A copper-nickel-silicon alloy with a uniform fine-grained structure and its preparation method

By performing processes such as melting, cooling electromagnetic stirring, stepwise solution treatment, cold rolling, and graded aging on copper-nickel-silicon alloys, the microstructure defects caused by the segregation of Ni, Si, and B elements were resolved, achieving high strength and high toughness of the alloy, reducing stress concentration and microcrack formation, and improving the overall performance of the copper-nickel-silicon alloy.

CN123108334APending Publication Date: 2026-11-17KUNMING UNIV OF SCI & TECH
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611187620.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-06
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

The segregation of Ni, Si, and B elements in copper-nickel-silicon alloys leads to microstructural defects, resulting in decreased alloy strength and toughness. During service, stress concentration and microcracks are prone to occur, which cannot be effectively solved by existing technologies.

Method used

Through a synergistic process of smelting, cooling, intermittent electromagnetic stirring, stepwise solution treatment, cold rolling, graded aging, and two low-temperature cooling processes, dendrites are broken up, promoting uniform element distribution and forming a uniform supersaturated solid solution. This process inhibits the segregation and ionization of the Ni-Si-B phase and reduces stress concentration.

Benefits of technology

It significantly improves the overall mechanical properties of copper-nickel-silicon alloys, enhances the alloy's strength and toughness, reduces the risk of microcracks, and extends its service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108334A_ABST
    Figure CN123108334A_ABST
Patent Text Reader

Abstract

This invention discloses a copper-nickel-silicon alloy with a uniform fine-grained structure and its preparation method, relating to the field of non-ferrous metal production technology. The preparation method involves adding boron to the copper-nickel-silicon alloy, followed by a process of melting and casting, cooling and intermittent electromagnetic stirring, step-by-step solution treatment, cold rolling, graded aging treatment, and two low-temperature cooling treatments to synergistically break down and refine the alloy grains. This promotes a uniform distribution of the alloy composition, inhibits the aggregation of the Ni-Si-B phase, and ensures its dispersed and discontinuous uniform distribution within the alloy. This reduces and adjusts internal stress concentration and lowers the probability of microcrack formation. The combined effect of grain refinement strengthening, deformation strengthening, and aging strengthening synergistically enhances the alloy's strength and toughness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a copper-nickel-silicon alloy with a uniform fine-grained structure and its preparation method, belonging to the field of non-ferrous metal production technology. Background Technology

[0002] Copper-nickel-silicon alloys possess excellent mechanical properties, corrosion resistance, and wear resistance, making them widely used in high-end equipment, precision instruments, and wear-resistant conductive components for new energy vehicles. However, the addition of trace amounts of boron (B) to copper-nickel-silicon alloys leads to the segregation of Ni, Si, and B elements, resulting in structural defects. This uneven alloy composition significantly reduces the alloy's strength and toughness. Specifically, the local enrichment of Ni, Si, and B prevents the formation of normal strengthening phases during subsequent aging processes in areas lacking these elements. The resulting coarse, incoherent Ni-Si-B phase is brittle and, due to its weak bonding with the matrix, easily becomes a crack initiation point, causing the alloy strength to be far below expectations, with a significant decrease in elongation and impact toughness. When alloy components are subjected to stress, the Ni-Si-B phase becomes free in the alloy matrix, transforming from a dispersed and uneven distribution to an aggregated state. As the force continues to increase, stress concentration occurs, becoming the initiation point for microcracks. This results in insufficient alloy strength and toughness, leading to fracture, and significantly impacting the service life and cost of the alloy components. Chinese invention patent application CN106498322A discloses a static magnetic field cryogenic treatment method for improving the strength and toughness of copper or copper alloys. After surface treatment of the copper or copper alloy product, it is placed in a static magnetic field for programmed cryogenic treatment, followed by controlled cooling rate and holding time, and then room temperature recovery and natural aging. This method effectively refines grains and reduces harmful phases without altering the material's composition and dimensions, thus improving the material's strength and toughness. However, the effectiveness of this method is significantly affected by the product thickness, and it fails to address the problem of micro-stress concentration and microcracks that easily lead to component failure during service.

[0003] For copper-nickel-silicon alloys, grain size and microstructure uniformity play a crucial role in their strength and toughness. This invention employs a series of processes to refine the grains multiple times, increasing the alloy's strength and toughness. It maximizes the dissolution of the Ni-Si-B phase to obtain a uniform supersaturated solid solution while maintaining its morphology, promoting the homogeneous distribution of the Ni-Si-B phase and limiting its migration. This effectively reduces stress concentration and the probability of microcrack formation, further increasing the alloy's strength and toughness. Furthermore, it more smoothly adjusts the internal stress of the alloy, reducing the risk of microcrack formation and further enhancing the alloy's toughness. Summary of the Invention

[0004] To address the shortcomings of related technologies, this invention provides a copper-nickel-silicon alloy with a uniform fine-grained structure and its preparation method. This alloy achieves high strength and high toughness while effectively suppressing Ni-Si-B phase segregation and microcrack initiation, significantly improving the alloy's comprehensive mechanical properties and service life. It solves the problems of microstructural defects and performance degradation caused by Ni, Si, and B element segregation in boron-added copper-nickel-silicon alloys, as well as the inability of related technologies to effectively address stress concentration and microcracks during service.

[0005] One objective of this invention is to provide a method for preparing a copper-nickel-silicon alloy with a uniform fine-grained structure, specifically comprising the following steps: (1) Melting and casting: Weigh copper, nickel, silicon and boron raw materials according to proportion and mix them to obtain mixed raw materials. Melt the mixed raw materials in an inert atmosphere under vacuum to obtain alloy melt. Pour the alloy melt into the mold to obtain alloy melt poured into the mold.

[0006] (2) Cooling and intermittent electromagnetic stirring treatment: The alloy melt poured into the mold is cooled and intermittent electromagnetic stirring treatment is performed during the cooling process to obtain the ingot after cooling and intermittent electromagnetic stirring treatment.

[0007] (3) Step-by-step solution treatment: The ingots after cooling and intermittent electromagnetic stirring are subjected to step-by-step solution treatment and then dried to obtain the solution-treated ingots.

[0008] (4) Cold rolling: The solution-treated ingot is cold rolled to obtain the cold-rolled ingot.

