A resource recovery method based on leaching of lithium and transition metals from spent lithium batteries and catalytic degradation of antibiotics.
By calcining mixed waste lithium battery cathode powder and lobster shell powder, a catalyst was prepared for water leaching lithium and transition metal extraction. Based on this catalyst, potassium persulfate was activated, solving the problems of long resource utilization cycle and high cost of waste lithium batteries, and realizing efficient antibiotic degradation and environmentally friendly resource recycling.
Patent Information
- Application Number
- CN202611386676.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-08
- Publication Date
- 2026-11-17
AI Technical Summary
In existing technologies, the resource utilization cycle of waste lithium batteries is too long and the cost is high. Furthermore, heterogeneous carbon-based catalysts require additional strong reducing agents, resulting in complicated processes and secondary pollution, making it difficult to efficiently degrade antibiotic pollutants in water.
Lobster shell powder is mixed with waste lithium battery cathode powder and calcined to prepare solid-phase pyrolysis residue. Lithium and transition metals are recovered by water leaching treatment. The solid-phase water leaching residue recovered from waste lithium batteries is used as a catalyst and activated with potassium persulfate to achieve the catalytic degradation of antibiotics.
It achieves efficient resource utilization of waste lithium batteries, rapidly degrades antibiotics, reduces costs and environmental pollution, and has significant economic and environmental benefits.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] This invention belongs to the field of environmental pollution treatment technology, specifically relating to a resource recovery method based on the leaching and recovery of lithium and transition metals from waste lithium batteries and the catalytic degradation of antibiotics. Background Technology
[0002] With the large-scale production and widespread use of antibiotics globally, various antibiotics (such as tetracyclines, sulfonamides, and chlortetracycline hydrochloride) are frequently detected in natural water bodies through the discharge of pharmaceutical and aquaculture wastewater, posing a serious threat to ecological security and human health. Sulfate free radicals (SO4) based on potassium persulfate (PMS) are also a concern. - Heterogeneous advanced oxidation technologies (SR-AOPs) have become a core method for removing recalcitrant organic pollutants from water due to their wide pH range and high oxidation potential. The core of this technology lies in activating polystyrene (PMS) with a heterogeneous carbon-based catalyst to generate highly reactive oxygen species that degrade pollutants. However, existing heterogeneous carbon-based catalysts often rely on expensive transition metal salts or require complex secondary surface loading modifications using strong reducing agents such as ascorbic acid (VC). This not only involves cumbersome processes and high synthesis costs but also easily causes secondary pollution during preparation.
[0003] If catalysts can be prepared using waste as raw materials, a win-win situation of "treating waste with waste" can be achieved. Lithium-ion batteries are widely used in electronic products due to their high energy density and long cycle life. The cathode materials of spent lithium-ion batteries typically contain transition metal elements such as cobalt, nickel, and manganese. If these transition metal elements can be recycled and reused, it will not only solve the problem of waste battery disposal but also realize their resource utilization.
[0004] Chinese invention patent CN115739108A discloses a method for the resource utilization of waste lithium-ion batteries. The method involves disassembling and soaking the waste batteries, then mixing them with activated carbon and calcining to prepare a catalyst, which is then used in conjunction with an oxidant to remove antibiotic pollutants from water. However, this method requires the waste lithium-ion batteries to be soaked in NaCl solution for 10 to 20 days, resulting in an excessively long pretreatment cycle, which is not conducive to rapid industrial processing and leads to a low resource utilization rate.
[0005] Therefore, there is an urgent need to find a low-cost, simple, and environmentally friendly method for the efficient resource utilization and antibiotic degradation of waste lithium batteries. Summary of the Invention
[0006] To address the problems existing in the prior art, the present invention aims to provide a resource utilization method based on the extraction of lithium and transition metals from waste lithium batteries and the catalytic degradation of antibiotics in water. This method has a high reaction rate and purification efficiency, and achieves high added value utilization of industrial solid waste such as waste lithium battery cathode powder and lobster shell powder, effectively reducing costs and having significant economic and environmental benefits.
