High-strength, heat-resistant, and wear-resistant hypereutectic aluminum-silicon alloy for heavy-load, high-speed friction conditions and its preparation method

By combining high Mg and high Zn elements and Ce elements to improve the morphology of eutectic silicon and network Al2Cu phases, and by combining graded solid solution and double-stage aging heat treatment, the problem of insufficient strength and wear resistance of aluminum alloy materials under heavy load and high speed friction conditions has been solved, and aluminum alloy materials with high strength, excellent wear resistance and high temperature stability have been achieved.

CN123108362APending Publication Date: 2026-11-17NONFERROUS METALLIC OF HEBEI NEW LIZHONG GRP CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202611267155.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-20
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing aluminum alloy materials cannot simultaneously possess high strength and excellent wear resistance under heavy-load, high-speed friction conditions, and some solutions are costly or have limited processing capabilities, making them unsuitable for complex structural components.

Method used

By combining high Mg and high Zn, the Cu/Mg ratio is precisely controlled within the range of 2.5-4. Ce element is added to improve the morphology of eutectic silicon and network Al2Cu phases. Then, a multi-component nano-precipitated strengthening phase is formed by hierarchical solid solution and two-stage aging heat treatment, which improves the wear resistance and high temperature stability of the material.

Benefits of technology

It achieves a synergistic match of high strength, excellent wear resistance and good high temperature stability under heavy load and high speed friction conditions, and is suitable for large-scale production of complex structural parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108362A_ABST
    Figure CN123108362A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of aluminum alloy material preparation, and discloses a high-strength, heat-resistant, and wear-resistant hypereutectic aluminum-silicon alloy for heavy-load, high-speed friction conditions and its preparation method. By synergistically combining high Mg and high Zn to generate multi-component nano-precipitated strengthening phases, and by using Ce to improve the morphology of the eutectic silicon and network Al2Cu phases, the matrix's holding force on primary silicon is increased, reducing shedding and thus increasing wear resistance. Combined with graded solution treatment and double-stage aging heat treatment, the alloy achieves a room temperature tensile strength of 378-395 MPa, a high-temperature tensile strength of 342-353 MPa at 200℃, and a friction coefficient as low as 0.031-0.041. This achieves a synergistic match of high strength, excellent wear resistance, and good high-temperature stability under heavy-load, high-speed friction conditions, making it suitable for large-scale production of complex structural components such as compressor pump bodies.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of aluminum alloy material preparation, and relates to a high-strength, heat-resistant, and wear-resistant hypereutectic aluminum-silicon alloy for heavy-load, high-speed friction conditions and its preparation method. Background Technology

[0002] Aluminum alloys, due to their low density, good specific strength, and excellent corrosion resistance, have become key structural materials in aerospace, rail transportation, high-end equipment manufacturing, and new energy vehicles. As modern industry rapidly develops towards lightweighting, high speed, long service life, and high reliability, more stringent requirements are being placed on the comprehensive performance of aluminum alloy materials. Especially in applications such as moving parts, load-bearing structures, and friction pairs, the materials not only need to possess sufficiently high strength to withstand complex loads and high-temperature environments, but also must have excellent wear resistance to resist wear and extend service life.

[0003] Currently, most automotive air conditioning compressor pump body structural components are made of iron-based materials such as cast iron and stainless steel, resulting in a relatively large overall structural weight that is difficult to meet the development requirements of vehicle lightweighting, necessitating the replacement with aluminum alloys. However, existing aluminum alloy materials each have their own shortcomings in performance: traditional high-strength aluminum alloys, while achieving high strength through heat treatment, often lack sufficient wear resistance, leading to severe wear and component failure under dry friction or boundary lubrication conditions; while ordinary wear-resistant aluminum alloys often suffer from low strength or poor plasticity, making it difficult to meet the requirements of main load-bearing structures. Therefore, developing a new aluminum alloy material that combines high strength and excellent wear resistance has become a pressing technical challenge in this field. To this end, a large amount of research has been conducted in this field focusing on hypereutectic aluminum-silicon alloys, and the existing technologies are analyzed as follows: Chinese patent CN102965551A discloses a hypereutectic aluminum-silicon alloy for manufacturing engines, comprising 16.0%-19.0% silicon, 3.0%-4.0% copper, 0.40%-0.70% magnesium, 1.0%-2.0% nickel, 0.40%-1.2% rare earth element Re, 0.001%-0.006% phosphorus, <0.40% Fe, and <0.50% total other impurities, with the balance being aluminum. This solution addresses heat resistance and wear resistance by adding Ni and rare earth elements. However, due to the high cost of using precious metals and the low T6 strength and toughness of the material obtained through gravity casting and extrusion, it is difficult to meet the requirements of heavy-load, high-speed friction conditions.

[0004] The aluminum alloy disclosed in Chinese patent CN106893901A has the following composition: silicon 8%-15%, copper 0.5%-3%, magnesium ≤0.8%, iron ≤0.9%, nickel ≤0.5%, manganese ≤0.5%, and aluminum up to 100%. It is formed by T6 heat treatment of aluminum ingots followed by extrusion casting, resulting in a uniform distribution of spherical silicon eutectic within the α-Al solid solution, thereby achieving the required strength and friction performance. However, this method relies primarily on the wear resistance provided by the eutectic silicon in the eutectic aluminum-silicon alloy, which is insufficient for high-load, high-speed friction environments.