[0009] (5) Graded aging treatment: The cold-rolled ingot is subjected to graded aging treatment to obtain graded aging treated ingot.

[0010] (6) Two low-temperature cooling treatments: The ingots after graded aging treatment are subjected to two low-temperature cooling treatments to obtain a copper-nickel-silicon alloy with a uniform fine-grained structure.

[0011] Preferably, the mixed raw materials in step (1) include, by mass percentage: 1-4% nickel, 0.15-1.5% silicon, 0.02% boron, with the balance being copper and unavoidable impurities.

[0012] More preferably, the raw materials mixed in step (1) include, by mass percentage: 2-4% nickel, 0.5-1% silicon, 0.02% boron, with the balance being copper and unavoidable impurities.

[0013] Preferably, the temperature of vacuum melting in step (1) is 1450~1550℃ and the vacuum degree is 0.03MPa.

[0014] More preferably, the vacuum melting temperature in step (1) is 1530°C; the inert atmosphere is high-purity argon (Ar≥99.9%).

[0015] More preferably, the vacuum melting in step (1) is carried out in a vacuum induction melting furnace with a voltage of 150~300V, a current of 200~400A, and a frequency of 900Hz.

[0016] Preferably, the cooling rate of step (2) is 180~220℃ / min.

[0017] More preferably, the cooling rate of the cooling process in step (2) is 200°C / min.

[0018] Preferably, the conditions for the intermittent electromagnetic stirring treatment in step (2) are: the electromagnetic stirring current frequency is 800Hz and the magnetic induction intensity is 0.01~1T; the specific method of the intermittent electromagnetic stirring treatment is: the first stirring is carried out immediately after the alloy melt is poured into the mold, the stirring duration is 5s, and then the stirring is repeated for 5s every 10s, and the total stirring time is 130s.

[0019] More preferably, the magnetic induction intensity of the intermittent electromagnetic stirring treatment in step (2) is 0.5~1T.

[0020] More preferably, the temperature after the cooling treatment in step (2) is room temperature.

[0021] Preferably, the conditions for the step (3) solution treatment are as follows: a first-stage solution treatment is performed at 820~840℃ for 1.5h, followed by a second-stage solution treatment at 910~920℃ for 1.5h, and then quenching is performed after the second-stage solution treatment is completed.

[0022] More preferably, the heating rate of the step (3) solution treatment is 10℃ / min; the quenching treatment is carried out in room temperature water at 24℃.

[0023] Preferably, the cold rolling process in step (4) consists of 6 to 8 passes, with a deformation of 6 to 9% per pass and a total deformation of 36 to 72%.

[0024] More preferably, the total deformation of the cold rolling process in step (4) is 54-63%.

[0025] More preferably, the cold rolling in step (4) is carried out at room temperature.

[0026] Preferably, the conditions for the graded aging treatment in step (5) are: first-level aging treatment at 350~400℃ for 4~6h, second-level aging treatment at 460~490℃ for 4~6h, followed by cooling, and the total time for graded aging treatment is 8~12h.

[0027] More preferably, the cooling method in step (5) is air cooling.

[0028] Preferably, the conditions for the two cryogenic cooling treatments in step (6) are as follows: first, a first cryogenic cooling treatment of -90℃ for 4 hours, followed by warming, then a second cryogenic cooling treatment of -196℃ in a liquid nitrogen environment for 6 hours, followed by warming.

[0029] More preferably, the warming rate in step (6) is 5°C / min; and the warming process is to bring the temperature back to room temperature.

[0030] Another object of the present invention is to provide a copper-nickel-silicon alloy with a uniform fine-grained structure prepared by the method of the present invention.

[0031] Mechanism of the invention: This invention utilizes the synergistic effects of raw material selection, cooling and intermittent electromagnetic stirring, stepwise solution treatment, cold rolling, graded aging treatment, and two low-temperature cooling treatments to break up growing dendrites and promote uniform distribution of alloying elements, avoiding segregation and local enrichment, and suppressing dendrite segregation. Simultaneously, it effectively prevents the Ni-Si-B phase from concentrating in a point-like distribution at small grain boundaries, causing uneven stress distribution. Furthermore, it achieves complete re-dissolution of the Ni-Si-B phase, obtaining a uniformly composed supersaturated solid solution. This method further breaks down grains to produce fine-grained strengthening, significantly increasing alloy strength, while simultaneously allowing the broken grains to... Grain boundary synergy fixes and confines the free Ni-Si-B phase, creating an effect similar to dislocation pinning, thereby reducing the probability of microcracks in the alloy under stress, improving stress concentration, and enhancing strength and toughness. The generated high-density dislocations provide high-density nucleation sites, resulting in a finer grain structure and a finer, more uniform Ni-Si-B phase, thus improving both the strength and toughness of the alloy. The method of this invention can smoothly adjust internal stress and promote its homogenization, thereby reducing the risk of microcrack formation and further enhancing the strength and toughness of the alloy. The process flow diagram for the preparation of the copper-nickel-silicon alloy of this invention is shown below. Figure 1 As shown.

[0032] The beneficial effects of this invention are: This invention achieves grain refinement in copper-nickel-silicon alloys through the synergistic effects of raw material selection, cooling and intermittent electromagnetic stirring, step-by-step solution treatment, cold rolling, graded aging treatment, and two low-temperature cooling treatments. This promotes the formation of more uniform nucleation cores to increase the nucleation rate, effectively breaks up growing dendrites to refine the grains, and makes the alloy melt more uniform.

[0033] The preparation method of this invention can achieve a dispersed and uniform distribution of the Ni-Si-B phase in copper-nickel-silicon alloys. The Ni-Si-B phase is fixed and restricted by the strong constraint of the matrix lattice on the precipitated phase. At the same time, the uniform distribution of internal stress in the alloy is achieved, which effectively reduces the risk of microcracks caused by stress concentration and achieves a synergistic improvement and high matching of the alloy's strength and toughness.

[0034] The electromagnetic stirring, cold rolling, aging treatment, and low-temperature cooling process of this invention achieves the refinement and homogenization of the alloy microstructure. The combined effect of fine grain strengthening, deformation strengthening, and aging strengthening enables the alloy to obtain high strength and toughness, and has excellent engineering application prospects. Attached Figure Description

[0035] Figure 1 This is a process flow diagram for preparing a copper-nickel-silicon alloy with a uniform fine-grained structure according to the present invention.