[0007] To achieve the above objectives, the present invention adopts the following technical solution: A resource recovery method based on lithium extraction and transition metal leaching from spent lithium batteries and catalytic degradation of antibiotics in water is provided, comprising the following steps: 1) Lobster shell powder is thoroughly mixed with waste lithium battery cathode powder and then calcined in air to obtain solid-phase pyrolysis residue; the obtained solid-phase pyrolysis residue is subjected to water leaching treatment to extract lithium and transition metals Ni, Co, and Mn, and the leaching solution rich in lithium and transition metals and the water leaching filter residue are collected. Then the water leaching filter residue is washed and dried to obtain waste lithium battery recycling solid-phase water leaching filter residue catalyst material; wherein: the waste lithium battery is a nickel-cobalt-manganese ternary lithium battery; 2) Add the waste lithium battery recycling solid phase water leaching filter residue catalyst material prepared in step 1) to the antibiotic wastewater, stir to carry out dark adsorption until dark adsorption equilibrium is reached; 3) Add potassium persulfate (PMS) to the reaction system obtained in step 2) to carry out the catalytic degradation of antibiotics.
[0008] According to the above scheme, in step 1), the mass ratio of lobster shell powder to waste lithium battery cathode powder is 1.5~4:1, preferably 1.5~3:1, and more preferably 1.8~2.5:1.
[0009] According to the above scheme, in step 1), the lobster shell powder is passed through a 100-mesh sieve.
[0010] According to the above scheme, in step 1), the waste lithium battery is LiNi x Co y Mn z Power lithium-ion batteries using O2 as the positive electrode active material; including but not limited to NCM111, NCM523, NCM622 and NCM811 systems.
[0011] According to the above scheme, in step 1), the calcination temperature is 400~600℃, preferably 450~520℃; the time is 30~60 min; preferably, the heating rate is 5~10℃ / min.
[0012] According to the above scheme, in step 1), the immersion time is 10~30 min.
[0013] According to the above scheme, in step 1), the liquid-to-solid ratio during water immersion treatment is 5~20 g / L.
[0014] According to the above scheme, in step 1), after water immersion treatment, the lithium leaching rate in the lithium-rich filtrate is 90-98%; the leaching rates of Ni, Co, and Mn are independently 85-95%.
[0015] The leaching rate refers to the percentage of the mass of the metal leached into the solution relative to the total mass of that metal in the original waste lithium battery cathode material.
[0016] According to the above scheme, in step 1), the water-leached filter residue mainly contains transition metal oxides such as Ni, Co, and Mn, graphitized carbon, and amorphous carbon materials, while also containing a small amount of aluminum oxide and residual inorganic salts. This multi-component structure endows the material with excellent electron transport capabilities and redox activity, enabling it to function as a persulfate-activated catalyst.
[0017] According to the above scheme, in step 2), the mass ratio of the solid phase water leaching filter residue catalyst material to the antibiotic is 5~15:1.
[0018] According to the above scheme, in step 2), the dark adsorption time is 10~30 min.
[0019] According to the above scheme, in step 2), the antibiotic is a tetracycline, quinolone, sulfonamide or β-lactam antibiotic, such as chlortetracycline hydrochloride, tetracycline, ciprofloxacin, norfloxacin, sulfamethoxazole or amoxicillin.
[0020] According to the above scheme, in step 2), the concentration of antibiotic wastewater is 5-100 mg / L, such as 10 mg / L, 20 mg / L, 30 mg / L, 40 mg / L, 50 mg / L, 60 mg / L, 70 mg / L, 80 mg / L, 90 mg / L, and 100 mg / L.
[0021] According to the above scheme, in step 3), the mass ratio of the solid phase water leaching filter residue catalyst material to PMS is 1:1 to 20, preferably 1:1 to 3.
[0022] According to the above scheme, in step 3), the degradation time is within 20 minutes, preferably 10 to 20 minutes.
[0023] According to the above scheme, in step 3), the degradation efficiency is above 75%.
