Titration and extraction method of titanium-rich slag
By subjecting titanium-rich slag to rapid and slow cooling treatments, combined with dilute acid leaching and concentrated sulfuric acid acidolysis, and by separating the slag according to the vanadium-titanium ratio, chromium-titanium ratio, and aluminum-titanium ratio, the problem of low resource utilization caused by the complex composition of titanium-rich slag and different cooling methods is solved, achieving efficient titanium resource recovery and purity improvement.
Patent Information
- Application Number
- CN202611549528.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-08
- Publication Date
- 2026-11-17
AI Technical Summary
In existing technologies, titanium-rich slag has a complex composition and different cooling methods, making it difficult to use a single route for treatment. This results in low resource utilization, and the entry of impurities into the liquid phase increases the burden and treatment cost of subsequent titanium liquid purification.
By subjecting titanium-rich slag to rapid and slow cooling treatments, and then pulverizing it separately, titanium products of different grades are prepared by leaching impurities with dilute acid and acid hydrolysis with concentrated sulfuric acid, and by precisely separating the titanium liquid according to the vanadium-titanium ratio, chromium-titanium ratio and aluminum-titanium ratio.
It enables precise classification and differentiated treatment of titanium-rich slag with different characteristics, improves resource recovery efficiency, reduces the negative impact of acid consumption and impurities on product color, and enhances the purity and utilization rate of titanium liquid.
Smart Images

Figure CN123108323A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of metallurgical and chemical technology, and in particular to a method for graded extraction of titanium-rich slag. Background Technology
[0002] my country possesses abundant vanadium-titanium resources. With the development of hydrogen metallurgy technology, the synergistic process of gas-based vertical shaft furnace reduction and electric furnace smelting can produce high-grade titanium-rich slag when processing vanadium-titanium magnetite. The efficient extraction and full resource utilization of this titanium-rich slag are of great significance for improving the utilization rate of mineral resources.
[0003] Titanium-rich slag has a complex composition, with significant variations in the content of impurities (such as Al2O3, V2O5, and Cr2O3). Furthermore, differences in cooling methods during the upstream smelting process lead to substantial variations in the internal mineral phase structure of the titanium-rich slag.
[0004] In existing technologies, to address the issue of titanium slag resource utilization, a non-blast furnace titanium slag sulfuric acid process for producing titanium dioxide, as disclosed in a related technology, is commonly used. This method involves finely grinding the titanium slag, mixing it with waste acid from titanium dioxide hydrolysis for pretreatment, then adding concentrated sulfuric acid for acidolysis and ripening, followed by slurry leaching to obtain titanium liquid. However, this approach fails to consider the significant differences in the mineral phase structure of titanium-rich slag under different cooling methods (rapid cooling and slow cooling), employing a "one-size-fits-all" concentrated sulfuric acid acidolysis process. This results in high acid consumption and the introduction of numerous impurities into the liquid phase for rapidly cooled slag with high glass content, increasing the burden and processing cost of subsequent titanium liquid purification.
[0005] To improve the acidolysis efficiency of titanium slag, another related technology discloses a method to increase the acidolysis rate of titanium slag. This method promotes the nucleation and growth of the zeolite phase by controlling the slow cooling process of the titanium slag, and then mixes the cooled titanium slag with sulfuric acid and heats it for acidolysis. However, although this scheme optimizes the acidolysis performance of the slow-cooled slag, it still lacks targeted separation methods for complex associated impurities (such as vanadium, chromium, and aluminum) in the titanium liquid. In the subsequent concentration and hydrolysis processes, high aluminum content easily induces gelation, while vanadium and chromium significantly affect the hue and whiteness of the final titanium dioxide, making it difficult to achieve the high-value-added, tiered utilization of multiple metal elements.
[0006] Furthermore, another related technology discloses a method for preparing titanium dioxide from titanium slag obtained by direct reduction of titanium iron oxide. This method first pre-leaches the titanium slag with hydrochloric acid to remove impurities, and then mixes the titanium-rich hydrochloric acid leaching residue after solid-liquid separation with sulfuric acid for heated acid hydrolysis. However, in this scheme, hydrochloric acid leaching and concentrated sulfuric acid acid hydrolysis are used in series on the same batch of titanium slag, resulting in a long process flow and high reagent consumption. Simultaneously, this scheme also fails to accurately separate the slag based on the specific content of vanadium, chromium, and aluminum in the titanium solution, leading to a relatively simple processing route and making it difficult to simultaneously meet the high purity requirements of pigment-grade products and the comprehensive recovery of associated resources. This application addresses these shortcomings. Summary of the Invention
[0007] In view of this, the purpose of this application is to provide a method for graded extraction of titanium-rich slag, so as to improve the problem that the existing technology makes it difficult to use a single route to process titanium-rich slag due to its complex composition and different cooling methods, resulting in low resource utilization.
[0008] To achieve the above objectives, this application provides a method for graded extraction of titanium-rich slag, comprising the following steps: S1. The titanium-rich slag is subjected to rapid cooling and slow cooling respectively to obtain rapidly cooled slag and slow cooled slag; the rapidly cooled slag and slow cooled slag are respectively ground into powder to obtain rapidly cooled slag powder and slow cooled slag powder. S2. The rapidly cooled slag powder is leached with dilute acid to remove impurities, and then filtered, washed and dried in sequence to obtain titanium-rich material; the dilute acid is an acidic medium with a mass fraction of 5% to 30%. S3. The slow-cooling slag powder is acidified and matured with concentrated sulfuric acid, and then leached and filtered with a leaching solution to obtain acidified slag and titanium liquid. S4. The titanium liquid is divided into high vanadium-chromium titanium liquid and low vanadium-chromium titanium liquid according to the vanadium-titanium ratio and chromium-titanium ratio. S5. The high-vanadium-chromium titanium solution is directly hydrolyzed to separate and obtain first metatitanic acid; and / or, some vanadium and / or chromium in the high-vanadium-chromium titanium solution is removed to obtain low-vanadium-chromium titanium solution. S6. According to the aluminum-titanium ratio, the low-vanadium-chromium titanium solution is divided into high-aluminum titanium solution and low-aluminum titanium solution; the high-aluminum titanium solution is concentrated after aluminum removal, and the low-aluminum titanium solution is directly concentrated to obtain concentrated titanium solutions respectively; the concentrated titanium solutions are hydrolyzed and washed to obtain second metatitanic acid.
[0009] In some embodiments, in step S1, the titanium-rich slag is one or more of the following: vanadium-titanium magnetite gas-based direct reduction slag, coal-based direct reduction slag, biomass direct reduction slag, molten reduction slag, plasma reduction slag, blast furnace slag, hydrometallurgical slag, and titanium-containing tailings after mineral processing.
[0010] In some embodiments, in step S1, the mass percentage of slag powder passing through a 325-mesh sieve in the rapidly cooled slag powder and the slowly cooled slag powder is not less than 95%.
[0011] In some embodiments, in step S1, the rapid cooling method includes water quenching or hot water splashing cooling.
[0012] In some embodiments, in step S1, the slow cooling method includes heat preservation slow cooling with an average cooling rate not exceeding 5°C / min.
[0013] In some embodiments, in step S2, the mass fraction of TiO2 in the obtained titanium-rich material is not less than 70%, and the titanium-rich material is used as a raw material for sulfuric acid titanium dioxide, molten salt chlorination or boiling chlorination.
[0014] In some embodiments, in step S3, the leaching solution is one or more of water, dilute acid water, and dilute titanium solution; the dilute acid water contains 5% to 30% acidic medium by mass, and the titanium concentration in the dilute titanium solution, calculated as TiO2, is 80 to 150 g / L.
[0015] In some embodiments, in step S4, the high vanadium-chromium titanium liquid has a vanadium-titanium ratio greater than or equal to 1×10⁻⁶. -2 Or, the chromium-to-titanium ratio is greater than or equal to 0.5 × 10⁻� -2 The titanium liquid is a low-vanadium-chromium titanium liquid with a vanadium-titanium ratio of less than 1×10⁻⁶. -2 And the chromium-to-titanium ratio is less than 0.5×10 -2 liquid titanium.
[0016] In some embodiments, in step S4, the titanium concentration in the high vanadium chromium titanium liquid, calculated as TiO2, is 80~150 g / L.
[0017] In some embodiments, in step S5, the first metatitanic acid is used as an additive in the preparation of ceramics, enamels, or welding electrodes.
[0018] In some embodiments, step S5 further includes: calcining the first metatitanic acid to obtain a first titanium dioxide or synthetic rutile.
[0019] In some embodiments, step S5 further includes: obtaining vanadium-rich products and / or chromium-rich products, wherein obtaining vanadium-rich products and / or chromium-rich products includes: separating and recovering vanadium-rich products and / or chromium-rich products from waste acid after separating the first metatitanic acid from the hydrolysis of the high vanadium-chromium titanium liquid; and / or, recovering a portion of the vanadium and / or chromium removed from the high vanadium-chromium titanium liquid to obtain vanadium-rich products and / or chromium-rich products.