[0005] The aluminum alloy disclosed in Chinese patent CN112048644A has the following composition: Si: 0.05-23%, Cu: 0.05-8%, Mg: 0.02-1.5%, Ti: 0.04-0.10%, Mn: 0.10-0.50%, Cr: 0.01-0.08%, Ni: 0.05-2%, Zn: 0.05-4%, with the balance being Al. It is processed and shaped by methods such as heat treatment of aluminum ingots, rolling, pressing, and machining. This patent has a wide range of composition, relatively low strength (around 210-220 MPa), and relatively high coefficient of friction (0.15-0.17), making it unsuitable for processing wear-resistant parts with high loads and high speeds.

[0006] Chinese patent CN119979986A discloses a lightweight aluminum alloy with excellent wear resistance, comprising: zinc 0.1–0.3 wt%, copper 0.5–1 wt%, silicon 0.5–0.7 wt%, magnesium 0.8–1.2 wt%, titanium 0.1–0.3 wt%, cerium 0.05–0.2 wt%, manganese 0.1–0.2 wt%, nickel 0.1–0.3 wt%, impurity element iron less than 0.03 wt%, and other unavoidable impurity elements less than 0.005 wt%, with the balance being aluminum. The aluminum alloy is prepared using a process of melting and injection molding + salt spraying surface impact treatment + cleaning. High-speed impact of abrasives on the aluminum alloy surface introduces a residual stress field and simultaneously refines the grains. Furthermore, under the conditions of high-speed impact and high frictional temperature, the abrasives form a titanium-aluminum coating with the aluminum alloy matrix, significantly improving the mechanical properties and wear resistance of the aluminum alloy. However, the tested friction load of 10 N is too low and unsuitable for high-load friction environments. In addition, this spraying process is suitable for surface treatment of simple structural parts, but for complex porous structural parts, the uniformity of internal impact treatment will decrease.

[0007] Chinese patent CN117026024A discloses a separator with comprehensive mechanical properties and its preparation method, with the following composition: Fe 0.2-1%, Si 18-23%, Cu 2-6%, Mn 0.02-0.5%, Mg 0.1-0.8%, Cr 0-0.2%, Ni 1-2%, Zn 0.1-0.3%, Ti 0.1-0.5%, B 0-0.1%, rare earth elements 0.02-0.1%, Li 0.02-0.1%, V 0-0.1%, Sn 0-0.1%, Mo 0.5-2%, and the remainder being Al. The partition components are produced by melting and casting blanks + T6 heat treatment + machining. This scheme also adds Ni and rare earth elements, mainly focusing on low expansion coefficient (20℃-150℃ range, not greater than 16×10-6 / ℃), but the material hardness is low HB102-125, which is also not suitable for high load friction environment.

[0008] In summary, existing hypereutectic aluminum-silicon alloys mainly have the following problems: First, cost issues, some solutions rely on adding expensive Ni metal elements to improve performance, resulting in high material costs; second, insufficient performance issues, solutions without precious metals have low strength or limited wear resistance, making them unsuitable for heavy load conditions; third, process limitations issues, some solutions require additional surface treatment processes, resulting in low production efficiency and unsuitability for complex structural components.

[0009] Therefore, a high-strength, heat-resistant, and wear-resistant hypereutectic aluminum-silicon alloy is needed to meet the requirements of existing heavy-load, high-speed friction conditions. Summary of the Invention

[0010] To overcome the shortcomings of existing technologies, this invention provides a high-strength, heat-resistant, and wear-resistant hypereutectic aluminum-silicon alloy for heavy-load, high-speed friction conditions and its preparation method. Addressing the issues of high cost due to the addition of expensive Ni, and low strength and insufficient wear resistance in solutions without precious metals, this invention achieves this by synergistically combining high Mg and high Zn, precisely controlling the Cu / Mg ratio within the range of 2.5-4, and the Cu / Ce weight ratio within the range of 5-12. Ce element improves the morphology of the eutectic silicon and network Al₂Cu phases, increasing the matrix's holding force on primary silicon, reducing shedding, and thus increasing wear resistance and improving the material's wear resistance. Combining graded solution treatment and two-stage aging heat treatment, a synergistic match of high strength, excellent wear resistance, and good high-temperature stability is achieved in the material under heavy-load, high-speed (>250N) friction conditions.

[0011] The technical solution adopted by this invention to solve the technical problem is: This invention discloses a high-strength, heat-resistant, and wear-resistant hypereutectic aluminum-silicon alloy for heavy-duty, high-speed friction conditions. The alloy composition, by mass percentage, is as follows: Si 15-18%, Mg 0.8-1.5%, Cu 2.0-4.0%, Mn 0.25-0.55%, Fe 0.1-0.5%, Ti 0.05-0.1%, P 0.005-0.02%, Zn 3.0-6.0%, Ce 0.3-0.7%, Cu / Mg weight ratio 2.5-4, Cu / Ce weight ratio 5-12, with the remainder being aluminum and unavoidable trace impurities. The content of any single trace impurity element is ≤0.05%, and the total amount of trace impurities is ≤0.15%.