[0024] This invention provides a method for catalytically degrading antibiotics in water using solid-phase water leaching filter residue from spent lithium batteries. First, lobster shell powder and spent lithium battery cathode powder are calcined in an air atmosphere. On one hand, the local reducing atmosphere generated by the pyrolysis of the organic components of the lobster shell, the synergistic effect of carbonaceous intermediates and Ca-based mineral phases obtained from the thermal decomposition of CaCO3, alter the occurrence morphology and local chemical environment of metals such as Li, Ni, Co, and Mn in the spent lithium battery cathode powder. This promotes the deconstruction of the original layered structure and the reconstruction of transition metal oxide phases, thereby significantly improving the migration of various metal elements during the subsequent leaching process. Efficiency; simultaneously, the chitin and proteins in the lobster shell powder form a nitrogen-containing porous carbon structure during heat treatment, providing abundant surface defects and potential coordination sites for transition metal species; the resulting Ca-based inorganic phase and carbon-based structure together constitute a multiphase interface, which is beneficial for limiting the migration and aggregation of transition metal species, thereby obtaining a metal-carbon composite catalytic material with high metal dispersion and stability; on the other hand, calcination in an air atmosphere can remove organic residues (PVDF, electrolyte, organic pollutants) and improve the pore structure, while forming a metal oxide active phase and constructing carbon defect-enhanced adsorption and electron transfer. Then, the solid-phase pyrolysis residue obtained from calcination is placed in water as a leaching agent for water immersion treatment. Most of the metals in the waste lithium battery cathode powder are released by water immersion, while the carbon skeleton with a small number of transition metal oxide active sites is retained, resulting in a catalytic material with abundant defects, which is beneficial for subsequent PMS activation. Subsequently, dark adsorption was carried out at room temperature. Due to the hierarchical porous structure, oxygen- and nitrogen-containing functional groups, and uniformly dispersed active sites of transition metal oxides of the lobster shell-derived carbon-based material, antibiotic molecules in the water can be captured rapidly and in large proportion. Finally, potassium persulfate (PMS) was added, and the redox cycle of metal elements such as Ni, Co, and Mn was used to activate PMS, generating reactive oxygen species such as sulfate radicals, hydroxyl radicals, and singlet oxygen, thereby achieving efficient degradation of antibiotic pollutants in the water.
[0025] The beneficial effects of this invention are as follows: 1. This invention provides a method for catalytically degrading antibiotics in water using solid-phase water leaching filter residue from waste lithium batteries. The method utilizes the solid residue generated after lithium extraction from waste lithium batteries and lobster shell biomass as a multifunctional heterogeneous catalyst to activate potassium persulfate (PMS) for efficient degradation of antibiotic wastewater. Specifically, the lobster shell-derived biochar not only serves as an electron transport carrier but also provides abundant adsorption sites, facilitating rapid and high-proportion pre-enrichment of antibiotic molecules, thus laying an excellent interfacial kinetic foundation for subsequent efficient catalysis. Combined with the formed metal oxide active phase and the constructed carbon defects, the method exhibits a high reaction rate and purification efficiency during the catalytic activation stage, achieving deep elimination of high-concentration antibiotics within 15 minutes, demonstrating significant industrial application value.
[0026] 2. While efficiently extracting and recovering large quantities of metals such as Li / Ni / Co / Mn, the filter residue with a small amount of residual metal attached can still serve as a catalyst due to its high metal dispersion, stability, and abundant surface defects, thus achieving excellent antibiotic removal effects.
[0027] 3. This invention uses the solid phase water leaching filter residue from recycled waste lithium batteries as a catalyst, realizing high-value utilization of industrial solid waste, eliminating the secondary pressure of solid waste on the ecological environment, and greatly reducing the material costs required for wastewater treatment, thus having significant economic and environmental benefits. Attached Figure Description
[0028] Figure 1 (a) The effect of CS (lobster shell powder) dosage on the selective migration of lithium and transition metals during water immersion; (b) The effect of different calcination temperatures on the selective migration of lithium and transition metals during water immersion.
[0029] Figure 2 SEM images of waste ternary lithium battery cathode material (a), original lobster shell powder (b), calcined composite obtained in step 1) of Example 1, and residue after water immersion in step 1) of Example 1.
[0030] Figure 3 The graph shows the variation of the catalytic degradation and removal rate of chlortetracycline hydrochloride in water in different reaction systems of Comparative Examples 1-5 and Example 1. Detailed Implementation
[0031] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to specific embodiments.