[0020] In some embodiments, in step S6, the high-aluminum titanium liquid is a low-vanadium-chromium titanium liquid with an aluminum-to-titanium ratio greater than or equal to 0.25, and the low-aluminum titanium liquid is a low-vanadium-chromium titanium liquid with an aluminum-to-titanium ratio less than 0.25.
[0021] In some embodiments, in step S6, the aluminum removal method of the high-alumina titanium liquid includes: adding sulfate to the high-alumina titanium liquid to precipitate aluminum, or freezing the high-alumina titanium liquid to allow aluminum sulfate to crystallize out and separate from the titanium liquid, thereby obtaining aluminum-containing acid slag.
[0022] In some embodiments, in step S6, the titanium concentration in the concentrated titanium solution, calculated as TiO2, is 180~220 g / L.
[0023] In some embodiments, in step S6, the second metatitanic acid is used to produce a second titanium dioxide or to prepare a titanium-based catalyst, wherein the second titanium dioxide is pigment-grade titanium dioxide.
[0024] In some embodiments, the method further includes step S7: collecting waste acid, performing graded concentration to obtain concentrated waste acid and sulfuric acid residue, and reusing the concentrated waste acid for acid hydrolysis of the slow-cooling residue; the collected waste acid includes at least the waste acid generated by hydrolysis and washing of the concentrated titanium liquid.
[0025] In some embodiments, step S7 further includes: calcining the sulfuric acid residue, the acidolysis residue, and the aluminum-containing acid residue generated from the aluminum removal of the high-alumina titanium liquid to decompose the sulfates therein; converting and absorbing the sulfur-containing flue gas generated from calcination to obtain recycled sulfuric acid, and using the recycled sulfuric acid to supplement the sulfuric acid used for the acidolysis of the slow-cooling residue.
[0026] In some embodiments, step S7 further includes: using the calcination residue generated from calcination as an aluminum-rich material as a raw material for aluminum smelting.
[0027] The technical solution provided in this application has at least the following beneficial effects: The titanium-rich slag fractionation extraction method provided in this application distinguishes the cooling methods of the titanium-rich slag. For rapidly cooled slag with high glass content, dilute acid leaching is used to remove impurities and directly obtain titanium-rich material. For slowly cooled slag with large titanium grains, concentrated sulfuric acid acidolysis is used to obtain titanium liquid. This improves the problems of high acid consumption and many impurities caused by a single processing route.
[0028] Meanwhile, this application precisely separates the titanium liquid obtained from acid hydrolysis according to the vanadium-titanium ratio and the chromium-titanium ratio. High vanadium-chromium titanium liquid can be directly hydrolyzed to prepare high-purity artificial rutile, or used to prepare pigment-grade titanium dioxide and other products after removing vanadium and chromium, thereby reducing the negative impact of coloring impurities on the color of the products.
[0029] Furthermore, this application separates low-vanadium-chromium titanium liquor based on the aluminum-to-titanium ratio and performs aluminum removal on high-aluminum titanium liquor, thereby reducing the concentration of non-titanium ions, lowering the viscosity of the titanium liquor, and reducing the risk of gelation during the concentration stage. Through tiered separation and tailored treatment techniques, this application achieves precise classification and differentiated treatment of titanium-rich slag with different characteristics, improving the efficiency of full resource recovery from titanium-rich slag. Attached Figure Description
[0030] Figure 1 This is a schematic flowchart of an optional titanium-rich slag fractionation extraction method provided in the embodiments of this application. Detailed Implementation
[0031] The following combination Figure 1 The method for graded extraction of titanium-rich slag provided in this application is described. Figure 1 The process flow for the graded extraction of titanium-rich slag along different processing paths is illustrated. The embodiments described herein serve to illustrate the processing steps, material flow directions, and their interrelationships. Where there are no process conflicts, the technical features of the various embodiments can be combined with each other.
[0032] In this article, titanium-rich slag refers to metallurgical slag, hydrometallurgical slag, or titanium-containing tailings that contain titanium minerals and can be used as raw materials for titanium extraction. Quenching refers to a cooling process that rapidly lowers the temperature of molten slag to form quenched slag, such as water quenching. Slow cooling refers to a process that cools molten slag at a rate lower than the average cooling rate of the quenching process to form slow-cooled slag, such as heat preservation and slow cooling.
[0033] In this article, titanium solution refers to a titanium-containing solution obtained after slow-cooling slag undergoes acid hydrolysis with concentrated sulfuric acid, aging, leaching, and filtration. Dilute titanium solution is a titanium-containing solution obtained directly after acid hydrolysis of titanium solution. Concentrated titanium solution is a titanium-containing solution obtained after necessary aluminum removal treatment and concentration of low-vanadium-chromium titanium solution with high aluminum content (i.e., high-aluminum titanium solution), or directly after concentration of low-aluminum titanium solution. The concentration of titanium solution is expressed as the mass of titanium dioxide per unit volume of solution.
[0034] In this paper, the vanadium-titanium ratio represents the ratio of vanadium pentoxide content to titanium dioxide content in the titanium solution under the same analytical standards. The chromium-titanium ratio represents the ratio of chromium trioxide content to titanium dioxide content in the titanium solution under the same analytical standards. The aluminum-titanium ratio represents the ratio of aluminum trioxide content to titanium dioxide content in the titanium solution under the same analytical standards. When classifying the same batch of titanium solution, the same sampling method and analytical standards are used for each substance to ensure the comparability of the ratios.
[0035] The first metatitanic acid is obtained by directly hydrolyzing high-vanadium-chromium titanium solution and is mainly used in specialized functional products. The second metatitanic acid is obtained by removing aluminum, concentrating, hydrolyzing, and washing low-vanadium-chromium titanium solution and is mainly used in pigment-grade titanium dioxide or titanium-based catalysts. The above names are used to distinguish between the two processing routes and their corresponding products, and do not indicate a fixed order of preparation.
[0036] In this article, waste acid includes sulfuric acid-containing liquids generated during hydrolysis, washing, dilute acid leaching for impurity removal, and other acidic material separation processes. Sulfuric acid residue is a sulfate solid obtained through solid-liquid separation after precipitation or freeze crystallization of high-alumina titanium liquor. "Multiple" refers to two or more.
[0037] Titanium-rich slag can originate from various reduction, smelting, smelting, hydrometallurgical, or mineral processing processes. Different sources of titanium-rich slag not only differ in titanium dioxide content, but also in the content of components such as aluminum, vanadium, chromium, calcium, magnesium, iron, and silicon, as well as the state of the titanium phase. Different cooling processes affect the ratio of glassy to crystalline phases in the slag. Therefore, when using the same acid system to treat different titanium-rich slags, it is easy to encounter situations where acid consumption, leaching selectivity, and subsequent purification load cannot be simultaneously optimized.
[0038] Related processing routes typically focus on a single raw material or a single acidolysis process. The quench slag has a high proportion of glassy phase, and some impurities such as calcium, magnesium, and iron exhibit high reactivity with dilute acids. In contrast, the titanium phase in the slow-cooling slag undergoes crystallization and growth, resulting in lower reactivity, making it difficult to fully integrate titanium into the liquid phase when treated with dilute acids. If both types of slag are acidolyzed with concentrated sulfuric acid, many impurities in the quench slag may enter the liquid phase simultaneously with the titanium, increasing the load on subsequent separation. If both are leached with dilute acid, the crystalline titanium phase in the slow-cooling slag may not be fully utilized.
[0039] Vanadium, chromium, and aluminum in molten titanium exhibit different subsequent behaviors. Vanadium and chromium affect the hue of calcined metatitanic acid products, while high aluminum content can affect the concentration, hydrolysis, and filtration of the molten titanium. If the molten titanium is not split after obtaining it and the same concentration and hydrolysis conditions are used directly, the differences in impurities between different batches of molten titanium will be passed on to metatitanic acid and its subsequent products, making it difficult to coordinate product applications and processing costs.
[0040] This application uses cooling method, vanadium-chromium content, and aluminum content as sequentially linked grading criteria. Cooling method determines whether solid titanium-rich slag should be treated with dilute acid for impurity removal or concentrated sulfuric acid for acidolysis. Vanadium-titanium ratio and chromium-titanium ratio determine whether the acid-treated titanium solution should enter a dedicated functional grade product route or, after vanadium and chromium removal, enter a low-vanadium-chromium route. Aluminum-titanium ratio determines whether the low-vanadium-chromium titanium solution undergoes aluminum removal before concentration. These grading criteria correspond to differences in solid mineral phases, differences in color-causing impurities, and differences in interference from concentration and hydrolysis, respectively.
[0041] The difficulty of the above processing logic lies not in completing a single dilute acid leaching, sulfuric acid acidolysis, or titanium liquor hydrolysis, but in enabling the materials from different branches to be reconnected at subsequent stages. High-vanadium-chromium titanium liquor, after vanadium and chromium removal, can be transferred to the low-vanadium-chromium titanium liquor treatment branch; high-aluminum titanium liquor, after aluminum removal, can undergo corresponding concentration and hydrolysis processes with low-aluminum titanium liquor; hydrolysis waste acid and solid sulfates can also be returned to the acidolysis or acid production branch. Thus, titanium-rich slag with different cooling states and different impurity compositions can be processed within the same grading framework.
