A method for extracting TiCl4 from TiO2-containing slag
By adding an iron source to high-titanium blast furnace slag to reconstruct titanium into the Fe2TiO4 phase and using magnetic separation, the problem of efficient titanium resource recovery was solved, and efficient extraction and purity improvement of titanium in high-titanium blast furnace slag were achieved.
Patent Information
- Application Number
- CN202611373036.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-04
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies are difficult to efficiently process titanium resources dispersed in high-titanium blast furnace slag, and the process is complex, with low titanium extraction rate and high cost.
By adding an iron source, the dispersed titanium in titanium-containing blast furnace slag is reconstructed into an easily separable Fe2TiO4 phase. Phase separation is achieved using magnetic separation, followed by molten salt chlorination and condensation separation to obtain TiCl4.
It has achieved efficient recovery of titanium resources from high-titanium blast furnace slag, with a titanium extraction rate of over 80% and a purity of 95.6%~98.2%, thereby reducing overall production costs.
Smart Images

Figure CN123108322A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of chemical technology, specifically relating to a method for extracting TiCl4 from TiO2-containing slag. Background Technology
[0002] Panzhihua region is rich in titanium resources, accounting for over 90% of my country's total titanium resources, mostly vanadium-titanium magnetite. Current technologies primarily employ a process route of first selecting iron and then titanium. Through the traditional blast furnace ironmaking process, titanium resources ultimately end up in the blast furnace slag. Therefore, the blast furnace slag is a unique high-titanium type produced by vanadium-titanium magnetite smelting, with a TiO2 content of approximately 20-24%. There is currently no method for the industrial reuse of this titanium-containing blast furnace slag. Apart from a small amount crushed and used for industrial building materials such as roadbed materials, most of it is still stockpiled. The current stockpile is over 65 million tons, equivalent to over 13 million tons of TiO2 reserves, and it continues to grow at a rate of 7 million tons of waste blast furnace slag per year.
[0003] Domestic and international scholars and research institutions have conducted extensive research on the utilization of high-titanium blast furnace slag, proposing various methods such as "production of titanium-silicon (aluminum) alloys from high-titanium blast furnace slag," "acid leaching extraction of TiO2," "alkali molten salt calcination extraction of titanium," "mineral processing separation of perovskite," "selective separation after high-temperature modification and enrichment," "high-temperature carbonization-mineral processing separation of titanium carbide," and "high-temperature carbonization-low-temperature chlorination." However, most of these studies are currently still in the laboratory basic research stage, and all suffer from problems such as complex process flows, low titanium extraction rates, and high costs.
[0004] Chinese patent CN107758729A discloses a modification process for high-calcium-magnesium-titanium slag. This process involves adding fluorides as modifiers to the high-temperature reaction system of a fluidized bed chlorination furnace or the high-temperature molten slag system of an electric furnace used to prepare high-calcium-magnesium-titanium slag. This chemically modifies the calcium and magnesium impurities carried by the high-calcium-magnesium-titanium slag into stable solid components such as CaF2, CaAlF5, and MgF2. However, this process only modifies the calcium and magnesium impurities in the chlorination system in situ and does not recover the dispersed titanium components in the stockpiled high-titanium blast furnace slag, limiting the applicability of the raw materials. Furthermore, all slag material directly enters the chlorination reaction, resulting in a high impurity load. It also requires fluoride modification agents, leading to increased agent costs and a burden of treating fluorine-containing tail gas. Additionally, it cannot utilize the sensible heat of the molten blast furnace slag, resulting in high overall operating costs.