[0012] Preferably, the alloy composition by mass percentage is as follows: Si 16.5-17.7%, Mg 0.92-1.2%, Cu 3.0-3.2%, Mn 0.35%, Fe 0.25%, Ti 0.08%, P 0.009-0.01%, Zn 4.8-5.2%, Ce 0.3-0.5%, Cu / Mg weight ratio 2.5-4, Cu / Ce weight ratio 6-10, with the remainder being aluminum and unavoidable trace impurities, wherein the content of a single element of the trace impurity is ≤ 0.05%, and the total amount of trace impurities is ≤ 0.15%.

[0013] Preferably, the high-strength, heat-resistant, and wear-resistant hypereutectic aluminum-silicon alloy has a tensile strength of 350-400 MPa, a yield strength of 300-360 MPa, and an elongation after fracture of 0.5-2% at room temperature; and a tensile strength of 320-360 MPa, a yield strength of 310-340 MPa, and an elongation after fracture of 1-3% at 200℃.

[0014] Another aspect of the present invention discloses a method for preparing the above-mentioned high-strength, heat-resistant, and wear-resistant hypereutectic aluminum-silicon alloy for heavy-load, high-speed friction conditions, comprising the following steps: (1) Put 99.97% of A00 aluminum ingot, 3303 industrial silicon, electrolytic copper, AlMn10 master alloy, AlFe10 master alloy and AlTi10 master alloy into a melting furnace, heat to 850-860℃, stir after the aluminum ingot is completely melted, and take a sample to test the composition after standing. (2) After the alloy composition is qualified, adjust the temperature of the aluminum liquid to 820-830℃, add granular refining agent for spraying, and remove slag after standing. (3) Add 99.95% magnesium ingots and AlP4 master alloy to the aluminum alloy liquid after slag removal and stir for modification treatment. Incubate for 10-20 minutes for phosphorus modification, then add 99.5% metallic cerium blocks and stir for 3-5 minutes. (4) Maintain the temperature of the aluminum alloy liquid at 810-820℃ and connect it with argon gas for rotary degassing; (5) After refining and degassing, let it stand to remove slag; (6) The aluminum alloy liquid after slag removal enters the degassing box for online degassing; (7) After being degassed online, the aluminum alloy liquid enters the filter tank for filtration and purification, with a ceramic filter plate of 40 mesh. (8) Control the temperature of the aluminum alloy liquid to 780-800℃. The aluminum alloy liquid enters the preheated ingot mold and is poured into the preheated ingot mold. The mold is cooled by rotating water spray at the bottom to obtain the aluminum alloy ingot. After heat treatment, a high-strength, heat-resistant, and wear-resistant hypereutectic aluminum-silicon alloy is obtained.

[0015] Preferably, after the aluminum ingot is completely melted in step (1), it is stirred again for 2 minutes, and after standing for 10-20 minutes, a sample is taken to test the composition.

[0016] Preferably, in step (2), the granular refining agent is Sitong STJ-A1 granular refining agent, the amount added is 0.1-0.13% of the total amount of aluminum liquid, the blowing speed is 0.8-1.0 kg / min, the pressure of the connected argon gas is 0.6-0.8 MPa, and the mixture is left to stand for 10-20 min after refining.

[0017] Preferably, in step (4), the rotor speed for rotary degassing is 380-400 r / min, and the argon flow rate is 3-6 m³ / min. 3 / h; In step (6), the rotation speed of the dual rotors for online degassing is 430-450 r / min, and the argon flow rate is 15-25 L / min.

[0018] Preferably, the heat treatment adopts a staged solution treatment and two-stage aging method, specifically: the aluminum alloy ingot is heated to 420±5℃ at a heating rate of 5-10℃ / min, held for 2-3 hours, then heated to 480±5℃, held for 2-3 hours, and then quenched; after quenching, the ingot is heated to 120-130℃ at a heating rate of 5-10℃ / min, held for 3-4 hours, then heated to 170-180℃, held for 10-12 hours, and then air-cooled to room temperature.

[0019] The main elemental analysis of the aluminum alloy of this invention is as follows: With silicon (Si) as the main element, a Si content exceeding the eutectic point is called a hypereutectic cast aluminum alloy. In addition to eutectic silicon, primary silicon is also present in the microstructure, which is the main component contributing to the wear resistance of the material in this invention. In hypereutectic cast alloys, primary silicon is harder than the aluminum matrix. Under frictional conditions, the soft surface of the aluminum matrix is ​​easily worn, while the surface primary silicon, acting as hard particles, hinders friction. Lubricating oil accumulates in the wear pits of the aluminum matrix, continuously lubricating the surface. This dual effect further enhances wear resistance. However, higher Si content is not always better. High Si content leads to larger primary silicon crystals and severe segregation, resulting in decreased mechanical properties and wear resistance. Conversely, low Si content results in insufficient primary silicon to provide wear resistance. Therefore, the Si content in this invention is controlled at 15-18%, more preferably 16.5-17.7%.