[0042] Through the aforementioned grading method, dilute acid primarily performs selective impurity removal in the rapidly cooled slag, while concentrated sulfuric acid primarily performs acidolysis and transformation of various substances, including the titanium phase, in the slowly cooled slag. The separation of vanadium, chromium, and aluminum is no longer applied indiscriminately to all titanium liquid, but rather based on their respective concentrations. This coordination reduces the repeated processing of low-impurity materials and directs high-impurity materials into products or purification pathways that match their composition, thereby improving the comprehensive utilization of titanium and associated elements in the titanium-rich slag.
[0043] See Figure 1 In one basic embodiment, the method for graded extraction of titanium-rich slag includes steps S1 to S6. Step S1 involves subjecting the titanium-rich slag to rapid cooling and slow cooling respectively, obtaining rapidly cooled slag and slowly cooled slag. The rapidly cooled slag and slowly cooled slag are then separately powdered to obtain rapidly cooled slag powder and slowly cooled slag powder. Rapid cooling and slow cooling can be performed on different batches of molten titanium-rich slag, or they can be performed separately on molten titanium-rich slag from the same source after diversion.
[0044] The pulverization in step S1 is used to reduce the particle size of the slag and increase the contact area between the subsequent acid solution and the solid particles. Pulverizing the quench slag and the slow-cooling slag separately reduces the impact of the two types of slag mixing on leaching selectivity and acidolysis conditions. After pulverization, samples can be taken separately to analyze the content of titanium, vanadium, chromium, aluminum, and other impurities in the quench slag powder and the slow-cooling slag powder, and the analysis results will be used to determine the subsequent material ratios and processing batches.
[0045] Step S2 involves leaching the quenched slag powder with dilute acid to remove impurities. The dilute acid is hydrochloric acid or sulfuric acid with a mass fraction of 5% to 30%. During leaching, the quenched slag powder is brought into contact with the dilute acid and reacts, allowing some acid-soluble impurities in the quenched slag powder to enter the liquid phase. The resulting solid-liquid mixture is then filtered, washed, and dried sequentially. The solid obtained from filtration is washed to remove adhering acid and soluble salts, and then dried to obtain titanium-rich material.
[0046] Both hydrochloric acid and sulfuric acid can provide acidic media for dissolving acid-soluble impurities in quenched slag. The liquid phase obtained from the hydrochloric acid route mainly contains the corresponding metal chlorides, while the liquid phase obtained from the sulfuric acid route mainly contains the corresponding metal sulfates. The type of acid can be selected based on the subsequent utilization of the waste acid. When using sulfuric acid, the dilute acid leachate can be connected to the subsequent sulfuric acid system; when using hydrochloric acid, the solubility characteristics of some metal impurities in chloride systems can be utilized for impurity removal.
[0047] The mass fraction of the acidic medium in the dilute acid is 5% to 30%, for example, 5%, 20%, or 30%. Within this range, the acid dosage and contact time can be adjusted according to the content of acid-soluble impurities in the quenched slag powder. When the acid mass fraction is close to the lower limit, impurity removal can be promoted by increasing the contact time or the degree of liquid-solid contact; when the acid mass fraction is close to the upper limit, the treatment time can be controlled according to the acid dissolution loss of the titanium-rich phase. This range enables the dilute acid to leach impurities while reducing the probability of the titanium-rich phase entering the liquid phase.
[0048] In step S2, filtration separates the impurity-containing liquid phase from the titanium-rich solid phase. Washing can be performed using deionized water and can continue until the washing solution meets the acid residue requirements set by the process. In a specific example, washing continues until the washing solution is neutral. Drying is used to reduce the free water in the titanium-rich solid phase, making the titanium-rich material suitable for storage, transportation, or subsequent sulfuric acid titanium dioxide, molten salt chlorination, or boiling chlorination processes.
[0049] Step S3 involves acidolysis and aging of the slowly cooled slag powder using concentrated sulfuric acid with a mass fraction of 80% to 98%. Acidolysis causes the titanium minerals in the slowly cooled slag powder to react with sulfuric acid, transforming them into sulfuric acid-containing titanium oxide that can enter the liquid phase during subsequent leaching. Aging allows the acidolysis reaction to continue within the acid-treated material and facilitates the formation of titanium-containing aged material that can be dissolved by the leaching solution.
[0050] The concentrated sulfuric acid has a mass fraction of 80% to 98%, for example, 80%, 85%, 90%, 92%, or 98%. Within this range, concentrated sulfuric acid has the ability to destroy the crystalline mineral phase of the slowly cooled slag and induce titanium sulfation. In actual operation, the acid concentration can be selected within this range based on the degree of crystallinity, titanium dioxide content, and impurity content of the slowly cooled slag, and the mixing state of the acidolysis and ripening processes can be controlled.
[0051] The acid-hydrolyzed and matured materials are leached using a leachate. Upon contact with the matured material, the soluble titanium salts enter the liquid phase, while the insoluble substances remain in the solid phase. The leached material is then filtered to obtain acid-hydrolyzed residue and titanium liquor. The acid-hydrolyzed residue is sent to a subsequent sulfur resource recovery line, while the titanium liquor is sent to a vanadium-chromium content grading line.
[0052] Steps S2 and S3 are designed separately for titanium-rich slag under different cooling states. Rapidly cooled slag powder is leached with dilute acid to primarily remove acid-soluble impurities while retaining the titanium-rich solid phase. Slowly cooled slag powder is acidified with concentrated sulfuric acid to allow titanium to enter the liquid phase. Neither path requires the sequential use of dilute acid and concentrated sulfuric acid on the same batch of slag powder, thus reducing repeated acid treatments and ensuring the treatment method matches the mineral phase state in the slag.
[0053] Step S4 divides the titanium solution obtained in step S3 into high-vanadium-chromium titanium solution and low-vanadium-chromium titanium solution based on the vanadium-titanium ratio and chromium-titanium ratio. Before division, samples of the titanium solution can be taken to determine the contents of vanadium, chromium, and titanium, and the corresponding ratios can be calculated. When either the vanadium-titanium ratio or the chromium-titanium ratio reaches the high-vanadium-chromium condition, the titanium solution enters the high-vanadium-chromium treatment branch; when both ratios reach the low-vanadium-chromium condition, the titanium solution enters the low-vanadium-chromium treatment branch.
[0054] Step S5 provides two types of treatment methods for the high-vanadium-chromium titanium solution, which can be used alone or in combination. The first method involves directly hydrolyzing the high-vanadium-chromium titanium solution and performing solid-liquid separation to obtain first metatitanic acid. The second method removes some of the vanadium, some of the chromium, or both from the high-vanadium-chromium titanium solution, reducing the vanadium-titanium ratio and the chromium-titanium ratio, resulting in a low-vanadium-chromium titanium solution that can be transferred to subsequent treatments.
[0055] When the same batch of high-vanadium-chromium titanium liquor is treated using two different methods simultaneously, it can be diverted first. One portion of the high-vanadium-chromium titanium liquor is hydrolyzed to prepare primary metatitanic acid, while the other portion is converted into low-vanadium-chromium titanium liquor through vanadium and chromium removal. Alternatively, some vanadium or chromium can be removed first, and the material can then be directed to the low-vanadium-chromium branch line or undergo further separation based on the ratio of the removed vanadium or chromium. Therefore, the processing capacity of the high-vanadium-chromium titanium liquor can be allocated according to the demand for primary metatitanic acid and the processing capacity of the low-vanadium-chromium titanium liquor.
[0056] Step S6, based on the aluminum-to-titanium ratio, divides the low-vanadium-chromium titanium solution obtained directly in step S4 and the low-vanadium-chromium titanium solution obtained in step S5 after vanadium and chromium removal into high-aluminum titanium solution and low-aluminum titanium solution. The high-aluminum titanium solution undergoes aluminum removal before entering the concentration process. The low-aluminum titanium solution has an aluminum content within the range that does not require a separate aluminum removal process and can directly enter the concentration process.
[0057] The high-alumina titanium solution, after aluminum removal, and the low-alumina titanium solution are concentrated separately to obtain concentrated titanium solutions. These two types of concentrated titanium solutions can be hydrolyzed separately, or they can be combined into the corresponding concentrated titanium solution treatment process if the subsequent hydrolysis conditions are met. Hydrolysis of the concentrated titanium solution transforms titanium from the liquid phase to the metatitanic acid solid phase. Solid-liquid separation and washing then remove the mother liquor and soluble impurities to obtain the second metatitanic acid.
[0058] Steps S1 to S6 form a continuous hierarchical processing relationship. The first stage determines the acid treatment route for solid materials based on the cooling method and mineral phase state; the second stage determines the product application or impurity removal route for titanium liquid based on the vanadium-titanium ratio and chromium-titanium ratio; the third stage determines whether aluminum removal is necessary before concentration based on the aluminum-titanium ratio. Each stage of diversion uses material properties directly related to subsequent processing, reducing unnecessary unified processing throughout the entire process.