[0005] Chinese patent CN120081415A discloses a method for preparing titanium tetrachloride from molten titanium slag through gas-based reduction carbonization and molten salt chlorination. The method includes: grinding titanium slag obtained from hydrogen reduction and electric furnace smelting of vanadium-titanium magnetite concentrate to a certain particle size; placing the titanium slag obtained in the first step in a tubular furnace and heating it to 1100–1300°C, while simultaneously introducing a mixed gas of methane and hydrogen to react and obtain a carbonization product; mixing the carbonization product obtained in the second step with a chloride salt and carrying out a chlorination reaction at a certain temperature to produce crude titanium tetrachloride. However, this method is only applicable to molten titanium slag and cannot directly process the large stockpiles of high-titanium blast furnace slag. Furthermore, it requires a methane-hydrogen mixed gas for gas-based carbonization, which demands strict atmosphere control and significant equipment investment; and it lacks a magnetic separation pre-removal process, with all gangue impurities entering the entire carbonization-chlorination process, resulting in high overall energy consumption and increased industrial safety management costs due to the flammable and explosive process gases.
[0006] Therefore, how to develop a method that can directly process stockpiled high-titanium blast furnace slag and recover titanium dispersed in the slag, while having a simple process, high titanium extraction efficiency, and lower overall production cost, is a technical problem that urgently needs to be solved in this field. Summary of the Invention
[0007] To address the shortcomings of existing technologies, the main objective of this invention is to provide a method for extracting TiCl4 from TiO2-containing blast furnace slag. By adding an iron source, the dispersed titanium in titanium-containing blast furnace slag is reconstructed into a uniform and easily separable Fe2TiO4 phase. Then, phase separation is achieved through magnetic separation to obtain a magnetic concentrate with a high TiO2 grade. Subsequently, the magnetic concentrate is subjected to molten salt chlorination and condensation separation to obtain TiCl4, thus realizing the overall recovery of titanium from the slag. This process is simple, has high titanium extraction efficiency, and lower overall production costs.
[0008] According to one aspect of the present invention, a method for extracting TiCl4 from TiO2-containing slag is provided, the method comprising the following steps: S1. TiO2-containing slag, iron source and reducing agent are mixed and calcined to obtain modified slag; S2. The modified slag is subjected to crushing, fine grinding and magnetic separation in sequence to obtain magnetic concentrate; S3. The metal chloride is heated to melt to obtain molten salt. The molten salt, the magnetic concentrate and the reducing agent are mixed and chlorine gas is introduced to react and obtain mixed chloride. S4. The mixed chloride is continuously condensed in two stages. After the first stage of condensation, a first-stage condensation product containing FeCl3 is obtained; after the second stage of condensation, a second-stage condensation product containing TiCl4 is obtained.
[0009] According to one embodiment of the present invention, in S1, the mass fraction of TiO2 in the TiO2-containing slag is 10%-90%, and the remainder is impurities, which contain CaO, MgO, SiO2 and Al2O3; In S1, the iron source is an iron-containing oxide, which is Fe2O3 and / or iron concentrate; In S1 and S3, the reducing agent is independently selected from at least one of petroleum coke, metallurgical coke, pulverized coal, and graphite.
[0010] According to one embodiment of the present invention, in S1, the mass ratio of TiO2, iron source and reducing agent in the TiO2-containing slag is 1:(2~3):(0.18~0.22), wherein the mass of the iron source is calculated as Fe2O3.
[0011] According to one embodiment of the present invention, in S1, the calcination temperature is 1350~1650°C.
[0012] According to one embodiment of the present invention, in S2, after the crushing and fine grinding process, powder is obtained, wherein the mass percentage of particles that can pass through a 150-mesh sieve in the powder is ≥70%. In step S2, the magnetic field strength of the magnetic separation process is 0.8~1.5T.
[0013] According to one embodiment of the present invention, in S3, the metal chloride is NaCl and / or KCl.
[0014] According to one embodiment of the present invention, in S3, the mass ratio of the magnetic concentrate, reducing agent and chlorine is 1:(0.24-0.32):(1.50-2.30).
[0015] According to one embodiment of the present invention, in S3, the temperature of the reaction is 700~900°C.
[0016] According to one embodiment of the present invention, in S4, the temperature of the first stage of condensation is 850~250°C; The temperature for the second stage of condensation is 250~130℃.
[0017] According to one embodiment of the present invention, in step S4, the purity of TiCl4 is 95.6%~98.2%, and the titanium extraction rate is 80.8%~90.3%.