[0020] Cu and Mg, as the main reinforcing elements, form reinforcing phases such as Q-Al5Cu2Mg8Si6, θ-Al2Cu, and β-Mg2Si with other elements. The Cu / Mg ratio is controlled within the range of 2.5-4. When the Cu / Mg ratio is below 2.5, the proportion of precipitated β-Mg2Si phase increases, while the proportions of Q-Al5Cu2Mg8Si6 and θ-Al2Cu phases decrease, and the copper-containing phase becomes the main high-temperature reinforcing phase, thus reducing the material's high-temperature performance. Conversely, when the Cu / Mg weight ratio is above 4, the precipitation of Q-Al5Cu2Mg8Si6 and θ-Al2Cu phases increases, leading to increased strength but decreased elongation. Therefore, this invention controls the Cu / Mg weight ratio within the range of 2.5-4 to achieve a balance between strength and toughness in the material.

[0021] Zn has high solid solubility in Al, with a large number of Zn atoms dissolved in the α-Al matrix, causing lattice distortion, hindering dislocation movement, and providing basic strength. However, the strengthening effect of adding Zn alone is limited; it must be combined with Mg and Cu to achieve high strength. During aging, Zn, Mg, and Cu form nanoscale dispersed strengthening phases, such as the η' phase (metastable MgZn2), η phase (stable MgZn2), T phase (Al2Mg3Zn3), and S phase (Al2CuMg). These fine, uniformly distributed precipitated strengthening phases strongly pin dislocations, significantly improving the alloy's strength. However, excessively high Zn content reduces plasticity, increases the tendency for hot cracking, and dramatically increases the susceptibility to stress corrosion cracking. Therefore, the Zn content is controlled at 3.0-6.0%, with 4.8-5.2% being more preferred.

[0022] Fe, as an impurity element, forms the AlFeSi phase, severely affecting the mechanical properties of the alloy. Adding Mn can replace Fe atoms in the acicular AlFeSi phase, forming a blocky AlFeMnSi phase, thus reducing the harmful effects of Fe. However, adding Mn leads to coarsening of the AlFeMnSi phase, which is detrimental to material properties. Furthermore, the addition of Fe and Mn improves mold release properties; these should be controlled within appropriate ranges to ensure performance while improving die-casting release. The Fe content should be controlled between 0.1-0.5%, with a further preferred 0.25%, and the Mn content between 0.25-0.55%, with a further preferred 0.35%.

[0023] Ti forms Al3Ti, which, on the one hand, allows for heterogeneous nucleation through dispersed distribution, promoting grain refinement and improving strength and plasticity; on the other hand, it forms stable precipitates, enhancing heat resistance and high-temperature strength. Excessive Ti can interfere with the modification effect of P and form harmful phases, reducing the material's mechanical properties.

[0024] An appropriate amount of Ce is a key element in improving the eutectic silicon and Al₂Cu phases. During solidification, Ce accumulates at the solid-liquid interface, delaying Cu atom precipitation, refining the grain boundary Al₂Cu network phase, and mitigating the problem of coarse, continuous, brittle Al₂Cu networks tearing the matrix. A small amount of Ce can pin the θ' phase, inhibiting Al₂Cu coarsening at high temperatures and improving high-temperature strength and thermal stability at 200℃. However, Ce > 0.7% easily leads to the formation of a coarse, brittle Al-Ce-Cu phase, resulting in a loss of aged strength and plasticity. Simultaneously, the Cu / Ce ratio needs to be controlled between 5 and 12 to ensure improved material properties while avoiding the formation of a coarse, brittle Al-Ce-Cu phase.

[0025] Phosphorus (P) is a key element in enhancing the properties of hypereutectic aluminum-silicon alloys. It primarily acts as a "modifier" in aluminum alloys, its core function being the refinement of the primary silicon phase. The crystal structure of AlP compounds is very similar to silicon, serving as an effective heterogeneous nucleation site for the silicon phase. This promotes the abundant and uniform nucleation of primary silicon in the melt, achieving a refinement effect. Refining the primary silicon significantly improves the alloy's hardness, wear resistance, and tensile strength; excessive P will have the opposite effect. Therefore, the P content is controlled at 0.005-0.02%, further preferably 0.009-0.01%.

[0026] Based on the above elemental formulation combined with graded solution treatment and two-stage aging heat treatment, the synergistic effect of the multi-element strengthening system can be fully utilized.

[0027] The graded solution treatment process achieves matrix homogenization and maximizes solute solution, thus constructing an aluminum matrix with high stability and high supersaturation.

[0028] Low-temperature solution treatment (420±5℃) can avoid the delamination defects caused by excessive dissolution of surface solute and insufficient dissolution of core solute. At the same time, it can effectively release casting residual stress, stabilize the morphology of primary silicon phase, and prevent abnormal coarsening of primary silicon particles in subsequent high-temperature stages.

[0029] High-temperature solution treatment (480±5℃) further dissolves the remaining undissolved Cu-Mg-Si and Mg-Zn intermetallic compounds into the α-Al matrix, significantly increasing the matrix supersaturation. Simultaneously, irregular, blocky, and coarse-edged primary silicon undergoes passivation, spheroidization, and refinement, dissolving some fine silicon particles, alleviating dendrite aggregation and regional segregation of primary silicon, reducing the matrix-cutting effect of coarse primary silicon, and improving stress concentration issues.

[0030] The two-stage aging process precisely controls the precipitation morphology, size and distribution of multi-component nano-reinforcing phases, achieving a synergistic improvement in toughness and wear resistance.