[0059] In some embodiments, the titanium-rich slag processed in step S1 is one or more of the following: vanadium-titanium magnetite gas-based direct reduction slag, coal-based direct reduction slag, biomass direct reduction slag, molten reduction slag, plasma reduction slag, blast furnace slag, hydrometallurgical slag, and titanium-containing tailings after mineral processing. Titanium-rich slag from different sources can be processed separately, or they can be batched and processed after the composition and mineral phase conditions are compatible.
[0060] Gas-based direct reduction slag is titanium-rich slag produced after gas reduction and smelting of titanium-containing raw materials. Coal-based direct reduction slag and biomass direct reduction slag are titanium-rich slags produced after direct reduction using coal-based reducing media and biomass reducing media, respectively, followed by smelting. After reduction and slag-iron separation, the iron in the above-mentioned slags is reduced, and titanium, along with some aluminum, vanadium, chromium, magnesium, calcium, and silicon, are enriched in the slag phase.
[0061] Molten reduction slag and plasma reduction slag can be rapidly or slowly cooled depending on their slag discharge state. Blast furnace slag can be titanium-containing slag that is directly cooled in a molten state, or it can be blast furnace slag that has been crushed, sorted, or otherwise pretreated to have titanium extraction value. Hydrometallurgical slag and titanium-containing tailings after mineral processing can also be included in the corresponding processing branches according to their mineral phase structure and impurity composition when they have the corresponding titanium-containing components.
[0062] When using titanium-rich slag from multiple sources, the content of titanium, aluminum, vanadium, and chromium in each raw material can be determined separately, and the slag can be powdered according to its cooling state. If multiple titanium-rich slags already have the same quenching or slow cooling state, they can be mixed under compatible subsequent acid treatment conditions. If there are significant differences in cooling state or acid reaction characteristics, they should be fed into separate quenching or slow cooling slag branches to maintain the selectivity of the staged treatment.
[0063] In some implementations, the mass percentage of slag powder passing through a 325-mesh sieve in both quenched and slow-cooled slag powder is not less than 95%. In other words, when a certain mass of slag powder is sieved through a 325-mesh sieve, the mass percentage of slag powder passing through the sieve openings accounts for more than 95% of the total sample mass. This particle size requirement can be applied to both quenched and slow-cooled slag powder.
[0064] Both dilute acid leaching and concentrated sulfuric acid acidolysis are solid-liquid contact reactions. When the mass percentage of slag powder passing through a 325-mesh sieve reaches over 95%, the slag powder has a large acid-liquid contact area. For rapidly cooled slag powder, dilute acid can contact acid-soluble impurities dispersed in the glassy phase; for slowly cooled slag powder, concentrated sulfuric acid can more fully coat the particles and act on the crystalline titanium phase, reducing the impact of unreacted areas inside the particles on titanium leaching.
[0065] A minimum of 95% of the slag powder passes through a 325-mesh sieve, which improves the particle size consistency between different batches, resulting in better repeatability of acid dosage and solid-liquid mixing. Powdering can be performed using grinding equipment capable of processing titanium-rich slag to the aforementioned particle size. After grinding, the sieving is carried out; the oversize material can be returned to the powdering process, while the undersize material is used as quenched slag powder and slow-cooled slag powder, respectively.
[0066] In some embodiments, rapid cooling is achieved through water quenching or hot water pouring. The molten titanium-rich slag rapidly cools upon contact with water, forming a rapidly cooled, water-quenched slag. This rapid cooling prevents some components in the slag from fully crystallizing, which is beneficial for forming a rapidly cooled structure containing a glassy phase. After pulverization, this structure allows dilute acid to preferentially leach some of the calcium, magnesium, iron, and other acid-soluble impurities.
[0067] In some embodiments, the slow cooling method employs a holding-down slow cooling with an average cooling rate not exceeding 5°C / min. During slow cooling, the average cooling rate of the molten slag is kept within the aforementioned range by holding the slag at room temperature or controlling heat dissipation. The lower average cooling rate provides time for the nucleation and crystal growth of the titanium phase in the slag, allowing the slowly cooled slag to form a different crystalline structure than the quenched slag, and making it suitable for subsequent concentrated sulfuric acid acidolysis.
[0068] Rapid cooling, slow cooling, powder particle size, and raw material source can be used individually or in combination. For example, a portion of the gas-based direct reduction slag is water-quenched and produced as rapidly cooled slag powder with a mass percentage passing through a 325-mesh sieve of not less than 95%. The other portion is slowly cooled by holding at an average cooling rate not exceeding 5°C / min and produced as slowly cooled slag powder with the same particle size requirements. This combination can be used for the compatible production of the same raw material in two processing branches.
[0069] In some embodiments, the titanium dioxide mass fraction in the titanium-rich material obtained in step S2 is not less than 70%. During the leaching of the quenched slag powder with dilute acid, some non-titanium impurities enter the liquid phase, while titanium is mainly retained in the solid phase. After filtration, washing, and drying, the relative mass fraction of titanium dioxide in the solid phase increases, forming a titanium-rich material that can be used as a downstream titanium extraction feedstock.
[0070] Titanium-rich materials with a titanium dioxide mass fraction of not less than 70% can be used as raw materials for the sulfuric acid process in titanium dioxide production. In this application, the titanium-rich material further reacts with sulfuric acid to form a titanium-containing solution. Titanium-rich materials can also be used as raw materials for molten salt chlorination or boiling chlorination, where the titanium component is chlorinated to form titanium-containing chlorides. The specific application of titanium-rich materials can be determined based on the content of residual impurities such as calcium, magnesium, iron, and silicon.
[0071] In one example of quenched slag treatment, the main components of the titanium-rich slag are: titanium dioxide 46.59%, ferrous oxide 3.43%, calcium oxide 4.24%, silicon dioxide 19.6%, magnesium oxide 8.94%, aluminum oxide 15.47%, vanadium pentoxide 0.35%, and chromium trioxide 0.12%. The titanium-rich slag is quenched in water to form quenched slag, and then powdered.
[0072] The above-mentioned quenched residue powder was leached in 20% hydrochloric acid for 120 minutes. After the reaction was complete, the mixture was filtered, and the filtrate carried away some of the dissolved impurities. The resulting solid was washed with deionized water until neutral and then dried to obtain a titanium-rich material with a titanium dioxide content of over 70%. This example illustrates that hydrochloric acid in the range of 5% to 30% can be used for leaching and removing impurities from quenched residue.
[0073] As an alternative implementation, sulfuric acid at a mass fraction of 5%, 20%, or 30% can be used instead of hydrochloric acid to treat the quenched slag powder. The acidic filtrate obtained from sulfuric acid leaching can be used as dilute acid water in the leaching branch of the slow-cooled slag curing material, or in the waste acid classification and concentration branch. Using hydrochloric acid or sulfuric acid does not change the step sequence of leaching, filtration, washing, and drying of the quenched slag powder to form titanium-rich material.
[0074] In some embodiments, the leaching solution used in step S3 is one or more of water, dilute acid water, and dilute titanium solution. When using multiple leaching solutions, they can be pre-mixed and then added to the curing material, or they can be added sequentially. The amount of leaching solution added is based on the requirement that soluble titanium salts in the curing material enter the liquid phase and form a filterable slurry.
[0075] When water is used as the leaching solution, it dissolves soluble titanium salts in the calcined material, forming a titanium solution. When dilute acid water is used, maintaining a certain acidity in the leaching system helps reduce the probability of premature hydrolysis of titanium-containing species during the leaching process, forming insoluble metatitanic acid. The dilute acid water can be prepared dilute sulfuric acid or other acidic liquids within the system.
[0076] For example, the dilute acid solution contains 5% to 30% by mass of acidic medium, including waste acid obtained after leaching and filtering quenched slag powder with dilute acid to remove impurities. This waste acid still contains residual acid and carries metal salts dissolved from the quenched slag powder. Using it for leaching slowly cooled slag maturation material can utilize the remaining acidity and reduce the amount of material required to treat this portion of waste acid separately. Before use, the decision to use it directly or in combination with water can be made based on the acidity and impurity load.
[0077] For example, the titanium concentration in the dilute titanium solution, calculated as TiO2, is 80-150 g / L, which can be the high vanadium-chromium titanium solution obtained in step S4. When this dilute titanium solution is used as the leaching solution, the leaching system initially contains titanium and sulfuric acid components, which can reduce the formation of large concentration gradients in localized areas by newly dissolved titanium-containing species. The titanium solution obtained after leaching is further analyzed for vanadium-titanium ratio and chromium-titanium ratio, and then split according to step S4.
[0078] There is no mandatory combination relationship between water, dilute acid solution, and dilute titanium solution. Water can be used alone; dilute acid solution can be used alone; and dilute titanium solution can also be used alone. Two or all three can also be used in combination. For example, the leaching material can be moistened with dilute acid solution first, and then water can be added to complete the leaching; or dilute titanium solution can be used in combination with water to make the resulting titanium solution reach the concentration and fluidity required for subsequent fractionation.
[0079] In some embodiments, the criterion for determining a high vanadium-chromium titanium liquid is: a vanadium-titanium ratio greater than or equal to 1×10⁻⁶. -2 Or, the chromium-to-titanium ratio is greater than or equal to 0.5 × 10⁻� -2 As long as either the vanadium-titanium ratio or the chromium-titanium ratio reaches the corresponding threshold, the titanium solution can be classified into the high-vanadium-chromium titanium solution treatment branch.