[0032] Example 1 This embodiment proposes a method for catalytically degrading antibiotics in water using solid-phase water leaching filter residue from waste lithium batteries. The specific steps are as follows: S1. Catalytic material preparation: Lobster shell powder that has passed through a 100-mesh sieve is mixed with waste ternary lithium batteries (NCM622 batteries, with lithium nickel cobalt manganese oxide LiNi) as the positive electrode material. 0.6 Co 0.2 Mn 0.2O2) positive electrode powder was thoroughly mixed at a mass ratio of 2:1; the resulting material to be reacted was placed in a furnace and heated to 500 ℃ at a rate of 5 ℃ / min under air atmosphere, and calcined at a constant temperature for 30 min; the collected solid pyrolysis residue was placed in deionized water leaching agent, the liquid-to-solid ratio (g / L) was 10, mechanically stirred at 300 rpm, and the leaching time was 30 min; after leaching, the mixture was filtered, and the leaching solution rich in Li and transition metals Ni, Co, and Mn and the leaching residue were collected separately. The leaching residue was washed and dried multiple times with deionized water to obtain a solid-phase water leaching filter residue catalyst material for waste lithium battery recycling, named No Li-LB-CS. Among them, the lithium extraction rate in the leaching solution rich in Li and transition metals Ni, Co, and Mn reached 94%, and the leaching rates of Ni, Co, and Mn were 88%, 85%, and 80%, respectively, with the remainder in the leaching residue.
[0033] S2, Dark adsorption equilibrium: Add 20 mg of the No Li-LB-CS catalyst prepared in step S1 and a rotor to a 100 mL solution of chlortetracycline hydrochloride with a concentration of 20 mg / L, and adjust the magnetic stirrer to 300 r / min for dark adsorption.
[0034] S3, Catalytic activation degradation: After dark adsorption for 15 min, add 30 mg PMS.
[0035] S4. Sampling and Performance Evaluation: Small amounts of liquid were taken at specified reaction time intervals (1.0, 3.0, 5.0, 7.0, 10.0, 15.0 min), and the residual concentration of chlortetracycline hydrochloride was measured using a UV-Vis spectrophotometer. The No Li-LB-CS catalyst achieved a removal rate of 80.97% for chlortetracycline hydrochloride in water during the advanced oxidation process.
[0036] Example 2 This embodiment proposes a method for catalytically degrading antibiotics in water using solid-phase water leaching filter residue from waste lithium batteries. The specific steps are as follows: S1. Preparation of catalytic material: Lobster shell powder passing through a 100-mesh sieve was thoroughly mixed with positive electrode powder from waste ternary lithium batteries (NCM622 batteries) at a mass ratio of 4:1; the resulting material to be reacted was placed in a furnace and heated to 500 ℃ at 5 ℃ / min under an air atmosphere, and calcined at a constant temperature for 30 min; the collected solid-phase pyrolysis residue was placed in deionized water leaching agent, the liquid-to-solid ratio (g / L) of the leaching was 10, mechanically stirred at 300 rpm, and the leaching time was 30 min; after leaching, the residue was filtered, and the leaching solution rich in Li and transition metals Ni, Co, and Mn and the leaching residue were collected respectively. The leaching residue was washed and dried multiple times with deionized water to obtain the solid-phase water leaching residue catalytic material for waste lithium battery recycling.
[0037] S2, Dark adsorption equilibrium: Add 20 mg of the No Li-LB-CS catalyst prepared in step S1 and a rotor to a 100 mL solution of chlortetracycline hydrochloride with a concentration of 20 mg / L, and adjust the magnetic stirrer to 300 r / min for dark adsorption.
[0038] S3, Catalytic activation degradation: After dark adsorption for 15 min, add 30 mg PMS.
[0039] S4. Sampling and Performance Evaluation: Small amounts of liquid were taken at specified reaction time intervals (1.0, 3.0, 5.0, 7.0, 10.0, 15.0 min), and the residual concentration of chlortetracycline hydrochloride was measured using a UV-Vis spectrophotometer. The catalyst achieved a degradation rate of 78.25% of chlortetracycline hydrochloride in water during the advanced oxidation process.