[0018] By adopting the above technical solution, the present invention has the following advantages compared with the prior art: 1) This invention reconstructs the dispersed titanium in titanium-containing blast furnace slag into a uniform and easily separable Fe2TiO4 phase by adding an iron source. Then, the phase is separated by magnetic separation, so that the titanium-containing phase is enriched in the magnetic concentrate. This enables the recovery and utilization of titanium resources in TiO2-containing slag, and the titanium extraction rate can reach more than 80%, which has good economic value.
[0019] 2) When this invention is industrialized, the sensible heat of the slag can be utilized. An iron source and a reducing agent are added to the chute during the process of loading liquid slag into the electric furnace, and the liquid slag is directly heated to the reaction temperature to complete the slag modification. Attached Figure Description
[0020] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.
[0021] Figure 1 The following is a flowchart of a method for extracting TiCl4 from TiO2-containing slag according to an embodiment of the present invention. Figure I ; Figure 2 The following is a flowchart of a method for extracting TiCl4 from TiO2-containing slag according to an embodiment of the present invention. Figure II . Detailed Implementation
[0022] To make the objectives, technical solutions, and advantages of the present invention clearer, the embodiments of the present invention will be further described in detail below with reference to specific examples and the accompanying drawings.
[0023] It should be understood that the embodiments of the invention shown in the exemplary embodiments are merely illustrative. Although only a few embodiments have been described in detail in this invention, those skilled in the art will readily recognize that various modifications are possible without substantially departing from the teachings of the invention. Accordingly, all such modifications should be included within the scope of the invention. Other substitutions, modifications, variations, and deletions can be made to the design, operating conditions, and parameters of the following exemplary embodiments without departing from the spirit of the invention.
[0024] like Figure 1 , 2As shown, a method for extracting TiCl4 from TiO2-containing slag includes the following steps: S1, mixing TiO2-containing slag, an iron source, and a reducing agent, and calcining to obtain modified slag; S2, sequentially crushing, fine grinding, and magnetic separation of the modified slag to obtain magnetically separated concentrate; S3, heating a metal chloride to melt to obtain molten salt, mixing the molten salt, magnetically separated concentrate, and reducing agent, and introducing chlorine gas to react and obtain mixed chloride; S4, continuously condensing the mixed chloride in two stages. After the first stage of condensation, a first-stage condensation product containing FeCl3 is obtained; after the second stage of condensation, a second-stage condensation product containing TiCl4 is obtained. This process reconstructs the dispersed titanium in titanium-containing blast furnace slag into a uniform and easily separable Fe2TiO4 phase by adding an iron source. Then, phase separation is achieved through magnetic separation to obtain a magnetic concentrate with a high TiO2 grade. Subsequently, the magnetic concentrate is subjected to molten salt chlorination and condensation separation to obtain TiCl4, thus realizing the overall recovery of titanium from the slag. This process is simple, has high titanium extraction efficiency, and lower overall production cost.
[0025] In S1, the mass fraction of TiO2 in the TiO2-containing slag is 10%-90%, with the remainder being impurities containing CaO, MgO, SiO2, and Al2O3. In S1, the iron source is an iron oxide, specifically Fe2O3 and / or iron concentrate. In both S1 and S3, the reducing agent is independently selected from at least one of petroleum coke, metallurgical coke, pulverized coal, and graphite. In S1, the mass ratio of TiO2, iron source, and reducing agent in the TiO2-containing slag is 1:(2~3):(0.18~0.22), where the iron source is calculated as Fe2O3, meaning the amount of iron source added is 200%~300% of the mass of TiO2 in the slag, and the amount of reducing agent added is 6%~11% of the amount of iron source added. In S1, the calcination temperature is 1350~1650℃.
[0026] In S2, after crushing and fine grinding, powder is obtained, and the mass percentage of particles that can pass through a 150-mesh sieve is ≥70%; in S2, the magnetic field strength of the magnetic separation process is 0.8~1.5T.