[0080] The criteria for determining low vanadium-chromium titanium liquid is: vanadium-to-titanium ratio less than 1×10⁻⁶. -2 Furthermore, the chromium-to-titanium ratio is less than 0.5 × 10⁻⁶. -2 Under low vanadium-chromium conditions, both vanadium and chromium are considered. When the vanadium-titanium ratio reaches the low requirement but the chromium-titanium ratio still reaches the high vanadium-chromium condition, the titanium solution is still treated as a high vanadium-chromium titanium solution; when the chromium-titanium ratio reaches the low requirement but the vanadium-titanium ratio still reaches the high vanadium-chromium condition, it is also treated as a high vanadium-chromium titanium solution.
[0081] The aforementioned thresholds are used to establish a correlation between the color risks of subsequent products caused by vanadium and chromium and the corresponding treatment paths. Titanium solutions with low vanadium-titanium ratios and low chromium-titanium ratios can enter the pigment-grade metatitanic acid branch. Titanium solutions with at least one high ratio will first enter the special functional grade product branch, or the corresponding ratio will be reduced through vanadium and chromium removal before entering the low vanadium-chromium branch, thereby reducing the possibility of high vanadium-chromium materials directly entering the pigment-grade product route.
[0082] In one specific example, the vanadium-to-titanium ratio of the titanium solution obtained from the slow-cooling slag leaching is 2.8 × 10⁻⁶. -2 The chromium-to-titanium ratio is 8×10-3 The vanadium-titanium ratio is higher than 1×10. -2 The chromium-to-titanium ratio is also higher than 0.5×10. -2 Therefore, this titanium solution is classified as a high-vanadium-chromium titanium solution. The titanium concentration in the solution, calculated as titanium dioxide, is 125 g / L, and it can be introduced into the first metatitanic acid preparation branch or the vanadium and chromium removal branch.
[0083] The separation of high-vanadium-chromium titanium solutions and low-vanadium-chromium titanium solutions is carried out using the same analytical standard, which can reduce false separations caused by changes in the detection aperture. After separation, the vanadium-titanium ratio and chromium-titanium ratio can be re-measured at subsequent key points. For example, after extraction treatment, the two ratios of the high-vanadium-chromium titanium solution are re-measured. If the low-vanadium-chromium condition is met, proceed to step S6; if not, the corresponding vanadium-chromium separation can continue.
[0084] In some embodiments, the titanium concentration of the high vanadium chromium titanium solution, calculated as titanium dioxide, is 80 g / L to 150 g / L, for example, it can be 80 g / L, 125 g / L or 150 g / L.
[0085] When the concentration of high-vanadium-chromium titanium solution is between 80 g / L and 150 g / L, the hydrolysis system has a lower titanium concentration compared to pigment-grade concentrated titanium solution, thus classifying it as a dilute titanium solution. The metatitanic acid particles generated by hydrolysis can have particle size and filtration performance suitable for specialized functional applications. Vanadium and chromium do not need to be completely removed before hydrolysis, thus reducing the need for deep purification steps when directly preparing specialized functional-grade metatitanic acid from high-vanadium-chromium titanium solution.
[0086] Metatitanic acid can be used as an additive in the preparation of ceramics. In ceramic formulations, metatitanic acid provides the titanium component, which participates in the formation of the ceramic phase after subsequent heat treatment. Metatitanic acid can also be used as an additive in the preparation of enamel, participating as a titanium-containing raw material in the glaze formulation. When used as an additive in the preparation of welding electrodes, metatitanic acid can serve as a titanium-containing component in the electrode coating formulation, participating in slag formation and the welding process.
[0087] Metatitanic acid (RTA) can be used in combination with high-vanadium-chromium titanium hydroxide solution in ceramics, enamel, or welding electrodes, or separately. Specifically, the concentration of the high-vanadium-chromium titanium hydroxide solution can be controlled between 80 g / L and 150 g / L, while RTA is used for other specialized functional applications. RTA can also be used in one or more of the ceramics, enamel, or welding electrodes industries. These applications do not change the source of the RTA obtained from the hydrolysis of high-vanadium-chromium titanium hydroxide solution.
[0088] In some embodiments, the first metatitanic acid is further calcined to obtain first titanium dioxide or synthetic rutile. Calcination removes free water, bound water, and residual acidic components from the first metatitanic acid and causes a corresponding phase transformation of titanium dioxide. When the calcined product is used as first titanium dioxide, it can be used in specialized functional-grade applications with color and functional properties adapted to its specifications.
[0089] The synthetic rutile obtained from the calcination of metatitanic acid can be used as synthetic rutile for boiling chlorination. This synthetic rutile contains a high proportion of titanium dioxide, which comes into contact with the chlorination medium during boiling chlorination and is converted into titanium-containing chlorides. Converting metatitanic acid into synthetic rutile allows titanium from high-vanadium-chromium titanium liquor to enter the chlorination process feedstock route, expanding the product applications of high-vanadium-chromium titanium liquor.
[0090] Vanadium and chromium in high-vanadium-chromium titanium solutions can be separated before hydrolysis or from waste acid after hydrolysis. Before hydrolysis, the titanium solution undergoes vanadium and chromium removal to become a low-vanadium-chromium titanium solution. After hydrolysis, the high-vanadium-chromium titanium solution first forms primary metatitanic acid, while at least a portion of the vanadium and chromium are retained or enriched in the hydrolysis waste acid. The vanadium-rich and chromium-rich products are then separated and recovered from the waste acid.
[0091] Vanadium-rich products may include vanadium pentoxide or vanadium electrolyte. Chromium-rich products may include chromium trioxide. The product form can be selected based on the valence state and concentration of vanadium and chromium in the recovery solution. After obtaining the vanadium-rich solution, further precipitation, separation, or conversion can be carried out to form vanadium pentoxide or to be used in the preparation of vanadium electrolyte; after obtaining the chromium-rich concentrate, it can be precipitated and converted to form chromium trioxide.
[0092] In some embodiments, the high-vanadium-chromium titanium solution is first oxidized to convert vanadium or chromium to a valence state suitable for subsequent separation, and then at least one of vanadium and chromium is removed. The oxidized titanium solution is then extracted using a chelating extractant that can maintain extraction performance in acidic titanium solutions. The chelating extractant transfers the target vanadium or chromium component from the aqueous phase of the titanium solution to the extraction phase.
[0093] Extraction can be performed separately for vanadium and chromium, or it can be done sequentially through fractional extraction. During extraction, the organic phase is contacted with the high-vanadium-chromium titanium solution, and phase separation occurs after mass transfer. Based on the extraction behavior of vanadium and chromium under different conditions, the oxidation state, phase ratio, and contact stage can be adjusted to achieve removal rates of over 95% for both vanadium and chromium.
[0094] The vanadium-to-titanium ratio and chromium-to-titanium ratio of the extracted titanium solution were re-measured in aqueous phase. When both ratios met the low vanadium-chromium condition, the titanium solution was designated as a low vanadium-chromium titanium solution and proceeded to step S6. Therefore, the output of the extraction was not an isolated purified liquid, but rather directly connected to the aluminum content classification node of the low vanadium-chromium titanium solution, allowing the purified titanium to continue entering the second metatitanic acid treatment branch.
[0095] The vanadium- or chromium-loaded extractant phase is back-extracted using an alkaline solution. Upon contact with the loaded extractant phase, the alkaline solution transfers the vanadium or chromium to the back-extraction solution. The back-extraction solution then undergoes precipitation and solid-liquid separation to obtain vanadium-rich and chromium-rich products, respectively. The extraction, back-extraction, and precipitation separation work together to retain titanium in the main process titanium solution and to form enriched products of vanadium and chromium that can be used separately.
[0096] In one specific example, after oxidation, the high-vanadium-chromium titanium solution was used to extract vanadium and chromium separately with an acid-resistant extractant, achieving removal rates of over 95% for both vanadium and chromium. The supported organic phase was back-extracted with alkaline solution, followed by precipitation and separation to obtain industrial-grade vanadium pentoxide and chromium trioxide products. The raffinate titanium solution reached low-vanadium-chromium conditions and was further fractionated using the aluminum-titanium ratio.
[0097] In other embodiments, the high-vanadium-chromium titanium solution is directly hydrolyzed, and the first metatitanic acid is separated to obtain vanadium- and chromium-containing waste acid. This waste acid can be completely separated from the first metatitanic acid before vanadium and chromium are extracted using an acid-resistant extractant. The acidic liquid after extraction can enter the waste acid fractionation and concentration branch line, and the loaded extraction phase is then subjected to the aforementioned alkaline back-extraction and precipitation method to obtain vanadium-rich and chromium-rich products.
[0098] There is no fixed combination relationship between the calcination of the first metatitanic acid, the recovery of vanadium and chromium from waste acid, and the oxidative extraction of high-vanadium-chromium titanium liquor. Only the first metatitanic acid can be calcined; only vanadium and chromium can be recovered from hydrolyzed waste acid; only the high-vanadium-chromium titanium liquor can be oxidized and extracted; or a combination based on material balance can be used. Each pathway revolves around the differentiated utilization of titanium, vanadium, and chromium in the high-vanadium-chromium titanium liquor.