[0040] Example 3 This embodiment proposes a method for catalytically degrading antibiotics in water using solid-phase water leaching filter residue from waste lithium batteries. The specific steps are as follows: S1. Preparation of Catalytic Material: Lobster shell powder passing through a 100-mesh sieve was thoroughly mixed with positive electrode powder from waste ternary lithium batteries (NCM622 batteries) at a mass ratio of 4:1. The resulting material to be reacted was placed in a furnace and heated to 600 ℃ at 5 ℃ / min under an air atmosphere, and calcined at a constant temperature for 30 min. The collected solid-phase pyrolysis residue was placed in deionized water leaching agent, with a liquid-to-solid ratio (g / L) of 10, mechanically stirred at 300 rpm, and leaching time of 30 min. After leaching, the residue was filtered, and the leaching solution rich in Li and transition metals Ni, Co, and Mn and the leaching residue were collected separately. The leaching residue was washed and dried multiple times with deionized water to obtain the solid-phase water leaching residue catalytic material for waste lithium battery recycling, named No Li-LB-CS.
[0041] S2, Dark adsorption equilibrium: Add 20 mg of the No Li-LB-CS catalyst prepared in step S1 and a rotor to a 100 mL solution of chlortetracycline hydrochloride with a concentration of 20 mg / L, and adjust the magnetic stirrer to 300 r / min for dark adsorption.
[0042] S3, Catalytic activation degradation: After dark adsorption for 15 min, add 30 mg PMS.
[0043] S4. Sampling and Performance Evaluation: Small amounts of liquid were taken at specified reaction time intervals (1.0, 3.0, 5.0, 7.0, 10.0, 15.0 min), and the residual concentration of chlortetracycline hydrochloride was measured using a UV-Vis spectrophotometer. The catalyst achieved a degradation rate of 76.98% of chlortetracycline hydrochloride in water during the advanced oxidation process.
[0044] Comparative Example 1 This comparative example serves as a performance comparison of biochar calcined solely from pure shrimp shells without the addition of battery cathode powder. The specific steps are as follows: S1. Preparation of catalytic material: The washed and dried lobster shell powder was placed directly in a furnace and heated to 500 ℃ at a heating rate of 5 ℃ / min in an air atmosphere. After calcination and holding at the temperature for 30 min, pure lobster shell biochar was obtained after cooling and named CS.
[0045] S2, Dark adsorption equilibrium: Add 20 mg of the CS catalyst prepared in step S1 and a rotor to a 100 mL solution of chlortetracycline hydrochloride with a concentration of 20 mg / L, and adjust the magnetic stirrer to 300 r / min for dark adsorption.
[0046] S3, Catalytic activation degradation: After dark adsorption for 15 min, add 30 mg PMS.
[0047] S4. Sampling and Performance Evaluation: Small amounts of liquid were taken at specified reaction time intervals, and the residual concentration of chlortetracycline hydrochloride was measured using a UV-Vis spectrophotometer. The CS catalyst achieved a removal rate of 54.34% of chlortetracycline hydrochloride in water during the advanced oxidation process over 15 minutes.
[0048] Comparative Example 2 This comparative example serves as a performance comparison of raw shrimp shell materials that have not undergone any high-temperature pyrolysis treatment. The specific steps are as follows: S1. Preparation of catalytic material: Lobster shell raw material ground into powder at room temperature is directly taken and named Raw-CS without any heat treatment.
[0049] S2, Dark adsorption equilibrium: Add 20 mg of the Raw-CS catalyst prepared in step S1 and a rotor to a 100 mL solution of chlortetracycline hydrochloride with a concentration of 20 mg / L, and set the magnetic stirrer to 300 r / min for dark adsorption.
[0050] S3, Catalytic activation degradation: After dark adsorption for 15 min, add 30 mg PMS.
[0051] S4. Sampling and Performance Evaluation: At specified reaction time intervals, a small amount of liquid was taken and the concentration of residual chlortetracycline hydrochloride was measured using a UV-Vis spectrophotometer. The Raw-CS catalyst achieved a degradation rate of 19.98% of chlortetracycline hydrochloride in water during the advanced oxidation process over 15 min.