[0036] Figure 2 This is a schematic diagram of the process for preparing a copper-nickel-silicon alloy with a uniform fine-grained structure according to the present invention. Detailed Implementation

[0037] To better illustrate the purpose, technical solution, and advantages of this invention, the invention will be further described below with reference to specific embodiments. In the embodiments and comparative examples of this invention, unless otherwise specified, all chemical reagents used were commercially available with analytical purity. The alloy raw materials used in the embodiments and comparative examples of this invention are high-purity copper (≥99.9%), high-purity nickel (≥99.9%), high-purity silicon (≥99.9%), and high-purity boron (≥99.9%). A schematic diagram of the preparation process of the copper-nickel-silicon alloy of this invention is shown below. Figure 2 As shown.

[0038] Example 1 A method for preparing a copper-nickel-silicon alloy with a uniform fine-grained structure specifically includes the following steps: (1) Melting and casting: Weigh copper, nickel, silicon and boron raw materials according to proportion and mix them to obtain mixed raw materials. The composition of the mixed raw materials by mass percentage includes: 2% Ni, 0.5% Si, 0.02% B, with the balance being Cu and unavoidable impurities. Place the mixed raw materials in a vacuum induction melting furnace, evacuate and fill with high-purity argon (Ar≥99.9%) to 0.03MPa. The melting furnace voltage is 200V, the current is 300A and the frequency is 900Hz. Melt at 1530℃ for 9min to obtain a uniform alloy melt. Cool the alloy melt to 1480℃ and then pour it into a 100mm×50mm×50mm mold.

[0039] (2) Cooling and intermittent electromagnetic stirring treatment: The alloy melt poured into the mold is cooled to promote solidification. The cooling rate is 200℃ / min. The temperature is reduced to room temperature. During the cooling process, intermittent electromagnetic stirring treatment is performed. The specific method of intermittent electromagnetic stirring treatment is as follows: the alloy melt is stirred for the first time immediately after being poured into the mold. The stirring duration is 5s. Then, the stirring is repeated for 5s every 10s. The total stirring time is 130s. The stirring current frequency is 800Hz and the magnetic induction intensity is 0.8T. The ingot after cooling and intermittent electromagnetic stirring treatment is obtained.

[0040] (3) Stepwise solution treatment: The temperature is raised to 830℃ at a rate of 10℃ / min. The ingot after cooling and intermittent electromagnetic stirring is subjected to stepwise solution treatment. After the first stage of solution treatment is completed, the temperature is raised to 915℃ at the same rate for the second stage of solution treatment. The first stage of solution treatment is: solution treatment at 830℃ for 1.5h; the second stage of solution treatment is: solution treatment at 915℃ for 1.5h. Then, the ingot is quenched in room temperature water at about 24℃. After the temperature of the ingot drops to room temperature, the surface moisture is dried with a blower to obtain the ingot after solution treatment.

[0041] (4) Cold rolling treatment: The solution-treated ingot is cold rolled at room temperature. The rolling passes are 7, the deformation amount per pass is 9%, and the total deformation amount is 63%. After rolling, the surface of the ingot is cleaned to remove surface dirt and impurities, and the cold-rolled ingot is obtained.

[0042] (5) Graded aging treatment: The cold-rolled ingot is first placed in a furnace at 375℃ for 5.5h for the first aging treatment, then at 480℃ for 5.5h for the second aging treatment, and finally air-cooled to room temperature to obtain the graded aging treatment ingot.

[0043] (6) Two-stage low-temperature cooling treatment: The ingot after the graded aging treatment is first placed in a low-temperature equipment at -90℃ for 4 hours, then slowly heated to room temperature at a rate of 5℃ / min, and then placed in a liquid nitrogen environment at -196℃ for 6 hours, and then slowly heated to room temperature at a rate of 5℃ / min to obtain a copper-nickel-silicon alloy with a uniform fine-grained structure.

[0044] The grain size of the copper-nickel-silicon alloy prepared in this embodiment was statistically analyzed using a metallographic microscope and image analysis software. Tensile tests were conducted on the copper-nickel-silicon alloy prepared in this embodiment at room temperature using a universal testing machine. The experimental results showed that the average grain size of the copper-nickel-silicon alloy prepared in this embodiment was 35±7μm, the tensile strength was 672MPa, the yield strength was 584MPa, and the elongation was 15%.

[0045] Example 2 A method for preparing a copper-nickel-silicon alloy with a uniform fine-grained structure specifically includes the following steps: (1) Melting and casting: Weigh copper, nickel, silicon and boron raw materials according to proportion and mix them to obtain mixed raw materials. The composition of the mixed raw materials by mass percentage includes: 3% Ni, 0.6% Si, 0.02% B, with the balance being Cu and unavoidable impurities. Place the mixed raw materials in a vacuum induction melting furnace, evacuate and fill with high-purity argon (Ar≥99.9%) to 0.03MPa. The melting furnace voltage is 200V, the current is 300A and the frequency is 900Hz. Melt at 1530℃ for 9min to obtain a uniform alloy melt. Cool the alloy melt to 1480℃ and then pour it into a 100mm×50mm×50mm mold.

[0046] (2) Cooling and intermittent electromagnetic stirring treatment: The alloy melt poured into the mold is cooled to promote solidification. The cooling rate is 200℃ / min. The temperature is reduced to room temperature. During the cooling process, intermittent electromagnetic stirring treatment is performed. The specific method of intermittent electromagnetic stirring treatment is as follows: the alloy melt is stirred for the first time immediately after being poured into the mold. The stirring duration is 5s. Then, the stirring is repeated for 5s every 10s. The total stirring time is 130s. The stirring current frequency is 800Hz and the magnetic induction intensity is 0.6T. The ingot after cooling and intermittent electromagnetic stirring treatment is obtained.