[0099] In some embodiments, step S6 classifies low-vanadium-chromium titanium solutions with an aluminum-to-titanium ratio greater than or equal to 0.25 as high-aluminum titanium solutions, and low-vanadium-chromium titanium solutions with an aluminum-to-titanium ratio less than 0.25 as low-aluminum titanium solutions. Before splitting, samples of the low-vanadium-chromium titanium solutions can be taken to determine the aluminum and titanium content, and the aluminum-to-titanium ratio can be calculated under the same analytical standard.
[0100] An aluminum-to-titanium ratio of 0.25 serves as the dividing line between whether and not to include a separate aluminum removal step. When the aluminum-to-titanium ratio is less than 0.25, the low-aluminum-to-titanium solution directly enters the concentration process, reducing the consumption of aluminum precipitation reagents and refrigeration energy. When the aluminum-to-titanium ratio is greater than or equal to 0.25, the high-aluminum-to-titanium solution undergoes aluminum removal first, reducing the probability of aluminum salts crystallizing and forming scale in the concentration equipment and forming colloidal interferences during hydrolysis.
[0101] In a specific example, the titanium solution after vanadium and chromium removal is a low-vanadium-chromium titanium solution with a measured aluminum-to-titanium ratio of 0.32. Since 0.32 is greater than 0.25, this titanium solution is classified as a high-aluminum titanium solution and undergoes aluminum removal before concentration. This determination establishes a continuous relationship between the vanadium-chromium purified titanium solution and the aluminum content classification.
[0102] One method for removing aluminum from high-alumina titanium solutions is to add sulfates to precipitate aluminum. The sulfate can be ammonium sulfate or potassium sulfate. When ammonium sulfate is added, ammonium ions, aluminum ions, and sulfate ions form aluminum-containing complex salt crystals with low solubility; when potassium sulfate is added, potassium ions react with aluminum ions and sulfate ions to form corresponding aluminum-containing complex salt crystals. After crystallization, solid-liquid separation is performed to obtain aluminum-containing acid slag and the aluminum-removed titanium solution.
[0103] When using ammonium sulfate for aluminum precipitation, it can be added to a high-alumina titanium solution and allowed to fully contact, allowing the aluminum-containing sulfate to crystallize and precipitate. When using potassium sulfate, the processing steps correspond to those for ammonium sulfate. Ammonium sulfate and potassium sulfate can be used separately or in combination, provided the aluminum precipitation requirements are met. The liquid phase after solid-liquid separation enters the concentration process, while the aluminum-containing slag enters the subsequent calcination branch.
[0104] In the specific example above with an aluminum-to-titanium ratio of 0.32, ammonium sulfate was added to the high-aluminum titanium solution to precipitate aluminum. After the aluminum-containing crystals precipitate, solid-liquid separation was performed, and the titanium solution after aluminum removal was concentrated to 190 g / L (based on titanium dioxide). 190 g / L falls within the range of 180 g / L to 220 g / L. The concentrated titanium solution was then hydrolyzed and washed to obtain pigment-grade metatitanic acid.
[0105] As an alternative implementation, aluminum is removed from the high-alumina titanium solution through freezing. The high-alumina titanium solution is cooled, causing the solubility of aluminum sulfate to decrease and reach a supersaturated state, resulting in aluminum sulfate crystallization. Solid-liquid separation is then performed, with the aluminum-containing crystals forming aluminum-containing acid slag. The liquid phase after aluminum removal enters the concentration process.
[0106] Both sulfate precipitation and freeze-precipitation aim to transfer aluminum from the titanium melt to the solid phase. When using sulfate, the crystallization behavior of aluminum-containing complex salts is utilized; when using freeze-precipitation, the property that the solubility of aluminum sulfate decreases with decreasing temperature is utilized. Both methods are integrated with subsequent calcination of aluminum-containing acid slag and utilization of aluminum-rich materials.
[0107] In some embodiments, the high-alumina titanium solution after aluminum removal and the low-alumina titanium solution that directly enters the concentration process are respectively concentrated to 180 g / L to 220 g / L based on titanium dioxide, for example, 180 g / L, 190 g / L, 200 g / L, or 220 g / L. During the concentration process, some water is removed so that the titanium solution reaches the titanium concentration required for subsequent hydrolysis.
[0108] When the titanium concentration is below the range required for pigment-grade hydrolysis, the conditions for crystal nucleation and crystal growth may change. Excessive titanium concentration may increase local supersaturation and viscosity, raising the probability of heterogeneous hydrolysis and particle agglomeration. Maintaining the concentrated titanium solution between 180 g / L and 220 g / L ensures that hydrolysis nucleation and subsequent crystal growth occur within the suitable concentration range for preparing second metatitanic acid.
[0109] After hydrolysis, concentrated titanium solution undergoes solid-liquid separation and washing. Hydrolysis converts titanium from a titanium-containing liquid phase into a hydrated titanium dioxide solid phase. Washing utilizes the solubility difference between solid metatitanic acid and soluble sulfates to reduce free acid and metal sulfates adhering to the second metatitanic acid. The waste acid generated during washing enters the waste acid collection branch of step S7.
[0110] Second metatitanic acid can be used to produce second titanium dioxide, which is a pigment-grade titanium dioxide. After subsequent calcination and treatment to be compatible with the target product, second metatitanic acid can form pigment-grade titanium dioxide. Since the titanium liquid entering this branch has already undergone vanadium and chromium content classification and necessary aluminum removal, the influence of vanadium, chromium, and aluminum on color, hydrolysis, and filtration is correspondingly reduced.
[0111] Metatitanic acid can also be used to prepare titanium-based catalysts. When used as a raw material for titanium-based catalysts, it provides a hydrated titanium dioxide matrix, and its subsequent processing can be carried out according to the intended use of the catalyst. The applications for pigment-grade titanium dioxide and titanium-based catalysts can be selected separately; it is not required that the same batch of metatitanic acid be used in both product routes simultaneously.
[0112] In some embodiments, the method further includes step S7. Step S7 collects waste acid and performs fractional concentration to obtain concentrated waste acid and sulfuric acid residue. The collected waste acid includes at least the waste acid generated from the hydrolysis of concentrated titanium solution and washing with second metatitanic acid, and may also include waste acid generated from the hydrolysis of first metatitanic acid, sulfuric acid system waste acid generated from the dilute acid leaching of quench slag, and sulfuric acid-containing liquids generated in other steps.
[0113] Staged concentration can include two or more concentration stages. Waste acid undergoes partial water removal in the first concentration stage before entering the next stage for further concentration. As the sulfuric acid concentration increases, some metal sulfates in the waste acid reach supersaturation and precipitate. The precipitated sulfates are separated into solid and liquid phases to form sulfuric acid slag, while the liquid phase forms concentrated waste acid.
[0114] Staged concentration can be implemented through evaporation. Evaporation reduces the water content in waste acid, increases the concentration of free sulfuric acid, and promotes the crystallization of at least one of ferrous sulfate, magnesium sulfate, aluminum sulfate, or other metal sulfates. Concentration and crystallization can be carried out at different stages of the same equipment, or in interconnected concentration and crystallization equipment.
[0115] Concentrated waste acid is reused in the acidolysis of slow-cooling sludge. Before reuse, the sulfuric acid concentration and impurity content of the concentrated waste acid can be analyzed and mixed with fresh sulfuric acid to ensure that the concentrated sulfuric acid used for acidolysis reaches the corresponding process concentration. By returning the concentrated waste acid to step S3, the sulfuric acid in the hydrolyzed waste acid participates again in the acidolysis of the slow-cooling sludge, reducing the amount of waste acid neutralization treatment and the amount of fresh sulfuric acid replenishment.
[0116] In one specific example, the waste acid from the hydrolysis of concentrated titanium solution is treated using a staged concentration method. During the concentration process, sulfate crystals precipitate and separate from the liquid phase, and the concentrate is returned to the acidolysis process. This treatment creates an acid cycle between the hydrolysis branch and the slow-cooling slag acidolysis branch, while simultaneously removing the metal sulfates accumulated in the waste acid from the liquid phase as sulfuric acid slag.
[0117] When quenched slag is leached with sulfuric acid, the dilute acid water obtained from filtration can be used for leaching the slowly cooled slag curing material. The acidic liquid formed after leaching enters subsequent treatment with the titanium liquid and eventually forms waste acid at hydrolysis or other separation points. Thus, the dilute acid water is reused for leaching and the concentrated waste acid is reused for acid hydrolysis, forming a recycling path with different acid concentration levels.
[0118] In some embodiments, step S7 further involves calcining the sulfuric acid residue, the acidolysis residue produced in step S3, and the aluminous acid residue produced from the aluminum removal process of the high-alumina titanium solution, either collectively or separately. These solids contain sulfates. Calcination causes the sulfates to decompose thermally, forming sulfur-containing flue gas and calcination residue.