[0052] Comparative Example 3 This comparative example was used to test the effectiveness of PMS oxidation of antibiotics in wastewater without the addition of any catalyst. The specific steps are as follows: S1. Preparation of catalytic materials: No catalytic materials were added in this comparative example.
[0053] S2, Dark Adsorption Equilibrium: Add a rotor to a 100 mL solution of chlortetracycline hydrochloride with a concentration of 20 mg / L, and adjust the magnetic stirrer to 300 r / min.
[0054] S3, Catalytic Activation Degradation: After 15 min of dark adsorption, 30 mg of PMS was added. Due to the lack of a catalyst, PMS alone has extremely limited effectiveness in the natural degradation and removal of antibiotics.
[0055] S4. Sampling and Performance Evaluation: Small amounts of liquid were taken at specified reaction time intervals, and the residual concentration of chlortetracycline hydrochloride was measured using a UV-Vis spectrophotometer. Pure PMS showed a degradation rate of 18.99% of chlortetracycline hydrochloride in water during the advanced oxidation process over 15 minutes.
[0056] Comparative Example 4 This comparative example serves as a control group that uses pure battery cathode powder catalysis in the absence of biomass porous carbon support. The specific steps are as follows: S1. Preparation of catalytic material: The positive electrode of industrial waste ternary lithium battery (NCM622 battery) is directly ground into powder without any pyrolysis or modification treatment, and named CP.
[0057] S2, Dark Adsorption Equilibrium: Add 20 mg of the CP catalyst prepared in step S1 and a rotor to a 100 mL solution of chlortetracycline hydrochloride with a concentration of 20 mg / L, and set the magnetic stirrer to 300 r / min for dark adsorption.
[0058] S3, Catalytic activation degradation: After dark adsorption for 15 min, add 30 mg PMS.
[0059] S4. Sampling and performance evaluation: A small amount of liquid was taken at the specified reaction time interval, and the concentration of residual chlortetracycline hydrochloride was measured using a UV-Vis spectrophotometer. The degradation rate of chlortetracycline hydrochloride in water by the CP catalyst was 43.71% in 15 min during the advanced oxidation process.
[0060] Comparative Example 5 This comparative example is used to compare the performance of calcined composite materials that have not undergone water immersion lithium extraction and washing and have a large amount of active metal residue on the surface. The specific steps are as follows: S1. Preparation of catalytic material: Lobster shell powder passing through a 100-mesh sieve was thoroughly mixed with waste ternary lithium battery (NCM622 battery) positive electrode powder at a mass ratio of 2:1; the resulting material to be reacted was placed in a furnace and heated to 500 ℃ at a heating rate of 5 ℃ / min under air atmosphere, and calcined at a constant temperature for 30 min. After cooling to room temperature, the solid phase pyrolysis material was directly collected without any room temperature water immersion washing or lithium extraction operation, and named LB-CS.
[0061] S2, Dark Adsorption Equilibrium: Add 20 mg of the LB-CS catalyst prepared in step S1 and a rotor to a 100 mL solution of chlortetracycline hydrochloride with a concentration of 20 mg / L, and set the magnetic stirrer to 300 r / min for dark adsorption.
[0062] S3, Catalytic activation degradation: After dark adsorption for 15 min, add 30 mg PMS.
[0063] S4. Sampling and performance evaluation: A small amount of liquid was taken at the specified reaction time interval, and the concentration of residual chlortetracycline hydrochloride was measured using a UV-Vis spectrophotometer. The degradation rate of chlortetracycline hydrochloride in water by the LB-CS catalyst was 82.16% in 15 min during the advanced oxidation process.
[0064] Therefore, although the metal loading of the composite catalyst material after water leaching for lithium extraction in Example 1 of this invention is not high, its degradation rate is not much different from that of the high-metal-loading composite material in the comparative example, and Example 1 has a faster degradation rate (see Example 1). Figure 3 (Comparison of the mid-purple and green lines) illustrates that in the catalytic material of this invention, the active metal is uniformly loaded on the biochar support, and together with the abundant defects, it produces a superior catalytic effect.