[0027] In S3, the metal chlorides are NaCl and / or KCl. In S3, the mass ratio of magnetic concentrate, reducing agent, and chlorine is 1:(0.24–0.32):(1.50–2.30). In S3, the reaction temperature is 700–900℃. During molten salt chlorination, the reaction temperature is controlled by adding cooled crude TiCl4 to the reactor. Simultaneously, the refractory molten salt in the molten salt chlorination furnace is periodically drained to maintain a stable molten salt level within the furnace.
[0028] In S4, the temperature of the first stage condensation is 850~250℃; the temperature of the second stage condensation is 250~130℃. The first stage causes high-boiling-point impurity chlorides such as FeCl3 to preferentially condense and precipitate; the second stage condenses and collects the target product TiCl4, realizing the fractional separation of impurities and target product and improving the purity of TiCl4 product.
[0029] In S4, the purity of TiCl4 is 95.6%~98.2%, and the overall extraction rate of titanium is 80.8%~90.3%.
[0030] The following are specific embodiments and process parameters of the method for extracting TiCl4 from TiO2-containing slag according to the present invention.
[0031] Example 1 The composition of TiO2-containing slag is as follows: TiO2 23.63%, CaO 25.23%, SiO2 24.98%, MgO 7.01%, Al2O3 13.78%, and other impurities 5.37%.
[0032] TiO2 slag was modified and calcined using a muffle furnace. 1000g of slag was mixed with 472g of Fe2O3 and 44g of petroleum coke. The mixture was then placed in a graphite crucible, which was then placed in the muffle furnace and heated to 1500℃ for 30 minutes. The mixture was then cooled with the furnace to obtain the modified slag.
[0033] The modified slag was removed from the muffle furnace, crushed, and finely ground to prepare powder with a particle size of -150 mesh ≥70%. The finely ground roasted ore was subjected to magnetic separation with a magnetic field strength of 1.5T to obtain magnetic concentrate, which was used as raw material for molten salt chlorination reaction. The titanium grade of the magnetic concentrate was measured to be 19.2%.
[0034] Add 50 kg of solid sodium chloride to the molten salt as chloride molten salt, heat to melt the solid molten salt, then mix 500 g of magnetic separation concentrate with 120 g of petroleum coke and add it to the liquid molten salt to react. At the same time, 1140 g of chlorine gas is introduced into the molten salt. The molten salt chlorination reaction temperature is 800-900℃.
[0035] A two-stage cooling process was adopted. The first stage of cooling and separation was carried out at a temperature of 850~250℃ to obtain chlorides such as FeCl3. The second stage of cooling and separation was carried out at a temperature of 250~130℃ to obtain chlorides containing product TiCl4. The purity of TiCl4 was determined to be 95.6%, and the overall extraction rate of titanium was 80.8%.
[0036] Example 2 The composition of TiO2-containing slag is as follows: TiO2 76.10%, CaO 2.65%, MgO 7.89%, SiO2 4.69%, Al2O3 2.78%, and other impurities 5.89%.
[0037] TiO2 slag was modified and calcined using a muffle furnace. 1000g of slag was mixed with 1903g of Fe2O3 and 143g of petroleum coke. The mixture was then placed in a graphite crucible, which was then placed in the muffle furnace and heated to 1500℃ for 30 minutes. The mixture was then cooled with the furnace to obtain the modified slag.
[0038] The modified slag was removed from the muffle furnace, crushed, and finely ground to prepare powder with a particle size of -150 mesh ≥70%. The finely ground roasted ore was subjected to magnetic separation with a magnetic field strength of 1.2T to obtain magnetic concentrate, which was used as raw material for molten salt chlorination reaction. The titanium dioxide grade of the magnetic concentrate was measured to be 20.4%.
[0039] Add 50 kg of solid sodium chloride to the molten salt as chloride molten salt, heat to melt the solid molten salt, then mix 500 g of magnetic separation concentrate with 156 g of petroleum coke and add it to the liquid molten salt to react. At the same time, 983 g of chlorine gas is introduced into the molten salt. The molten salt chlorination reaction temperature is 800-900℃.