[0119] Sulfuric acid residue mainly comes from the staged concentration of waste acid. Acidolysis residue mainly comes from the insoluble solids after leaching of slowly cooled slag maturation material, which may contain unreacted minerals, siliceous components, and sulfates. Aluminate-containing acid residue mainly comes from ammonium sulfate precipitation, potassium sulfate precipitation, or cryogenic aluminum precipitation, and contains a high proportion of aluminum-containing sulfates.
[0120] Sulfuric acid residue, acidolysis residue, and aluminous acid residue can be dehydrated separately before being fed into the calcination equipment according to the calcination capacity. The three types of solids can be calcined together or separately. When calcining together, the proportions can be adjusted based on the sulfate and alumina content of each solid to ensure that the sulfur-containing flue gas is suitable for subsequent conversion and absorption, and to provide the calcination residue with conditions for aluminum-rich material utilization.
[0121] During calcination, metal sulfates decompose upon heating, releasing sulfur components into the flue gas, while the metal components remain primarily in the solid residue. After necessary dust removal and purification, the sulfur-containing flue gas enters a conversion process, transforming the sulfur-containing components into a form suitable for sulfuric acid production. The converted flue gas then enters an absorption process to obtain recycled sulfuric acid.
[0122] Recycled sulfuric acid is used to replenish the sulfuric acid used in the acidolysis of the slow-cooling residue. The recycled sulfuric acid can be used alone in the acidolysis and acid preparation stage, or it can be combined with concentrated waste acid obtained from waste acid concentration and fresh sulfuric acid. Through two pathways—direct reuse of concentrated waste acid and acid production via solid sulfate calcination—both the acid resources in the liquid phase and the sulfur resources in the solid phase can be returned to step S3.
[0123] The calcination treatment of sulfuric acid residue, acidolysis residue, and aluminous acid residue is coordinated with the graded treatment of titanium liquor. Aluminum in the titanium liquor is removed and enters the aluminous acid residue; metal sulfates in the waste acid are concentrated and enter the sulfuric acid residue; and insoluble matter from the slow-cooling residue enters the acidolysis residue. These three types of solids are no longer treated as separate end-of-life wastes, but instead enter the sulfate decomposition and acid production lines, thereby reducing the amount of sulfur-containing solids discharged.
[0124] In some embodiments, the calcination residue produced can be used as an aluminum-rich feedstock for aluminum smelting. During calcination, aluminum sulfates decompose to form alumina, and sulfur components enter the sulfur-containing flue gas. As the aluminum in the aluminate slag is concentrated in the calcination residue, and the sulfur components are removed from the solid, the mass fraction of alumina in the calcination residue is correspondingly increased.
[0125] In one specific example, the acidolysis residue remaining after leaching, the sulfate obtained from aluminum removal, and the sulfate obtained from waste acid concentration are all subjected to calcination decomposition. The calcination flue gas is converted and absorbed to recover sulfuric acid. The mass fraction of alumina (Al₂O₃) in the calcination residue reaches over 60%, and it is used as an aluminum-rich feedstock for aluminum smelting. This pathway sequentially transfers aluminum initially present in the titanium-rich slag to high-alumina titanium liquid, aluminous acid slag, and calcination residue, which are then used as feedstock for aluminum smelting. The aluminum material flow is independent of, yet connected to, the recovery pathways for titanium, vanadium, chromium, and sulfur at process nodes.
[0126] See Figure 1 In a complete application example, the main components of the titanium-rich slag are: titanium dioxide 46.59%, ferrous oxide 3.43%, calcium oxide 4.24%, silicon dioxide 19.6%, magnesium oxide 8.94%, aluminum oxide 15.47%, vanadium pentoxide 0.35%, and chromium trioxide 0.12%. A portion of the molten titanium-rich slag is water-quenched to form a rapid-cooling slag, while the other portion is heat-insulated and slowly cooled to form a slow-cooling slag.
[0127] After quenching and pulverizing the slag, it is leached with 20% hydrochloric acid for 120 minutes. The reaction slurry is then filtered to obtain a solid phase, which is washed with deionized water until neutral and dried to obtain a titanium-rich material with a titanium dioxide content of over 70%. This titanium-rich material can be used as a raw material for sulfuric acid titanium dioxide production, molten salt chlorination, or fluidized bed chlorination, depending on the composition of the remaining impurities.
[0128] The slow-cooling branch line adopts a heat preservation and slow-cooling method, with an average cooling rate not exceeding 5℃ / min. After the slow-cooling slag is powdered, it is contacted with concentrated sulfuric acid with a mass fraction of 92% for acidolysis and aging. After acidolysis and aging, a dilute acid solution containing 40g / L titanium dioxide, formed from the leaching of blast furnace water-quenched slag, is used as the leaching solution for leaching. The solution is then filtered to obtain acidolysis slag and titanium liquid.
[0129] The vanadium-to-titanium ratio of the leached titanium solution is 2.8 × 10⁻⁶. -2 The chromium-to-titanium ratio is 8×10 -3 The titanium concentration, calculated as titanium dioxide, is 125 g / L. Since both the vanadium-titanium ratio and the chromium-titanium ratio meet the criteria for high-vanadium-chromium titanium solution, the titanium solution enters the high-vanadium-chromium treatment branch and is processed in two parts.
[0130] A portion of high-vanadium-chromium titanium liquid is hydrolyzed and subjected to solid-liquid separation to obtain primary metatitanic acid. Primary metatitanic acid has particulate properties suitable for specialized functional applications and can be used in ceramics, enamels, or welding electrodes. It can also be calcined to obtain primary titanium dioxide or synthetic rutile for boiling chlorination.
[0131] Another portion of the high-vanadium-chromium titanium solution is first oxidized, and then vanadium and chromium are extracted separately using an acid-resistant extractant. The removal rates of both vanadium and chromium reach over 95%. The loaded extract phase is back-extracted with alkaline solution, and the back-extract is precipitated and separated to obtain industrial-grade vanadium pentoxide and chromium trioxide, respectively. The raffinate aqueous phase is tested and found to meet low-vanadium-chromium conditions, and is then used as the low-vanadium-chromium titanium solution in the aluminum-titanium ratio fractionation step.
[0132] The low-vanadium-chromium titanium solution has an aluminum-to-titanium ratio of 0.32, and is therefore classified as a high-aluminum titanium solution. Ammonium sulfate is added to the high-aluminum titanium solution to precipitate aluminum, causing aluminum-containing sulfates to crystallize out. Solid-liquid separation yields an aluminum-removed titanium solution and aluminum-containing acid slag. The aluminum-removed titanium solution is concentrated, and the titanium concentration (calculated as titanium dioxide) is controlled to 190 g / L.
[0133] A concentrated titanium solution with a concentration of 190 g / L is hydrolyzed, transforming titanium from the liquid phase into a solid phase of metatitanic acid. The hydrolyzed slurry undergoes solid-liquid separation and washing to obtain secondary metatitanic acid. This secondary metatitanic acid can be used to produce pigment-grade titanium dioxide or as a raw material for preparing titanium-based catalysts. The waste acid generated from hydrolysis and washing is fed into a waste acid fractionation and concentration branch line.
[0134] Waste acid is treated using a staged concentration method. As moisture is removed, metal sulfates crystallize out, and after solid-liquid separation, sulfuric acid residue and concentrated waste acid are obtained. The concentrated waste acid is returned to the acidolysis process of the slow-cooling slag and used in combination with other sulfuric acid sources depending on the acid concentration. Thus, the sulfuric acid produced in the hydrolysis branch is reused for the acidolysis conversion of the titanium phase in the slow-cooling slag.
[0135] The acidolysis residue, the aluminous acid residue obtained from ammonium sulfate precipitation, and the sulfuric acid residue obtained from waste acid concentration enter the calcination process. Calcination decomposes the sulfates in the residue, producing sulfur-containing flue gas and calcination residue. The sulfur-containing flue gas is converted and absorbed to form recycled sulfuric acid, which is used to supplement the sulfuric acid required for the acidolysis of the slow-cooling residue.
[0136] The alumina content in the calcination residue reaches over 60%. This calcination residue is used as an aluminum-rich material as a raw material for aluminum smelting. Thus, the quenched slag forms a titanium-rich material, the titanium in the slow-cooled slag forms primary and secondary metatitanic acids, vanadium and chromium form corresponding enriched products, aluminum forms an aluminum-rich material, and sulfuric acid is returned to the acidolysis process through liquid-phase recycling and flue gas acid production.
[0137] If the titanium solution to be treated reaches the low vanadium-chromium condition in step S4, it can directly proceed to step S6 for aluminum-titanium ratio classification without going through the high vanadium-chromium hydrolysis or extraction branch. If the aluminum-titanium ratio of the low vanadium-chromium titanium solution is less than 0.25, a separate aluminum removal operation can be omitted, and it can be directly concentrated to 180 g / L to 220 g / L before hydrolysis and washing. This process reduces the additional treatment steps for low-impurity titanium solutions.