[0065] Referring to step 1) of Example 1, catalytic materials for solid-phase water leaching filter residue from waste lithium batteries were prepared by setting the mass ratio of lobster shell powder to waste ternary lithium battery cathode powder to 0.5:1 and 1:1, respectively. The effect of CS dosage on the selective migration of lithium and transition metals during water leaching was then compared with that in Examples 1 and 2. The results are shown in […]. Figure 1 (a), The figure shows: When the lobster shell powder content is insufficient (the mass ratio of lobster shell powder to spent lithium battery cathode powder is 0.5:1), only 42.8% of lithium enters the aqueous phase, while the leaching efficiency of Ni, Co, and Mn remains below 2%. This indicates that the original layered oxide framework is largely preserved, and the cascade migration process has not yet started. When the ratio of lobster shell powder to spent lithium battery cathode powder is increased to 1:1, the lithium leaching rate rises sharply to approximately 78%, while transition metals also migrate (33%~37%). This behavior suggests that the pyrolysis of lobster shell powder not only promotes lattice reconstruction but also generates sufficient reducing gases and active carbonaceous intermediates, thereby accelerating the decomposition of layered oxides. Further increasing the mass ratio of lobster shell powder to spent lithium battery cathode powder to 2:1 produces the most efficient cascade migration behavior: the lithium leaching rate reaches 94%, the leaching rates of Ni and Co are both close to approximately 88%, and Mn increases to nearly 78%. It is worth noting that further increasing the amount of lobster shell powder to 4:1 did not bring further improvement. On the contrary, it slightly reduced the migration efficiency of all elements. Excessive lobster shell powder may produce too much carbonaceous residue, which partially shields the active mineral phase and hinders interfacial mass transfer during water immersion.
[0066] Following the method in step 1) of Example 1, solid-phase water leaching filter residue catalysts for waste lithium battery recycling were prepared at calcination temperatures of 450℃ and 550℃, respectively. The effects of calcination temperature on the selective migration of lithium and transition metals during water leaching were then compared with those in Examples 1 and 3. The results are shown in […]. Figure 1 (b), as shown in the figure: Between 450 and 500 °C, lithium maintained an extremely high leaching efficiency of approximately 94%, while Ni and Co remained close to 88%, and Mn around 78%. During this stage, abundant oxygen-containing gases, nitrogen-containing substances, and newly formed porous carbon collectively constructed the most reactive gas-solid interface environment. When the temperature increased to 550 °C, the leaching efficiency of Ni, Co, and Mn decreased significantly, while lithium remained above 90%. Further heating to 600 °C resulted in a gradual decrease in lithium leaching rate, and a moderate reduction in the leaching of transition metals. Excessively high temperatures gradually consumed the active gaseous intermediates and promoted mineral sintering, thereby reducing interfacial diffusion and slowing down subsequent dissolution during the water leaching process.
[0067] Figure 2SEM images of waste ternary lithium battery cathode material (a), raw lobster shell powder (b), the calcined composite obtained in step 1) of Example 1, and the residue after water immersion in step 1) of Example 1. The images show: like Figure 2 As shown in Figure a, the cathode material of waste ternary lithium batteries consists of densely packed secondary particles with a smooth, spherical surface. In contrast, the original lobster shell powder exhibits a natural layered fibrous structure. Figure 2 (b) In this structure, calcium carbonate minerals are embedded within an organic biopolymer framework. This hierarchical structure provides both an active calcium precursor and a renewable carbon source for constructing the biomass-derived reaction microenvironment. After co-calcination at 500 °C, the original morphologies of both components almost completely disappeared. Figure 2 c). The cathode particles partially fragmented and were tightly embedded in the carbonaceous matrix generated by biomass pyrolysis. Simultaneously, a large number of nanoscale mineral particles were uniformly distributed on the reconstructed interface, indicating that biomass pyrolysis, carbonate decomposition, cathode reduction, and mineral nucleation occurred synergistically in the same local reaction environment, rather than as isolated processes. This interface reconstruction significantly expanded the gas-solid contact area and established abundant reaction interfaces for the migration of coupled elements. After water immersion, the reconstructed composite material evolved into a highly porous hierarchical framework (…). Figure 2 d). The dissolution of water-soluble lithium salts creates numerous interconnected pores while preserving the integrity of the carbon framework. Meanwhile, cobalt, nickel, and manganese remain uniformly anchored throughout the porous carbon framework, retaining transition metal active sites. This selective elemental redistribution simultaneously constructs open diffusion channels and exposes abundant catalytically active interfaces, providing an ideal structural platform for subsequent persulfate (PMS) activation.