[0047] (3) Stepwise solution treatment: The temperature is raised to 820℃ at a rate of 10℃ / min. The ingot after cooling and intermittent electromagnetic stirring is subjected to stepwise solution treatment. After the first stage of solution treatment is completed, the temperature is raised to 910℃ at the same rate for the second stage of solution treatment. The first stage of solution treatment is: solution treatment at 820℃ for 1.5h; the second stage of solution treatment is: solution treatment at 910℃ for 1.5h. Then, the ingot is quenched in room temperature water at about 24℃. After the ingot temperature drops to room temperature, the surface moisture is dried with a blower to obtain the ingot after solution treatment.

[0048] (4) Cold rolling treatment: The solution-treated ingot is cold rolled at room temperature. The rolling passes are 8, the deformation amount per pass is 7%, and the total deformation amount is 56%. After rolling, the surface of the ingot is cleaned to remove surface dirt and impurities, and the cold-rolled ingot is obtained.

[0049] (5) Graded aging treatment: The cold-rolled ingot is first placed in a furnace at 365℃ for 5.5h for the first stage of aging treatment, then at 460℃ for 5.5h for the second stage of aging treatment, and finally air-cooled to room temperature to obtain the graded aging treatment ingot.

[0050] (6) Two-stage low-temperature cooling treatment: The ingot after the graded aging treatment is first placed in a low-temperature equipment at -90℃ for 4 hours, then slowly heated to room temperature at a rate of 5℃ / min, and then placed in a liquid nitrogen environment at -196℃ for 6 hours, and then slowly heated to room temperature at a rate of 5℃ / min to obtain a copper-nickel-silicon alloy with a uniform fine-grained structure.

[0051] The grain size of the copper-nickel-silicon alloy prepared in this embodiment was statistically analyzed using a metallographic microscope and image analysis software. Tensile tests were conducted on the copper-nickel-silicon alloy prepared in this embodiment at room temperature using a universal testing machine. The experimental results showed that the average grain size of the copper-nickel-silicon alloy prepared in this embodiment was 42±10μm, the tensile strength was 664MPa, the yield strength was 567MPa, and the elongation was 14%.

[0052] Example 3 A method for preparing a copper-nickel-silicon alloy with a uniform fine-grained structure specifically includes the following steps: (1) Melting and casting: Weigh copper, nickel, silicon and boron raw materials according to proportion and mix them to obtain mixed raw materials. The composition of the mixed raw materials by mass percentage includes: 3.5% Ni, 0.9% Si, 0.02% B, with the balance being Cu and unavoidable impurities. Place the mixed raw materials in a vacuum induction melting furnace, evacuate and fill with high-purity argon (Ar≥99.9%) to 0.03MPa. The melting furnace voltage is 200V, the current is 300A and the frequency is 900Hz. Melt at 1530℃ for 9min to obtain a uniform alloy melt. Cool the alloy melt to 1480℃ and then pour it into a 100mm×50mm×50mm mold.

[0053] (2) Cooling and intermittent electromagnetic stirring: The alloy melt poured into the mold is cooled to promote solidification. The cooling rate is 200℃ / min. The temperature is reduced to room temperature. During the cooling process, intermittent electromagnetic stirring is performed. The specific method of intermittent electromagnetic stirring is as follows: the alloy melt is stirred for the first time immediately after being poured into the mold. The stirring duration is 5s. Then, the stirring is repeated for 5s every 10s. The total stirring time is 130s. The stirring current frequency is 800Hz and the magnetic induction intensity is 0.7T. The ingot after cooling and intermittent electromagnetic stirring is obtained.

[0054] (3) Stepwise solution treatment: The temperature is raised to 840℃ at a rate of 10℃ / min. The ingot after cooling and intermittent electromagnetic stirring is subjected to stepwise solution treatment. After the first stage of solution treatment is completed, the temperature is raised to 920℃ at the same rate for the second stage of solution treatment. The first stage of solution treatment is: solution treatment at 840℃ for 1.5h; the second stage of solution treatment is: solution treatment at 920℃ for 1.5h. Then, the ingot is quenched in room temperature water at about 24℃. After the ingot temperature drops to room temperature, the surface moisture is dried with a blower to obtain the ingot after solution treatment.

[0055] (4) Cold rolling treatment: The solution-treated ingot is cold rolled at room temperature. There are 6 rolling passes, and the deformation amount per pass is 9%, with a total deformation amount of 54%. After rolling, the surface of the ingot is cleaned to remove surface dirt and impurities, and the cold-rolled ingot is obtained.

[0056] (5) Graded aging treatment: The cold-rolled ingot is first placed in a furnace at 380℃ for 5.5h for the first aging treatment, then at 490℃ for 5.5h for the second aging treatment, and finally air-cooled to room temperature to obtain the graded aging treatment ingot.

[0057] (6) Two-stage low-temperature cooling treatment: The ingot after the graded aging treatment is first placed in a low-temperature equipment at -90℃ for 4 hours, then slowly heated to room temperature at a rate of 5℃ / min, and then placed in a liquid nitrogen environment at -196℃ for 6 hours, and then slowly heated to room temperature at a rate of 5℃ / min to obtain a copper-nickel-silicon alloy with a uniform fine-grained structure.

[0058] The grain size of the copper-nickel-silicon alloy prepared in this embodiment was statistically analyzed using a metallographic microscope and image analysis software. Tensile tests were conducted on the copper-nickel-silicon alloy prepared in this embodiment at room temperature using a universal testing machine. The experimental results showed that the average grain size of the copper-nickel-silicon alloy prepared in this embodiment was 38±9μm, the tensile strength was 667MPa, the yield strength was 575MPa, and the elongation was 15%.

[0059] This invention achieves refined and homogenized alloy microstructure through the synergistic effects of raw material selection, cooling and intermittent electromagnetic stirring, stepwise solution treatment, cold rolling, graded aging treatment, and two low-temperature cooling treatments. This promotes the dispersed distribution and stable pinning of strengthening phases and effectively releases and homogenizes internal stress. This synergistic mechanism significantly improves alloy strength while reducing stress concentration and the risk of microcracks, resulting in a simultaneous increase in toughness and ultimately a copper-nickel-silicon alloy with a good balance of strength and toughness. The preparation method of this invention can effectively refine grains, suppress Ni-Si-B phase aggregation, and promote its discontinuous and uniform distribution along grain boundaries within the alloy. This reduces and improves internal defects and stress concentration, lowers the probability of microcrack formation, and enhances the overall strength and toughness of the alloy through the synergistic effects of grain refinement strengthening, deformation strengthening, and aging strengthening.

