantly reducing subsequent wastewater treatment costs and environmental pressure.

[0026] After impurity removal, the high-pressure leachate of this invention contains Fe 3+ The concentration can be reduced to below 0.4 g / L, and the transmittance (450 nm) remains stable at over 90%. Characterization results, including Raman spectroscopy, show that titanium in the solution mainly exists as stable TiO2. 2+ It exists in a form without obvious hydrolysis product signals, thus solving the defects of easy hydrolysis and low light transmittance in the atmospheric pressure process.

[0027] Although the present invention has been described in detail by way of preferred embodiments, the present invention is not limited thereto. Various equivalent modifications or substitutions can be made to the embodiments of the present invention by those skilled in the art without departing from the spirit and essence of the invention, and such modifications or substitutions should all be within the scope of the present invention. Any variations or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention should also be covered within the protection scope of the present invention.

Claims

1. A method for preparing titanium oxychloride solution by pressure leaching of ilmenite with hydrochloric acid, characterized in that, Using ilmenite as raw material, it is reacted with hydrochloric acid under high temperature and high pressure conditions; after the reaction is completed, a hydrolysis inhibitor is added to obtain a titanium oxychloride solution.

2. The method for preparing titanium oxychloride solution by hydrochloric acid pressure leaching of ilmenite as described in claim 1, characterized in that, Ilmenite reacts with hydrochloric acid under conditions of 0.3~0.8 MPa.

3. The method for preparing titanium oxychloride solution by hydrochloric acid pressure leaching of ilmenite as described in claim 1, characterized in that, The reaction temperature of ilmenite with hydrochloric acid is controlled at 110 ℃~120 ℃.

4. The method for preparing titanium oxychloride solution by hydrochloric acid pressure leaching of ilmenite as described in claim 1, characterized in that, The hydrolysis inhibitor includes NH4Cl and oxalic acid, and the total concentration of NH4Cl and oxalic acid in the hydrolysis inhibitor is 0.15~0.35 mol / L.

5. The method for preparing titanium oxychloride solution by hydrochloric acid pressure leaching of ilmenite as described in claim 4, characterized in that, The hydrolysis inhibitor contains NH4Cl at a concentration of 0.1–0.3 mol / L and oxalic acid at a concentration of 0.05 mol / L.

6. The method for preparing titanium oxychloride solution by hydrochloric acid pressure leaching of ilmenite as described in claim 1, characterized in that, The concentration of the hydrochloric acid is 20 wt% to 25 wt%.

7. The method for preparing titanium oxychloride solution by hydrochloric acid pressure leaching of ilmenite as described in claim 1, characterized in that, After ilmenite reacts with hydrochloric acid under high temperature and high pressure, TiO2 powder is added to the reaction solution to adjust the pH of the reaction system to 1.5~2.

0.

8. The method for preparing titanium oxychloride solution by hydrochloric acid pressure leaching of ilmenite as described in claim 7, characterized in that, When adding TiO2 powder to purify the reaction system, the reaction is carried out under normal pressure.

9. The method for preparing titanium oxychloride solution by hydrochloric acid pressure leaching of ilmenite as described in claim 1, characterized in that, Before reacting with hydrochloric acid, ilmenite is crushed to a particle size of 200 mesh.

10. The method for preparing titanium oxychloride solution by hydrochloric acid pressure leaching of ilmenite as described in claim 1, characterized in that, The waste gas generated from the reaction of ilmenite and hydrochloric acid enters the absorption device, and the absorption liquid in the absorption device is H2O2.

Citation Information

Patent Citations

  • Method for preparing titaniferous solution

    CN101723448A