[0068] Figure 3 This is a graph showing the variation in the catalytic degradation and removal rate of chlortetracycline hydrochloride in water for different reaction systems in Comparative Examples 1-5 and Example 1. Combined with... Figure 3 Analysis of the changing trends shows that when the solid phase water leaching filter residue (No Li-LB-CS) generated during the recycling of waste lithium batteries is used as a heterogeneous catalyst in the embodiments of the present invention, due to the natural and compact in-situ construction of highly active residual transition metal sites and layered porous biomass carbon skeleton generated by shrimp shell pyrolysis, it exhibits good adsorption-catalysis dual-effect synergistic removal efficiency in the process of activating the advanced oxidant PMS. Various technical indicators and reaction rates significantly exceed most comparative systems, achieving the dual effect of green and low-carbon recycling of secondary resources and low-cost water environment treatment.
[0069] The specific embodiments of the present invention described above do not constitute a limitation on the scope of protection of the present invention. Any other corresponding changes and modifications made in accordance with the technical concept of the present invention should be included within the scope of protection of the present invention.
Claims
1. A resource recovery method based on lithium extraction and transition metal leaching from waste lithium batteries and catalytic degradation of antibiotics in water, characterized in that, Includes the following steps: 1) Lobster shell powder is thoroughly mixed with waste lithium battery cathode powder and then calcined in air to obtain solid-phase pyrolysis residue; the obtained solid-phase pyrolysis residue is subjected to water leaching treatment to extract lithium and transition metals Ni, Co, and Mn, and the leaching solution rich in lithium and transition metals and the water leaching filter residue are collected. Then the water leaching filter residue is washed and dried to obtain waste lithium battery recycling solid-phase water leaching filter residue catalyst material; wherein: the waste lithium battery is a nickel-cobalt-manganese ternary lithium battery; 2) Add the waste lithium battery recycling solid phase water leaching filter residue catalyst material prepared in step 1) to the antibiotic wastewater, stir to carry out dark adsorption until dark adsorption equilibrium is reached; 3) Add PMS to the reaction system obtained in step 2) to carry out the catalytic degradation of antibiotics.
2. The method according to claim 1, characterized in that, In step 1), the mass ratio of lobster shell powder to waste lithium battery cathode powder is 1.5~4:
1.
3. The method according to claim 1, characterized in that, In step 1), the roasting temperature is 400~600℃ and the time is 30~60 min.
4. The method according to claim 1, characterized in that, In step 1), the water immersion time is 10-30 min; the liquid-to-solid ratio during water immersion treatment is 5-20 g / L.
5. The method according to claim 1, characterized in that, In step 1), after water immersion treatment, the lithium leaching rate in the lithium-rich filtrate reaches over 90%; the leaching rates of Ni, Co, and Mn are independently over 85%.
6. The method according to claim 1, characterized in that, In step 2), the mass ratio of the catalytic material to the antibiotic is 5~15:
1.
7. The method according to claim 1, characterized in that, In step 2), the dark adsorption time is 10~30 min.
8. The method according to claim 1, characterized in that, In step 2), the antibiotic is a tetracycline, quinolone, sulfonamide, or β-lactam antibiotic.
9. The method according to claim 1, characterized in that, In step 2), the concentration of antibiotic wastewater is 5~100 mg / L.
10. The method according to claim 1, characterized in that, In step 3), the mass ratio of the catalyst material to PMS is 1:1 to 20; the degradation time is within 20 minutes.
Citation Information
Patent Citations
Resource utilization method of waste lithium ion battery
CN115739108A