[0138] If the high-vanadium-chromium titanium solution to be processed is mainly used for specialized functional products, a larger portion of the high-vanadium-chromium titanium solution can be directly hydrolyzed. If the demand for pigment-grade secondary metatitanic acid is high, a larger portion of the high-vanadium-chromium titanium solution can be oxidized and extracted to convert it into a low-vanadium-chromium titanium solution. Both material distribution methods use the same vanadium-titanium ratio and chromium-titanium ratio grading nodes.
[0139] If the high-alumina titanium liquor is not suitable for adding ammonium sulfate or potassium sulfate, aluminum sulfate can be precipitated by freeze crystallization. Both the aluminous acid slag obtained from freeze crystallization and the aluminous acid slag obtained from sulfate precipitation can be fed into the calcination branch. The titanium liquor after aluminum removal is output only to meet the conditions for subsequent concentration and hydrolysis; the main process for the second metatitanic acid remains unchanged regardless of the aluminum removal method.
[0140] If the quench slag is leached with dilute sulfuric acid, the waste acid obtained from filtration can be used as dilute acid water for leaching the slow-cooling slag curing material. If the quench slag is leached with dilute hydrochloric acid, the hydrochloric acid system filtrate can be collected and treated separately, while the slow-cooling slag branch line uses water, other dilute acid water, or dilute titanium solution for leaching. The choice of acid type does not change the overall relationship between the two solid processing branches set up according to the cooling method.
[0141] As can be seen from the above implementation methods, the cooling method splitting, vanadium-chromium content splitting, and aluminum content splitting are not isolated processing actions. The cooling method determines whether titanium is extracted in the form of a titanium-rich solid phase or titanium liquid; the vanadium-chromium content determines whether the titanium liquid enters the first metatitanic acid branch or enters the low vanadium-chromium branch after purification; and the aluminum content determines whether the low vanadium-chromium titanium liquid is dealuminized before concentration. The three-layer splitting collectively reduces the degree to which the differences in raw materials are transferred to the final product.
[0142] The treatment of waste acid and acid slag further closes the material cycle. Concentrated waste acid is directly returned to the slow-cooling slag for acidolysis, while sulfuric acid slag, acidolysis slag, and aluminous acid slag are calcined to recover sulfur resources, and the calcination residue is used as an aluminum-rich material. This coordination allows titanium, vanadium, chromium, aluminum, and sulfur to enter their respective products or recycling pathways, improving the comprehensive utilization of different types of titanium-rich slag.
[0143] The above embodiments are only used to illustrate the technical solutions of this application and are not intended to limit the scope of protection of this application. Those skilled in the art can adjust the conventional implementation forms of material conveying, solid-liquid separation, concentration, calcination, flue gas conversion, and absorption without changing the technical relationship between the cooling method diversion, vanadium-chromium content diversion, and aluminum content diversion. Equivalent substitutions or reasonable combinations of various technical features can be implemented according to the technical logic disclosed in this application.
Claims
1. A method for graded extraction of titanium-rich slag, characterized in that, Includes the following steps: S1. The titanium-rich slag is subjected to rapid cooling and slow cooling respectively to obtain rapidly cooled slag and slow cooled slag; the rapidly cooled slag and slow cooled slag are respectively ground into powder to obtain rapidly cooled slag powder and slow cooled slag powder. S2. The quenched slag powder from step S1 is leached with dilute acid to remove impurities, and then filtered, washed and dried in sequence to obtain titanium-rich material; the dilute acid contains an acidic medium with a mass fraction of 5% to 30%. S3. The slow-cooling slag powder from step S1 is acidified and matured with concentrated sulfuric acid, and then leached and filtered with a leaching solution to obtain acidified slag and titanium liquid. S4. Based on the vanadium-titanium ratio and the chromium-titanium ratio, the titanium liquid in step S3 is divided into high vanadium-chromium titanium liquid and low vanadium-chromium titanium liquid. S5. The high vanadium-chromium titanium solution obtained in step S4 is directly hydrolyzed to separate the first metatitanic acid; and / or, some vanadium and / or chromium in the high vanadium-chromium titanium solution obtained in step S4 are removed to obtain a low vanadium-chromium titanium solution. S6. According to the aluminum-titanium ratio, the low-vanadium-chromium titanium solution in step S4 and / or S5 is divided into high-aluminum titanium solution and low-aluminum titanium solution; the high-aluminum titanium solution is concentrated after aluminum removal, and the low-aluminum titanium solution is directly concentrated to obtain concentrated titanium solutions respectively; the concentrated titanium solutions are hydrolyzed and washed to obtain second metatitanic acid.
2. The method for graded extraction of titanium-rich slag according to claim 1, characterized in that, Step S1 shall be performed in accordance with at least one of the following requirements: The titanium-rich slag is one or more of the following: vanadium-titanium magnetite gas-based direct reduction smelting slag, coal-based direct reduction smelting slag, biomass direct reduction smelting slag, molten reduction slag, plasma reduction smelting slag, blast furnace slag, hydrometallurgical slag, and titanium-containing tailings after mineral processing. The mass percentage of slag powder passing through a 325-mesh sieve in the rapidly cooled slag powder and the slowly cooled slag powder shall not be less than 95%; Rapid cooling methods include water quenching or hot water pouring for cooling; Slow cooling methods include heat preservation and slow cooling with an average cooling rate not exceeding 5℃ / min.
3. The method for graded extraction of titanium-rich slag according to claim 1, characterized in that, In step S2, the mass fraction of TiO2 in the obtained titanium-rich material is not less than 70%, and the titanium-rich material is used as a raw material for sulfuric acid titanium dioxide, molten salt chlorination or boiling chlorination. And / or, in step S3, the leaching solution is one or more of water, dilute acid water, and dilute titanium solution; the dilute acid water contains 5% to 30% acidic medium by mass, and the titanium concentration in the dilute titanium solution, calculated as TiO2, is 80 to 150 g / L.
4. The method for graded extraction of titanium-rich slag according to claim 1, characterized in that, In step S4, the high vanadium-chromium-titanium liquid is a titanium liquid with a vanadium-titanium ratio greater than or equal to 1×10 -2 , or a chromium-titanium ratio greater than or equal to 0.5×10 -2 ; and the low vanadium-chromium-titanium liquid is a titanium liquid with a vanadium-titanium ratio less than 1×10 -2 and a chromium-titanium ratio less than 0.5×10 -2 .
5. The method for graded extraction of titanium-rich slag according to claim 1, characterized in that, In step S4, the titanium concentration in the high vanadium chromium titanium liquid, calculated as TiO2, is 80~150 g / L; And / or, in step S5, the first metatitanic acid is used as an additive in the preparation of ceramics, enamels, or welding electrodes.
6. The method for graded extraction of titanium-rich slag according to claim 1, characterized in that, Step S5 further includes: calcining the first metatitanic acid to obtain the first titanium dioxide or artificial rutile. And / or, step S5 further includes: obtaining vanadium-rich products and / or chromium-rich products, wherein the methods for obtaining vanadium-rich products and / or chromium-rich products include: separating and recovering vanadium-rich products and / or chromium-rich products from the waste acid after separating the first metatitanic acid from the hydrolysis of the high vanadium-chromium titanium solution; and / or, recovering part of the vanadium and / or chromium removed from the high vanadium-chromium titanium solution to obtain vanadium-rich products and / or chromium-rich products.
7. The method for graded extraction of titanium-rich slag according to claim 1, characterized in that, Step S6 shall be performed in accordance with at least one of the following requirements: The high-aluminum titanium liquid is a low-vanadium-chromium titanium liquid with an aluminum-to-titanium ratio greater than or equal to 0.25, and the low-aluminum titanium liquid is a low-vanadium-chromium titanium liquid with an aluminum-to-titanium ratio less than 0.
25. The aluminum removal methods of the high-alumina titanium liquid include: adding sulfate to the high-alumina titanium liquid to precipitate aluminum, or freezing the high-alumina titanium liquid to crystallize and separate aluminum sulfate from the titanium liquid to obtain aluminum-containing slag; The titanium concentration in the concentrated titanium solution, calculated as TiO2, is 180~220 g / L; The second metatitanic acid is used to produce a second titanium dioxide or to prepare a titanium-based catalyst, wherein the second titanium dioxide is a pigment-grade titanium dioxide.
8. The method for graded extraction of titanium-rich slag according to any one of claims 1 to 7, characterized in that, It also includes step S7: Waste acid is collected, graded and concentrated to obtain concentrated waste acid and sulfuric acid residue, and the concentrated waste acid is reused for the acidolysis of the slow-cooling residue; The collected waste acid includes at least the waste acid generated from the hydrolysis and washing of the concentrated titanium solution.
9. The method for graded extraction of titanium-rich slag according to claim 8, characterized in that, Step S7 also includes: The sulfuric acid residue, the acidolysis residue, and the aluminum-containing acid residue generated from the aluminum removal of the high-alumina titanium liquid are calcined to decompose the sulfates therein; the sulfur-containing flue gas generated from calcination is converted and absorbed to obtain recycled sulfuric acid, which is then used to supplement the sulfuric acid used for the acidolysis of the slow-cooling residue.
10. The method for graded extraction of titanium-rich slag according to claim 9, characterized in that, Step S7 also includes: using the calcination residue produced by calcination as an aluminum-rich material as a raw material for aluminum smelting.