[0031] Low-temperature pre-aging (120-130℃) promotes the uniform formation of numerous fine and stable Mg-Zn and Mg-Si atom-enriched GP regions in the matrix, effectively avoiding the problems of local enrichment and abnormal coarsening of precipitates during subsequent high-temperature aging. This stage does not significantly change the macroscopic morphology of primary silicon, but it can promote the trace precipitation and uniform dispersion of silicon phase, stabilize the silicon phase microstructure, and inhibit the coarsening and growth of silicon phase during service.

[0032] Based on the high-density precursor core formed by low-temperature pre-aging, the peak aging temperature range (170-180℃) can drive the GP region to be uniformly transformed into β″, Q′, η′ nano-metastable strengthening phases, ensuring sufficient and uniform precipitation of the precipitated phases, which is compatible with the precipitation kinetics of the alloy's multi-component strengthening system.

[0033] Uniformly dispersed nano-reinforcing phases, along with the matrix, in-situ TiB2 particles, and primary silicon phases, form a multi-level wear-resistant synergistic system. The uniform refinement and dispersed distribution of primary silicon can form a continuous and stable hard wear-resistant skeleton, avoiding local enrichment or absence of hard phases, solving the phase segregation problem caused by high silicon content, ensuring uniform frictional force on the contact surface, and effectively suppressing spalling wear and abrasive wear; at the same time, optimizing the hardness of the matrix and the matching of silicon reduces the coefficient of friction, improves wear resistance stability under high temperature and high speed conditions, and is suitable for the service environment of compressor pump bodies.

[0034] The advantages and positive effects of this invention are: 1. This invention achieves high performance matching based on the low-cost Al-Si-Cu-Mg-Zn alloy system. Through the synergistic effect of high Mg (0.8%-1.5%) and high Zn (0.5%-6.0%), multi-component nano-precipitated strengthening phases such as β″, η′, and Q′ are formed. By precisely controlling the Cu / Mg ratio within the range of 2.5-4, the ratio of Q phase to θ phase is balanced, ensuring both room-temperature strength and high-temperature performance. By adjusting the Cu / Ce weight ratio to 5-12, Ce element improves the morphology of eutectic silicon and network Al2Cu phase, avoiding the formation of coarse and brittle phases, thereby increasing the matrix's holding force on primary silicon, reducing shedding, and enhancing wear resistance.

[0035] 2. This invention employs a staged solution treatment (420℃→480℃) and a two-stage aging process (120-130℃→170-180℃). Low-temperature solution treatment avoids surface overheating and delamination defects caused by insufficient core solution, releases residual casting stress, and prevents abnormal coarsening of primary silicon. High-temperature solution treatment allows Cu-Mg-Si and Mg-Zn intermetallic compounds to fully dissolve into the matrix, maximizing the solid solution strengthening effect. Low-temperature pre-aging forms a high-density GP region precursor core, preventing local enrichment and abnormal coarsening of precipitates during subsequent high-temperature aging. Peak aging drives the GP region to uniformly transform into β″, Q′, and η′ nano-metastable strengthening phases. This process route eliminates the need for additional steps such as extrusion, rolling, or surface impact, making it suitable for large-scale production of complex structural components such as compressor pump bodies.

[0036] 3. The alloy of this invention achieves a synergistic balance of high strength, excellent wear resistance, and good high-temperature stability under heavy-load, high-speed (>250N) friction conditions: Tensile strength at room temperature: 378-395 MPa; yield strength: 365-385 MPa; elongation after fracture: 0.62%-1.55%; Tensile strength at 200℃: 342-353 MPa; yield strength: 324-326 MPa; elongation after fracture: 1.21%-2.11%; Coefficient of friction: 0.031-0.041; Wear volume: 0.0038-0.0051 mm. 3 Brinell hardness 170-186 HBW. Attached Figure Description

[0037] Figure 1 This is a metallographic image of the sample from Example 1 magnified 100 times; Figure 2 The metallographic structure of Comparative Example 2 sample is magnified 100 times. Figure 3 The metallographic structure of Comparative Example 1 sample is magnified 100 times. Figure 4 Here is a SEM image of the sample from Example 1; Figure 5 The friction coefficient test diagram is shown for sample 3 in Example 3; Figure 6 This is a wear mark image of the sample from Example 3. Detailed Implementation

[0038] The present invention will be further described in detail below through specific embodiments. The following embodiments are merely descriptive and not limiting, and should not be used to limit the scope of protection of the present invention.

[0039] Example 1 A high-strength, heat-resistant, and wear-resistant hypereutectic aluminum-silicon alloy for heavy-duty, high-speed friction applications has the following alloy composition by mass percentage: Si 16.5%, Mg 1.1%, Cu 3.2%, Mn 0.35%, Fe 0.25%, Ti 0.08%, Zn 5%, Ce 0.4%, P 0.007%, with the remainder being aluminum and unavoidable trace impurities. The content of any single trace impurity element is ≤0.05%, and the total amount of trace impurities is ≤0.15%. The Cu / Mg weight ratio is 2.91, and the Cu / Ce weight ratio is 8.