[0060] Comparative Example 1 A method for preparing a copper-nickel-silicon alloy is disclosed. This comparative example uses the same method as Example 1 to prepare the copper-nickel-silicon alloy, except that the alloy melt is not subjected to intermittent electromagnetic stirring during the cooling process. The method specifically includes the following steps: (1) Melting and casting: Weigh copper, nickel, silicon and boron raw materials according to proportion and mix them to obtain mixed raw materials. The composition of the mixed raw materials by mass percentage includes: 2% Ni, 0.5% Si, 0.02% B, with the balance being Cu and unavoidable impurities. Place the mixed raw materials in a vacuum induction melting furnace, evacuate and fill with high-purity argon (Ar≥99.9%) to 0.03MPa. The melting furnace voltage is 200V, the current is 300A and the frequency is 900Hz. Melt at 1530℃ for 9min to obtain a uniform alloy melt. Cool the alloy melt to 1480℃ and then pour it into a 100mm×50mm×50mm mold.

[0061] (2) Cooling treatment: The alloy melt poured into the mold is cooled to promote solidification. The cooling rate is 200℃ / min. The temperature is reduced to room temperature to obtain the cooled ingot.

[0062] (3) Stepwise solution treatment: The temperature is raised to 830℃ at a rate of 10℃ / min. The ingot after cooling is subjected to stepwise solution treatment. After the first stage of solution treatment is completed, the temperature is raised to 915℃ at the same rate for the second stage of solution treatment. The first stage of solution treatment is: solution treatment at 830℃ for 1.5h; the second stage of solution treatment is: solution treatment at 915℃ for 1.5h. Then, the ingot is quenched in room temperature water at about 24℃. After the temperature of the ingot drops to room temperature, the surface moisture is dried with a blower to obtain the ingot after solution treatment.

[0063] (4) Cold rolling treatment: The solution-treated ingot is cold rolled at room temperature. The rolling passes are 7, the deformation amount per pass is 9%, and the total deformation amount is 63%. After rolling, the surface of the ingot is cleaned to remove surface dirt and impurities, and the cold-rolled ingot is obtained.

[0064] (5) Graded aging treatment: The cold-rolled ingot is first placed in a furnace at 375℃ for 5.5h for the first aging treatment, then at 480℃ for 5.5h for the second aging treatment, and finally air-cooled to room temperature to obtain the graded aging treatment ingot.

[0065] (6) Two-stage low-temperature cooling treatment: The ingot after the graded aging treatment is first placed in a low-temperature equipment at -90℃ for 4 hours, then slowly heated to room temperature at a rate of 5℃ / min, and then placed in a liquid nitrogen environment at -196℃ for 6 hours, and then slowly heated to room temperature at a rate of 5℃ / min to obtain copper-nickel-silicon alloy.

[0066] The grain size of the copper-nickel-silicon alloy prepared in this comparative example was statistically analyzed using a metallographic microscope and image analysis software. Tensile tests were conducted on the copper-nickel-silicon alloy prepared in this comparative example at room temperature using a universal testing machine. The experimental results showed that the average grain size of the copper-nickel-silicon alloy prepared in this comparative example was 123±32μm, the tensile strength was 553MPa, the yield strength was 435MPa, and the elongation was 9%.

[0067] Comparative Example 2 A method for preparing a copper-nickel-silicon alloy is disclosed. This comparative example uses the same method as Example 1 to prepare the copper-nickel-silicon alloy, the only difference being that the magnetic induction intensity of the intermittent electromagnetic stirring treatment in this comparative example is 0.008T. The method specifically includes the following steps: (1) Melting and casting: Weigh copper, nickel, silicon and boron raw materials according to proportion and mix them to obtain mixed raw materials. The composition of the mixed raw materials by mass percentage includes: 2% Ni, 0.5% Si, 0.02% B, with the balance being Cu and unavoidable impurities. Place the mixed raw materials in a vacuum induction melting furnace, evacuate and fill with high-purity argon (Ar≥99.9%) to 0.03MPa. The melting furnace voltage is 200V, the current is 300A and the frequency is 900Hz. Melt at 1530℃ for 9min to obtain a uniform alloy melt. Cool the alloy melt to 1480℃ and then pour it into a 100mm×50mm×50mm mold.

[0068] (2) Cooling and intermittent electromagnetic stirring treatment: The alloy melt poured into the mold is cooled to promote solidification. The cooling rate is 200℃ / min. The temperature is reduced to room temperature. During the cooling process, intermittent electromagnetic stirring treatment is performed. The specific method of intermittent electromagnetic stirring treatment is as follows: the alloy melt is stirred for the first time immediately after being poured into the mold. The stirring duration is 5s. Then, the stirring is repeated for 5s every 10s. The total stirring time is 130s. The stirring current frequency is 800Hz and the magnetic induction intensity is 0.008T. The ingot after cooling and intermittent electromagnetic stirring treatment is obtained.

[0069] (3) Stepwise solution treatment: The temperature is raised to 830℃ at a rate of 10℃ / min. The ingot after cooling and intermittent electromagnetic stirring is subjected to stepwise solution treatment. After the first stage of solution treatment is completed, the temperature is raised to 915℃ at the same rate for the second stage of solution treatment. The first stage of solution treatment is: solution treatment at 830℃ for 1.5h; the second stage of solution treatment is: solution treatment at 915℃ for 1.5h. Then, the ingot is quenched in room temperature water at about 24℃. After the temperature of the ingot drops to room temperature, the surface moisture is dried with a blower to obtain the ingot after solution treatment.

[0070] (4) Cold rolling treatment: The solution-treated ingot is cold rolled at room temperature. The rolling passes are 7, the deformation amount per pass is 9%, and the total deformation amount is 63%. After rolling, the surface of the ingot is cleaned to remove surface dirt and impurities, and the cold-rolled ingot is obtained.

[0071] (5) Graded aging treatment: The cold-rolled ingot is first placed in a furnace at 375℃ for 5.5h for the first aging treatment, then at 480℃ for 5.5h for the second aging treatment, and finally air-cooled to room temperature to obtain the graded aging treatment ingot.