[0040] A two-stage cooling process was adopted. The first stage of cooling and separation was carried out at a temperature of 850~250℃ to obtain chlorides such as FeCl3. The second stage of cooling and separation was carried out at a temperature of 250~130℃ to obtain chlorides containing product TiCl4. The purity of TiCl4 was determined to be 96.6%, and the overall extraction rate of titanium was 84.4%.
[0041] Example 3 The composition of TiO2-containing slag is as follows: TiO2 90.2%, CaO 25.23%, SiO2 24.98%, MgO 7.01%, Al2O3 13.78%, and other impurities 5.37%.
[0042] TiO2 slag was modified and calcined using a muffle furnace. 1000g of slag was mixed with 2706g of Fe2O3 additive and 198g of reducing agent. The mixture was then placed in a graphite crucible, which was then placed in the muffle furnace and heated to 1500℃ for 30 minutes. The furnace was then cooled with the slag to obtain the modified slag.
[0043] The modified slag was removed from the muffle furnace, crushed, and finely ground to prepare powder with a particle size of -150 mesh ≥70%. The finely ground roasted ore was subjected to magnetic separation with a magnetic field strength of 0.8T to obtain magnetic concentrate, which was used as raw material for molten salt chlorination reaction. The titanium dioxide grade of the magnetic concentrate was measured to be 21.0%.
[0044] Add 50 kg of solid sodium chloride to the molten salt as chloride molten salt, heat to melt the solid molten salt, then mix 500 g of magnetic separation concentrate with 159 g of petroleum coke and add it to the liquid molten salt to react. At the same time, 753 g of chlorine gas is introduced into the molten salt. The molten salt chlorination reaction temperature is 800-900℃.
[0045] A two-stage cooling process was adopted. The first stage of cooling and separation was carried out at a temperature of 850~250℃ to obtain chlorides such as FeCl3. The second stage of cooling and separation was carried out at a temperature of 250~130℃ to obtain chlorides containing product TiCl4. The purity of TiCl4 was determined to be 98.2%, and the overall extraction rate of titanium was 90.3%.
[0046] Comparative Example 1 The preparation method in Comparative Example 1 involved no calcination modification or magnetic separation; all other operations were the same as in Example 1, as detailed below: The composition of TiO2-containing slag is as follows: TiO2 23.63%, CaO 25.23%, SiO2 24.98%, MgO 7.01%, Al2O3 13.78%, and other impurities 5.37%.
[0047] Take 1000g of slag, crush and grind it finely to prepare powder with a particle size of -150 mesh ≥70%, and obtain slag powder. Add 50kg of solid sodium chloride to the molten salt chlorination furnace as molten salt, heat to melt the solid molten salt, and then mix 500g of slag powder with 120g of petroleum coke and add it to the liquid molten salt for reaction. At the same time, 1140g of chlorine gas is introduced into the molten salt. The molten salt chlorination reaction temperature is 800~900℃.
[0048] A two-stage cooling process was adopted. The first stage of cooling and separation was carried out at a temperature of 850~250℃ to obtain chlorides such as FeCl3. The second stage of cooling and separation was carried out at a temperature of 250~130℃ to obtain chlorides containing product TiCl4. The purity of TiCl4 was determined to be 92.6%, and the overall extraction rate of titanium was 25.8%.
[0049] As shown in Examples 1-3, this invention, by adding an iron source, reconstructs the dispersed titanium in titanium-containing blast furnace slag into a uniform and easily separable Fe2TiO4 phase. Then, phase separation is achieved through magnetic separation to obtain a high-grade TiO2 magnetic concentrate. Subsequently, the magnetic concentrate undergoes molten salt chlorination and condensation separation to obtain TiCl4, thus achieving overall titanium recovery from the slag. The titanium extraction rate is 80.8%–90.3%, and the purity reaches 95.6%–98.2%. In contrast, the preparation method in Comparative Example 1, without roasting modification or magnetic separation, only includes molten salt chlorination and condensation separation. Because titanium remains dispersed and embedded in the gangue matrix, encapsulated by pyroxene and other components, its reactivity is poor, resulting in a lower titanium extraction rate. Simultaneously, a large amount of calcium and magnesium impurities directly enter the chlorination system, causing impurities to continuously accumulate in the molten salt, leading to rapid deterioration and significant consumption of the molten salt. In summary, the various process steps in this invention cooperate and work synergistically to achieve efficient overall titanium recovery from blast furnace slag.