[0040] The preparation method includes the following steps: (1) Put 99.97% of A00 aluminum ingot, 3303 industrial silicon, electrolytic copper, AlMn10 master alloy, AlFe10 master alloy and AlTi10 master alloy into the melting furnace, and heat the furnace to 850-860℃. Stir 1-3 times during the process. After the aluminum ingot is completely melted, stir again for 2 minutes. After standing for 10-20 minutes, take a sample to test the composition.

[0041] (2) After the alloy composition is qualified, adjust the temperature of the aluminum liquid to 820-830℃, weigh out 0.1-0.13% of the total amount of molten aluminum liquid and add it to the refining equipment. Adjust the parameters of the refining equipment and control the speed of blowing the granular refining agent to 0.8-1.0 kg / min. After connecting the refining equipment with argon gas at a pressure of 0.6-0.8 MPa, blow the granular refining agent evenly into the aluminum alloy liquid and let it stand for 10-20 minutes to allow the granular refining agent to react fully and float to the surface. Remove the slag formed on the surface of the aluminum alloy liquid for the first time. (3) Add 99.95% magnesium ingots and AlP4 master alloy to the aluminum alloy liquid after slag removal and stir for modification treatment. Incubate for 10-20 minutes for phosphorus modification, then add 99.5% metallic cerium blocks and stir for 3-5 minutes. (4) Maintain the temperature of the molten aluminum alloy at 810-820℃, use a rotary degasser in the melting furnace, connect it with argon gas at a pressure of 0.3-0.5MPa, control the rotor speed at 380-400r / min, and the argon gas flow rate at 3-6m³ / min. 3 / h; (5) After refining and degassing, let stand for 10-20 minutes to remove the slag formed on the surface of the aluminum alloy liquid; (6) The aluminum alloy liquid flows from the melting furnace into the degassing box along the flow channel. The degassing box is equipped with a dual-rotor rotary degasser for online degassing throughout the process. The degasser speed is set to 430-450 r / min and the argon flow rate is 15-25 L / min. (7) After being degassed online, the aluminum alloy liquid enters the filter tank for filtration and purification, with a ceramic filter plate of 40 mesh. (8) Control the temperature of the aluminum alloy liquid to 780-800℃. The aluminum alloy liquid enters the preheated ingot mold through the distributor. Adjust the flow control valve to control the flow rate of the aluminum alloy liquid. The aluminum alloy ingot is produced by rotating water spray cooling at the bottom of the ingot mold.

[0042] (9) Take the cast aluminum alloy ingot and heat it to 420±5℃ at a heating rate of 8℃ / min using the solution treatment process. Hold it for 2 hours, then heat it to 480℃ and hold it for 2-3 hours before quenching. After quenching, heat it to 120-130℃ at a heating rate of 8℃ / min and hold it for 3-4 hours. Then heat it to 170-180℃ and hold it for 10 hours before air cooling to room temperature.

[0043] Machining by turning on a lathe A 10mm diameter proportional test bar was used for mechanical property testing using a Sanstaijie CMT5105 universal electronic testing machine. Hardness and friction performance test samples were taken from the middle section of the ingot. Performance parameters are shown in Tables 2 and 3.

[0044] Example 2-3 The preparation method and sampling location are the same as in Example 1, the only difference being the element content. The specific element content is shown in Table 1, and the performance parameters are shown in Tables 2 and 3.

[0045] Comparative Examples 1-2 The preparation method and sampling location are the same as in Example 3. The Si element content is different in the comparison with Example 1. The specific element content is shown in Table 1, and the performance parameters are shown in Tables 2 and 3.

[0046] Comparative Examples 3-4 The preparation method and sampling location are the same as in Example 3. The Cu / Mg ratio is different in comparison with Example 3. The specific elemental contents are shown in Table 1, and the performance parameters are shown in Tables 2 and 3.

[0047] Comparative Example 5 The preparation method and sampling location are the same as in Example 2, using the standard grade ADC14. The specific elemental contents are shown in Table 1, and the performance parameters are shown in Tables 2 and 3.

[0048] Comparative Example 6 The composition and sampling location are the same as in Example 2. The difference lies in the heat treatment process. The heat treatment is carried out at 480℃ for 4 hours and then at 170℃ for 10 hours. The specific element content is shown in Table 1, and the performance parameters are shown in Tables 2 and 3.

[0049] Comparative Example 7 The preparation method and sampling location are the same as in Example 3, the only difference being the Ce element content of 0.9%. The specific element content is shown in Table 1, and the performance parameters are shown in Tables 2 and 3.

[0050] Comparative Example 8 The preparation method and sampling location are the same as in Example 2, the only difference being the Zn element content of 2.8%. The specific element content is shown in Table 1, and the performance parameters are shown in Tables 2 and 3.

[0051] Comparative Example 9 The preparation method and sampling location are the same as in Example 2, the only difference being that the Zn element is 7.1%, the specific element content is shown in Table 1, and the performance parameters are shown in Tables 2 and 3.

[0052] Comparative Example 10 The preparation method and sampling location are the same as in Example 2, the only difference being that the P element is 0.025%, the specific element content is shown in Table 1, and the performance parameters are shown in Tables 2 and 3.

[0053] Comparative Example 11 The preparation method and sampling location are the same as in Example 2, the only difference being that the P element is 0.002%, the specific element content is shown in Table 1, and the performance parameters are shown in Tables 2 and 3.