[0072] (6) Two-stage low-temperature cooling treatment: The ingot after the graded aging treatment is first placed in a low-temperature equipment at -90℃ for 4 hours, then slowly heated to room temperature at a rate of 5℃ / min, and then placed in a liquid nitrogen environment at -196℃ for 6 hours, and then slowly heated to room temperature at a rate of 5℃ / min to obtain copper-nickel-silicon alloy.

[0073] The grain size of the copper-nickel-silicon alloy prepared in this comparative example was statistically analyzed using a metallographic microscope and image analysis software. Tensile tests were conducted on the copper-nickel-silicon alloy prepared in this comparative example at room temperature using a universal testing machine. The experimental results showed that the average grain size of the copper-nickel-silicon alloy prepared in this comparative example was 96±23μm, the tensile strength was 592MPa, the yield strength was 478MPa, and the elongation was 10%.

[0074] Comparative Example 1 did not undergo intermittent electromagnetic stirring during the solidification process after the molten metal was poured. Comparative Example 2's molten metal was only subjected to intermittent electromagnetic stirring at a lower magnetic induction intensity. Both Comparative Examples 1 and 2 had larger average grain sizes and lower tensile strength and elongation. This is because the increased average grain size of the alloy reduces its grain boundary area, resulting in poor homogenization of B element within the alloy. The Ni-Si-B phase is concentrated in a dotted pattern on small grain boundaries, which easily causes uneven stress distribution in the alloy material during testing, thereby affecting the strength and toughness of the alloy material.

[0075] Comparative Example 3 A method for preparing a copper-nickel-silicon alloy is disclosed. This comparative example uses the same method as Example 2 to prepare the copper-nickel-silicon alloy, the only difference being that the solution treatment time for each stage in this comparative example is 30 minutes. The specific steps include: (1) Melting and casting: Weigh copper, nickel, silicon and boron raw materials according to proportion and mix them to obtain mixed raw materials. The composition of the mixed raw materials by mass percentage includes: 3% Ni, 0.6% Si, 0.02% B, with the balance being Cu and unavoidable impurities. Place the mixed raw materials in a vacuum induction melting furnace, evacuate and fill with high-purity argon (Ar≥99.9%) to 0.03MPa. The melting furnace voltage is 200V, the current is 300A and the frequency is 900Hz. Melt at 1530℃ for 9min to obtain a uniform alloy melt. Cool the alloy melt to 1480℃ and then pour it into a 100mm×50mm×50mm mold.

[0076] (2) Cooling and intermittent electromagnetic stirring treatment: The alloy melt poured into the mold is cooled to promote solidification. The cooling rate is 200℃ / min. The temperature is reduced to room temperature. During the cooling process, intermittent electromagnetic stirring treatment is performed. The specific method of intermittent electromagnetic stirring treatment is as follows: the alloy melt is stirred for the first time immediately after being poured into the mold. The stirring duration is 5s. Then, the stirring is repeated for 5s every 10s. The total stirring time is 130s. The stirring current frequency is 800Hz and the magnetic induction intensity is 0.6T. The ingot after cooling and intermittent electromagnetic stirring treatment is obtained.

[0077] (3) Stepwise solution treatment: The temperature is raised to 820℃ at a rate of 10℃ / min. The ingot after cooling and intermittent electromagnetic stirring is subjected to stepwise solution treatment. After the first stage of solution treatment is completed, the temperature is raised to 910℃ at the same rate for the second stage of solution treatment. The first stage of solution treatment is performed at 820℃ for 30 minutes. The second stage of solution treatment is performed at 910℃ for 30 minutes. Then, the ingot is quenched in room temperature water at about 24℃. After the temperature of the ingot drops to room temperature, the surface moisture is dried with a blower to obtain the ingot after solution treatment.

[0078] (4) Cold rolling treatment: The solution-treated ingot is cold rolled at room temperature. The rolling passes are 8, the deformation amount per pass is 7%, and the total deformation amount is 56%. After rolling, the surface of the ingot is cleaned to remove surface dirt and impurities, and the cold-rolled ingot is obtained.

[0079] (5) Graded aging treatment: The cold-rolled ingot is first placed in a furnace at 365℃ for 5.5h for the first stage of aging treatment, then at 460℃ for 5.5h for the second stage of aging treatment, and finally air-cooled to room temperature to obtain the graded aging treatment ingot.

[0080] (6) Two-stage low-temperature cooling treatment: The ingot after the graded aging treatment is first placed in a low-temperature equipment at -90℃ for 4 hours, then slowly heated to room temperature at a rate of 5℃ / min, and then placed in a liquid nitrogen environment at -196℃ for 6 hours, and then slowly heated to room temperature at a rate of 5℃ / min to obtain copper-nickel-silicon alloy.

[0081] The grain size of the copper-nickel-silicon alloy prepared in this comparative example was statistically analyzed using a metallographic microscope and image analysis software. Tensile tests were conducted on the copper-nickel-silicon alloy prepared in this comparative example at room temperature using a universal testing machine. The experimental results showed that the average grain size of the copper-nickel-silicon alloy prepared in this comparative example was 47±13μm, the tensile strength was 560MPa, the yield strength was 453MPa, and the elongation was 9%.

[0082] Comparative Example 3 showed that the stepwise solution treatment time was relatively short. Although the average grain size of the alloy did not change significantly, the tensile strength and elongation were low. This indicates that the intermittent electromagnetic stirring intensity has a good effect on increasing the nucleation core and refining the grains by breaking dendrites. However, the short solution time resulted in insufficient atomic diffusion, leading to incomplete dissolution of the Ni-Si-B precipitates. Many of these precipitates remained at the grain boundaries, failing to obtain a uniform supersaturated solid solution. This affected the subsequent aging treatment steps, making it difficult for solute atoms to precipitate in a very fine form and thus improve the strength and toughness of the alloy. Consequently, the tensile strength and yield strength of the alloy decreased significantly.