[0050] The above are merely preferred embodiments of the present invention and are not intended to limit the scope of the present invention. Any modifications or equivalent substitutions made to the present invention without departing from the spirit and scope thereof should be covered within the protection scope of the claims of the present invention.
[0051] Those skilled in the art should understand that the discussion of any of the above embodiments is merely exemplary and is not intended to imply that the scope of the disclosed embodiments of the present invention is limited to these examples; within the framework of the embodiments of the present invention, the technical features of the above embodiments or different embodiments can also be combined, and there are many other variations of different aspects of the embodiments of the present invention as described above, which are not provided in detail for the sake of brevity. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the embodiments of the present invention should be included within the protection scope of the embodiments of the present invention.
Claims
1. A method for extracting TiCl4 from TiO2-containing slag, characterized in that, The method includes the following steps: S1. TiO2-containing slag, iron source and reducing agent are mixed and calcined to obtain modified slag; S2. The modified slag is subjected to crushing, fine grinding and magnetic separation in sequence to obtain magnetic concentrate; S3. The metal chloride is heated to melt to obtain molten salt. The molten salt, the magnetic concentrate and the reducing agent are mixed and chlorine gas is introduced to react and obtain mixed chloride. S4. The mixed chloride is continuously condensed in two stages. After the first stage of condensation, a first-stage condensation product containing FeCl3 is obtained; after the second stage of condensation, a second-stage condensation product containing TiCl4 is obtained.
2. The method according to claim 1, characterized in that, In S1, the mass fraction of TiO2 in the TiO2-containing slag is 10%-90%, and the remainder is impurities, which contain CaO, MgO, SiO2 and Al2O3. In S1, the iron source is an iron-containing oxide, which is Fe2O3 and / or iron concentrate; In S1 and S3, the reducing agent is independently selected from at least one of petroleum coke, metallurgical coke, pulverized coal, and graphite.
3. The method according to claim 1, characterized in that, In S1, the mass ratio of TiO2, iron source and reducing agent in the TiO2-containing slag is 1:(2~3):(0.18~0.22), wherein the mass of the iron source is calculated as Fe2O3.
4. The method according to claim 1, characterized in that, In S1, the calcination temperature is 1350~1650℃.
5. The method according to claim 1, characterized in that, In S2, after the crushing and fine grinding process, powder is obtained, and the mass percentage of particles that can pass through a 150-mesh sieve in the powder is ≥70%. In step S2, the magnetic field strength of the magnetic separation process is 0.8~1.5T.
6. The method according to claim 1, characterized in that, In S3, the metal chloride is NaCl and / or KCl.
7. The method according to claim 1, characterized in that, In step S3, the mass ratio of the magnetic concentrate, reducing agent, and chlorine is 1:(0.24-0.32):(1.50-2.30).
8. The method according to claim 1, characterized in that, In step S3, the reaction temperature is 700~900℃.
9. The method according to claim 1, characterized in that, In S4, the temperature of the first stage of condensation is 850~250℃; The temperature for the second stage of condensation is 250~130℃.
10. The method according to claim 1, characterized in that, In S4, the purity of TiCl4 is 95.6%~98.2%, and the titanium extraction rate is 80.8%~90.3%.
Citation Information
Patent Citations
High-calcium-magnesium-titanium dreg modification treatment process
CN107758729A
Method for preparing titanium tetrachloride through melt separation titanium slag gas-based reduction carbonization-fused salt chlorination
CN120081415A