[0054] Comparative Example 12 The composition and sampling location are the same as in Example 2. The only difference is that the temperature is directly raised to 170-180℃ after quenching. The specific element content is shown in Table 1, and the performance parameters are shown in Tables 2 and 3.

[0055] Figure 1 The metallographic structure of the sample from Example 1 is magnified 100 times. It can be seen that the primary silicon crystals are evenly distributed and of similar size, with an average size of about 30 μm. Figure 2 The metallographic image of the Comparative Example 2 sample is magnified 100 times. It can be seen that the primary silicon has slight segregation and the size is not uniform, with an average size of about 50 μm. Figure 3 The metallographic structure of the Comparative Example 1 sample is magnified 100 times. It can be seen that the primary silicon content is small and the size is uneven, with an average size of about 45 μm.

[0056] Figure 4 The image shows the SEM image of the sample from Example 1. It can be seen that after Ce element regulation, the bright white Al2Cu phase transforms into a blocky structure, eliminating the network structure.

[0057] Figure 5The graph shows the relationship between the friction coefficient and time for the sample in Example 3. It can be seen that the friction coefficient stabilizes at 0.031 after 500s. Figure 6 The image shows the wear track pattern of the sample from Example 3. The average width of the wear track was 0.47 mm, and the calculated wear volume was 0.0043 mm. 3 This achieves the optimal wear level for the material.

[0058] Table 1. Element content (%) of Examples 1-3 and Comparative Examples 1-11

[0059] Table 2. Room temperature mechanical properties, Brinell hardness, and friction properties of the examples and comparative examples.

[0060] Friction test conditions: Lubrication used was Great Wall 4529 lubricating oil, load 260N, speed 400rpm, duration 60min. Test equipment: Jinan Chenda MH5 friction and wear tester; reference standard GB / T12444-2006 "Metallic Materials Wear Test Methods - Test Ring-Block Sliding Wear Test".

[0061] Table 3. High-temperature mechanical properties at 200℃ for the examples and comparative examples.

[0062] As can be seen from Tables 2 and 3, the mechanical and frictional properties of the alloys with adjusted Cu / Mg ratios and Zn content in Examples 1-3 are at a high level.

[0063] Comparative Examples 1-2 show that adjusting the Si content reduces alloy properties and hardness, leading to decreased wear resistance.

[0064] Comparative Examples 3-4 involved adjusting different Cu / Mg ratios. Below 2.5, the low Cu content led to an increased proportion of β-Mg₂Si phase precipitation and a decreased proportion of Q-Al₅Cu₂Mg₈Si₆ and θ-Al₂Cu phases, resulting in reduced material performance at both room and high temperatures. Above 4, the low Mg and high Cu ratios resulted in increased precipitation of Q-Al₅Cu₂Mg₈Si₆ and θ-Al₂Cu phases, leading to a slight increase in strength but a decrease in elongation, which was detrimental to improving strength and wear resistance.

[0065] Comparative Example 5 is an ADC14 alloy compared to Example 2. The material has high Cu and low Mg, and less Mg2Si strengthening phase. The material strength and wear resistance are lower than those of Example 2.

[0066] Comparative Example 6 uses single-stage solution treatment followed by aging. Compared to two-stage solution treatment, the solute solution cannot be maximized. Compared to the single-stage aging in Example 2, it cannot fully control the strengthening phase in the microstructure, resulting in limited improvement in material performance and an increase in friction coefficient and wear.

[0067] Comparative Example 7 increased the Ce content, with a Cu / Ce ratio of 3.4. Compared to Example 3, the higher Ce content would combine with Cu to form an Al-Ce-Cu needle-like brittle phase, which would break the matrix and reduce the material strength.

[0068] Comparative Examples 8-9 show that adjusting the Zn content can reduce the Zn content, which fails to provide sufficient reinforcement, while excessive Zn content increases the brittleness of the material and is detrimental to improving high-temperature performance.

[0069] In Comparative Examples 10-11, adjusting the phosphorus (P) content primarily affects the modification of primary silicon. A low P content results in fewer AlP nucleation sites, leading to insufficient primary silicon modification and larger particle sizes, which is detrimental to mechanical properties and wear resistance. Excessive P content exhibits a saturation effect, causing a large amount of excess AlP particles to agglomerate and sink to the bottom of the crucible, thus reducing the number of usable nucleation sites within the melt. This results in increased primary silicon size and uneven distribution, making the upper and lower castings prone to stratification and segregation, ultimately leading to a decrease in the material's mechanical properties and wear resistance.

[0070] Comparative Example 12 is a two-stage solid solution + single-stage aging. Compared with two-stage aging, the GP region of the directly high-temperature aging strengthening phase is more likely to coarsen and grow to form β, η, Q stable phases, which leads to a reduction in the proportion of multi-component nano-precipitated strengthening phases such as β″, η′, and Q′, which is not conducive to improving the strength of the material.

[0071] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several modifications and improvements can be made without departing from the inventive concept, and these all fall within the protection scope of the present invention.