[0083] Comparative Example 4 A method for preparing a copper-nickel-silicon alloy is disclosed. This comparative example uses the same method as Example 3 to prepare the copper-nickel-silicon alloy, except that the ingot after graded aging treatment in this comparative example only undergoes one low-temperature cooling treatment. The specific steps include: (1) Melting and casting: Weigh copper, nickel, silicon and boron raw materials according to proportion and mix them to obtain mixed raw materials. The composition of the mixed raw materials by mass percentage includes: 3.5% Ni, 0.9% Si, 0.02% B, with the balance being Cu and unavoidable impurities. Place the mixed raw materials in a vacuum induction melting furnace, evacuate and fill with high-purity argon (Ar≥99.9%) to 0.03MPa. The melting furnace voltage is 200V, the current is 300A and the frequency is 900Hz. Melt at 1530℃ for 9min to obtain a uniform alloy melt. Cool the alloy melt to 1480℃ and then pour it into a 100mm×50mm×50mm mold.

[0084] (2) Cooling and intermittent electromagnetic stirring: The alloy melt poured into the mold is cooled to promote solidification. The cooling rate is 200℃ / min. The temperature is reduced to room temperature. During the cooling process, intermittent electromagnetic stirring is performed. The specific method of intermittent electromagnetic stirring is as follows: the alloy melt is stirred for the first time immediately after being poured into the mold. The stirring duration is 5s. Then, the stirring is repeated for 5s every 10s. The total stirring time is 130s. The stirring current frequency is 800Hz and the magnetic induction intensity is 0.7T. The ingot after cooling and intermittent electromagnetic stirring is obtained.

[0085] (3) Stepwise solution treatment: The temperature is raised to 840℃ at a rate of 10℃ / min. The ingot after cooling and intermittent electromagnetic stirring is subjected to stepwise solution treatment. After the first stage of solution treatment is completed, the temperature is raised to 920℃ at the same rate for the second stage of solution treatment. The first stage of solution treatment is: solution treatment at 840℃ for 1.5h; the second stage of solution treatment is: solution treatment at 920℃ for 1.5h. Then, the ingot is quenched in room temperature water at about 24℃. After the ingot temperature drops to room temperature, the surface moisture is dried with a blower to obtain the ingot after solution treatment.

[0086] (4) Cold rolling treatment: The solution-treated ingot is cold rolled at room temperature. There are 6 rolling passes, and the deformation amount per pass is 9%, with a total deformation amount of 54%. After rolling, the surface of the ingot is cleaned to remove surface dirt and impurities, and the cold-rolled ingot is obtained.

[0087] (5) Graded aging treatment: The cold-rolled ingot is first placed in a furnace at 380℃ for 5.5h for the first aging treatment, then at 490℃ for 5.5h for the second aging treatment, and finally air-cooled to room temperature to obtain the graded aging treatment ingot.

[0088] (6) Low temperature cooling treatment: The ingot after graded aging treatment is placed in a liquid nitrogen environment at -196℃ for 6 hours, and then slowly heated to room temperature at a rate of 5℃ / min to obtain copper-nickel-silicon alloy.

[0089] The grain size of the copper-nickel-silicon alloy prepared in this comparative example was statistically analyzed using a metallographic microscope and image analysis software. Tensile tests were conducted on the copper-nickel-silicon alloy prepared in this comparative example at room temperature using a universal testing machine. The experimental results showed that the average grain size of the copper-nickel-silicon alloy prepared in this comparative example was 40±9μm, the tensile strength was 635MPa, the yield strength was 552MPa, and the elongation was 13%.

[0090] Comparative Example 4, which only underwent the second step of cryogenic cooling, showed no significant change in average grain size, but its tensile strength and elongation decreased. This is because directly immersing the alloy from room temperature into liquid nitrogen and then holding it at that temperature subjected the alloy to a severe impact at low temperatures, resulting in thermal stress concentration within the alloy compared to before treatment. Performing a treatment at a higher temperature than the liquid nitrogen environment before direct immersion allows the alloy to adapt to the direct effects of lower temperatures, enabling gentler internal stress adjustment to reduce microcrack formation and thus improve the alloy's strength and toughness.

[0091] Comparative Example 5 A method for preparing a copper-nickel-silicon alloy is disclosed. This comparative example uses the same method as Example 1 to prepare the copper-nickel-silicon alloy, the only difference being that the magnetic induction intensity of the intermittent electromagnetic stirring treatment in this comparative example is 2T. The method specifically includes the following steps: (1) Melting and casting: Weigh copper, nickel, silicon and boron raw materials according to proportion and mix them to obtain mixed raw materials. The composition of the mixed raw materials by mass percentage includes: 2% Ni, 0.5% Si, 0.02% B, with the balance being Cu and unavoidable impurities. Place the mixed raw materials in a vacuum induction melting furnace, evacuate and fill with high-purity argon (Ar≥99.9%) to 0.03MPa. The melting furnace voltage is 200V, the current is 300A and the frequency is 900Hz. Melt at 1530℃ for 9min to obtain a uniform alloy melt. Cool the alloy melt to 1480℃ and then pour it into a 100mm×50mm×50mm mold.

[0092] (2) Cooling and intermittent electromagnetic stirring treatment: The alloy melt poured into the mold is cooled to promote solidification. The cooling rate is 200℃ / min. The temperature is reduced to room temperature. During the cooling process, intermittent electromagnetic stirring treatment is performed. The specific method of intermittent electromagnetic stirring treatment is as follows: the alloy melt is stirred for the first time immediately after being poured into the mold. The stirring duration is 5s. Then, the stirring is repeated for 5s every 10s. The total stirring time is 130s. The stirring current frequency is 800Hz and the magnetic induction intensity is 2T. The ingot after cooling and intermittent electromagnetic stirring treatment is obtained.

[0093] (3) Stepwise solution treatment: The temperature is raised to 830℃ at a rate of 10℃ / min. The ingot after cooling and intermittent electromagnetic stirring is subjected to stepwise solution treatment. After the first stage of solution treatment is completed, the temperature is raised to 915℃ at the same rate for the second stage of solution treatment. The first stage of solution treatment is: solution treatment at 830℃ for 1.5h; the second stage of solution treatment is: solution treatment at 915℃ for 1.5h. Then, the ingot is quenched in room temperature water at about 24℃. After the temperature of the ingot drops to room temperature, the surface moisture is dried with a blower to obtain the ingot after solution treatment.