Claims

1. A high-strength heat-resistant wear-resistant hypereutectic Al-Si alloy for heavy-load high-speed friction service, characterized in that, The alloy composition by mass percentage is as follows: Si 15-18%, Mg 0.8-1.5%, Cu 2.0-4.0%, Mn 0.25-0.55%, Fe 0.1-0.5%, Ti 0.05-0.1%, P 0.005-0.02%, Zn 3.0-6.0%, Ce 0.3-0.7%, Cu / Mg weight ratio 2.5-4, Cu / Ce weight ratio 5-12, with the remainder being aluminum and unavoidable trace impurities, wherein the content of a single trace impurity is ≤0.05%, and the total amount of trace impurities is ≤0.15%.

2. The high-strength heat-resistant wear-resistant hypereutectic Al-Si alloy according to claim 1, characterized in that, The alloy composition by mass percentage is as follows: Si 16.5-17.7%, Mg 0.92-1.2%, Cu 3.0-3.2%, Mn 0.35%, Fe 0.25%, Ti 0.08%, P 0.007-0.01%, Zn 4.8-5.2%, Ce 0.3-0.5%, Cu / Mg weight ratio 2.5-4, Cu / Ce weight ratio 6-10, with the remainder being aluminum and unavoidable trace impurities, wherein the content of a single trace impurity is ≤0.05%, and the total amount of trace impurities is ≤0.15%.

3. The high-strength heat-resistant wear-resistant hypereutectic Al-Si alloy according to claim 1, characterized in that, The high-strength, heat-resistant, and wear-resistant hypereutectic aluminum-silicon alloy has a tensile strength of 378-395 MPa, a yield strength of 365-385 MPa, and an elongation after fracture of 0.62-1.55% at room temperature; and a tensile strength of 342-353 MPa, a yield strength of 324-326 MPa, and an elongation after fracture of 1.21-2.11% at 200℃.

4. A method for preparing a high-strength, heat-resistant, and wear-resistant hypereutectic aluminum-silicon alloy as described in any one of claims 1-3, comprising the following steps: (1) Put 99.97% of A00 aluminum ingot, 3303 industrial silicon, electrolytic copper, AlMn10 master alloy, AlFe10 master alloy and AlTi10 master alloy into a melting furnace, heat to 850-860℃, stir after the aluminum ingot is completely melted, and take a sample to test the composition after standing. (2) After the alloy composition is qualified, adjust the temperature of the aluminum liquid to 820-830℃, add granular refining agent for spraying, and remove slag after standing. (3) Add 99.95% magnesium ingots and AlP4 master alloy to the aluminum alloy liquid after slag removal and stir for modification treatment. Incubate for 10-20 minutes for phosphorus modification, then add 99.5% metallic cerium blocks and stir for 3-5 minutes. (4) Maintain the temperature of the aluminum alloy liquid at 810-820℃ and connect it with argon gas for rotary degassing; (5) After refining and degassing, let it stand to remove slag; (6) The aluminum alloy liquid after slag removal enters the degassing box for online degassing; (7) After being degassed online, the aluminum alloy liquid enters the filter tank for filtration and purification, with a ceramic filter plate of 40 mesh. (8) Control the temperature of the aluminum alloy liquid to 780-800℃. The aluminum alloy liquid enters the preheated ingot mold and is poured into the preheated ingot mold. The mold is cooled by rotating water spray at the bottom to obtain the aluminum alloy ingot. After heat treatment, a high-strength, heat-resistant, and wear-resistant hypereutectic aluminum-silicon alloy is obtained.

5. The preparation method according to claim 4, characterized in that, Step (1) After the aluminum ingot is completely melted, stir again for 2 minutes, let stand for 10-20 minutes, and then take a sample to test the composition.

6. The preparation method according to claim 4, characterized in that, In step (2), the granular refining agent is Sitong STJ-A1 granular refining agent, the amount added is 0.1-0.13% of the total amount of aluminum liquid, the blowing speed is 0.8-1.0 kg / min, the pressure of the connected argon gas is 0.6-0.8 MPa, and it is left to stand for 10-20 min after refining.

7. The preparation method according to claim 4, characterized in that, In step (4), the rotational speed of the rotor for rotary degassing is 380-400 r / min, and the argon flow rate is 3-6 m 3 / h; in step (6), the rotational speed of the double rotor for in-line degassing is 430-450 r / min, and the argon flow rate is 15-25 L / min.

8. The preparation method according to claim 4, characterized in that, The heat treatment adopts a staged solution treatment and two-stage aging method. Specifically, the aluminum alloy ingot is heated to 420±5℃ at a heating rate of 5-10℃ / min, held for 2-3 hours, then heated to 480±5℃, held for 2-3 hours, and then quenched. After quenching, the ingot is heated to 120-130℃ at a heating rate of 5-10℃ / min, held for 3-4 hours, then heated to 170-180℃, held for 10-12 hours, and then air-cooled to room temperature.

Citation Information

Patent Citations

  • Hypereutectic aluminium-silicon alloy and preparation method thereof

    CN102965551A

  • Aluminum alloy material, crossed sliding ring of scroll compressor and preparation method of crossed sliding ring

    CN106893901A

  • Special aluminum alloy material for air conditioner compressor pump body and production process method

    CN112048644A

  • Partition plate with comprehensive mechanical performance, preparation method of partition plate and compressor

    CN117026024A

  • Lightweight aluminum alloy with excellent wear resistance and preparation method thereof

    CN119979986A