[0094] (4) Cold rolling treatment: The solution-treated ingot is cold rolled at room temperature. The rolling passes are 7, the deformation amount per pass is 9%, and the total deformation amount is 63%. After rolling, the surface of the ingot is cleaned to remove surface dirt and impurities, and the cold-rolled ingot is obtained.

[0095] (5) Graded aging treatment: The cold-rolled ingot is first placed in a furnace at 375℃ for 5.5h for the first aging treatment, then at 480℃ for 5.5h for the second aging treatment, and finally air-cooled to room temperature to obtain the graded aging treatment ingot.

[0096] (6) Two-stage low-temperature cooling treatment: The ingot after the graded aging treatment is first placed in a low-temperature equipment at -90℃ for 4 hours, then slowly heated to room temperature at a rate of 5℃ / min, and then placed in a liquid nitrogen environment at -196℃ for 6 hours, and then slowly heated to room temperature at a rate of 5℃ / min to obtain copper-nickel-silicon alloy.

[0097] The grain size of the copper-nickel-silicon alloy prepared in this comparative example was statistically analyzed using a metallographic microscope and image analysis software. Tensile tests were conducted on the copper-nickel-silicon alloy prepared in this comparative example at room temperature using a universal testing machine. The experimental results showed that the average grain size of the copper-nickel-silicon alloy prepared in this comparative example was 24±4μm, the tensile strength was 615MPa, the yield strength was 508MPa, and the elongation was 11%.

[0098] Comparative Example 5 uses intermittent electromagnetic stirring with a higher magnetic induction intensity, resulting in finer grain size in the alloy material. However, the tensile strength decreases. This is because excessive magnetic induction intensity reduces equiaxed crystals and increases columnar crystals, and produces small structural defects such as pores. This leads to uneven stress and localized stress concentration in the alloy material during testing, making it more prone to fracture failure. Consequently, the toughness and strength of the alloy material decrease.

[0099] The various embodiments of the present invention have been described above. These descriptions are exemplary and not exhaustive, nor are they limited to the disclosed embodiments. Many modifications and variations will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments. The terminology used herein is chosen to best explain the principles, practical application, or improvement of the technology in the market, or to enable others skilled in the art to understand the embodiments disclosed herein.

Claims

1. A method of producing a copper-nickel-silicon alloy having a uniform fine-grained structure, characterized by, Specifically, the following steps are included: (1) Melting and casting: Weigh copper, nickel, silicon and boron raw materials according to proportion and mix them to obtain mixed raw materials. The mixed raw materials are vacuum melted in an inert atmosphere to obtain alloy melt. The alloy melt is poured into the mold to obtain alloy melt poured into the mold. (2) Cooling and intermittent electromagnetic stirring treatment: The alloy melt poured into the mold is cooled and intermittent electromagnetic stirring treatment is performed during the cooling process to obtain the ingot after cooling and intermittent electromagnetic stirring treatment. (3) Step-by-step solution treatment: The ingots after cooling and intermittent electromagnetic stirring are subjected to step-by-step solution treatment and then dried to obtain the solution-treated ingots. (4) Cold rolling: The solution-treated ingot is cold-rolled to obtain the cold-rolled ingot. (5) Graded aging treatment: The cold-rolled ingot is subjected to graded aging treatment to obtain graded aging treated ingot; (6) Two low-temperature cooling treatments: The ingots after graded aging treatment are subjected to two low-temperature cooling treatments to obtain a copper-nickel-silicon alloy with a uniform fine-grained structure.

2. The method of producing a copper-nickel-silicon alloy having a uniform fine-grain structure according to claim 1, characterized by, The raw materials mixed in step (1) include, by mass percentage: 1-4% nickel, 0.15-1.5% silicon, 0.02% boron, with the balance being copper and unavoidable impurities.

3. The method for preparing a copper-nickel-silicon alloy with a uniform fine-grained structure according to claim 1, characterized in that, The vacuum melting temperature in step (1) is 1450~1550℃ and the vacuum degree is 0.03MPa.

4. The method of producing a copper-nickel-silicon alloy having a uniform fine-grain structure according to claim 1, characterized by, The cooling rate of step (2) is 180~220℃ / min.

5. The method for preparing a copper-nickel-silicon alloy with a uniform fine-grained structure according to claim 1, characterized in that, The conditions for the intermittent electromagnetic stirring treatment in step (2) are: the electromagnetic stirring current frequency is 800Hz and the magnetic induction intensity is 0.01~1T; the specific method of the intermittent electromagnetic stirring treatment is: the first stirring is carried out immediately after the alloy melt is poured into the mold, the stirring duration is 5s, and then the stirring is repeated for 5s every 10s, and the total stirring time is 130s.

6. The method for preparing a copper-nickel-silicon alloy with a uniform fine-grained structure according to claim 1, characterized in that, The conditions for step (3) of the step-by-step solution treatment are as follows: the first-stage solution treatment is carried out at 820~840℃ for 1.5h, and then the second-stage solution treatment is carried out at 910~920℃ for 1.5h. After the second-stage solution treatment is completed, quenching treatment is carried out.

7. The method for preparing a copper-nickel-silicon alloy with a uniform fine-grained structure according to claim 1, characterized in that, The cold rolling process in step (4) consists of 6 to 8 passes, with a deformation of 6 to 9% per pass, and a total deformation of 36 to 72%.

8. The method for preparing a copper-nickel-silicon alloy with a uniform fine-grained structure according to claim 1, characterized in that, The conditions for the graded aging treatment in step (5) are as follows: the first-level aging treatment is carried out at 350~400℃ for 4~6 hours, the second-level aging treatment is carried out at 460~490℃ for 4~6 hours, followed by cooling, and the total time for the graded aging treatment is 8~12 hours.

9. The method for preparing a copper-nickel-silicon alloy with a uniform fine-grained structure according to claim 1, characterized in that, The conditions for the two cryogenic cooling treatments in step (6) are as follows: first, a first cryogenic cooling treatment of 4 hours is performed in an environment of -90℃, followed by warming; then, a second cryogenic cooling treatment of 6 hours is performed in a liquid nitrogen environment of -196℃, followed by warming.

10. A copper-nickel-silicon alloy with a uniform fine-grained structure prepared by the method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Static magnetic field cryogenic treatment method for improving strength and toughness of copper or copper alloy

    CN106498322A