A 5-series aluminum alloy sheet and its preparation method

By introducing core-shell Al3(Er,Zr) nano-dispersed phases into 5-series aluminum alloy sheets, combined with low-temperature recovery annealing and two-stage stabilization treatment, the problem of Lüders band formation and reproduction was solved, realizing high-performance aluminum alloy sheets without Lüders bands, suitable for the intergranular corrosion resistance and stability requirements of automotive thin sheets.

CN123108364APending Publication Date: 2026-11-17TIANJIN ZHONGWANG ALUMINUM IND CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202611511939.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-28
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

The existing 5-series aluminum alloy sheets have Lüders band defects in the annealed state, which affect the appearance quality of the car body and the dimensional accuracy of the parts. Moreover, Lüders bands are easy to reproduce during the aging process at room temperature, which cannot meet the needs of large-scale application in high-end models.

Method used

By employing a low-Er core-shell dispersed phase design, combined with low-temperature recovery annealing and two-stage stabilization treatment, small-angle subgrain boundaries are pinned at the subgrain boundaries to suppress Mg atom diffusion. Trace amounts of Zn elements are used to optimize the grain boundary structure, forming a core-shell Al3(Er,Zr) nano-dispersed phase, eliminating Lüders bands and improving resistance to intergranular corrosion.

Benefits of technology

It has achieved the production of 5-series aluminum alloy sheets without Lüders bands, which have excellent resistance to intergranular corrosion and long-term stability, reduce the cost of rare earth raw materials, and are suitable for the industrial production of automotive thin sheets.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108364A_ABST
    Figure CN123108364A_ABST
Patent Text Reader

Abstract

This invention relates to the field of non-ferrous metal plastic processing technology, specifically to a 5-series aluminum alloy sheet and its preparation method. The components and their weight percentages are as follows: Mg: 3.8~4.8%, Mn: 0.20~0.50%, Er: 0.05~0.09%, Zr: 0.12~0.15%, Zn: 0.05~0.15%, Fe≤0.25%, Si≤0.15%, Cu≤0.10%, Ti: 0.01~0.05%, and the Er / Zr mass ratio is 0.34~0.75. The resulting aluminum alloy sheet has both resistance to intergranular corrosion and is free of Lüders bands.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of non-ferrous metal plastic processing technology, specifically to a 5-series aluminum alloy sheet and its preparation method. Background Technology

[0002] Driven by the trend towards lightweighting in the automotive industry, 5-series Al-Mg aluminum alloys have become the mainstream material for automotive body panels due to their excellent deep-drawing formability, corrosion resistance, and cost-effectiveness. However, this type of alloy has inherent defects: in the annealed state, dissolved Mg atoms form Cottrell gas clusters around dislocations, pinning them. During sheet metal stamping, yield plateaus and elongation at yield point (Ae) occur, ultimately forming Lüders bands on the surface of the parts. Lüders bands not only affect the appearance quality of the car body through the paint but also cause localized concentrated thinning of the sheet metal, leading to out-of-tolerance dimensional accuracy of parts. This is the core bottleneck restricting the large-scale application of 5-series aluminum alloys in high-end models.

[0003] Currently, there are long-standing and irreconcilable contradictions in the industry's technology:

[0004] (1) O-state and H111-state aluminum alloys: low yield strength and excellent formability, but have inherent Lüders bands; these can be temporarily eliminated by pre-deformation, but after the plates are stored for 3 to 6 months, Mg atoms continue to diffuse and re-pin dislocations at room temperature, the yield point elongation (Ae) increases, the Lüders band defects reappear, and the stamping stability decreases significantly.

[0005] (2) Work-hardened aluminum alloys such as H22 and H32: They have no Lüders band, but their yield strength is greatly improved (≥180MPa), with a high yield strength ratio and a significant decrease in elongation. They have poor deep drawing ability and cannot meet the forming requirements of complex automotive inner panels.

[0006] Current mainstream technologies for eliminating Lüders strips in 5-series aluminum alloys all have fatal shortcomings:

[0007] (1) Composition control method: By adjusting the content of Mg and Mn to coarse the grains, the material strength is sacrificed to obtain the effect of no Lüders band, but the problem of aging reproduction during room temperature storage is not solved.

[0008] (2) Pre-deformation treatment method: Free movable dislocations are introduced by cold rolling, bending and straightening and low temperature pre-stretching. Only Lüders bands can be eliminated when the product leaves the factory. The free dislocations are easily re-pinned by Mg atoms that diffuse at room temperature. After 3 to 6 months of storage, the defects are fully reproduced.

[0009] (3) High-temperature water quenching annealing method: Rapid quenching suppresses the segregation of solute atoms, but the plate has poor shape and high residual stress, and there is still a risk of Lüders band recurrence after storage.

[0010] (4) Single-stage low-temperature stabilization method: It can only delay the diffusion rate of Mg atoms, but cannot eliminate the thermodynamic driving force of dislocation pinning from the root, and the long-term stability is insufficient.

[0011] Existing Chinese patents CN104988441B and CN105908026A both rely on the idea of ​​"free dislocation elimination yielding platform", which fails to break through the underlying mechanism defects of room temperature diffusion repinning of dislocations by Mg atoms, and cannot completely solve the industry pain points.

[0012] Chinese patent CN108342626A discloses an Er addition of ≥0.10wt%, mainly targeting thick plates for marine engineering, but lacks a recovery annealing and two-stage stabilization design for thin automotive plates. Chinese patent CN103938038A discloses a stabilization heat treatment for Al-Mg-Zn-Er-Zr pentagonal alloy plates, but its Er content is 0.15~0.3wt% and the stabilization temperature is 240~250℃. Chinese patents CN118563230A and CN118563231A disclose a low-temperature two-stage treatment scheme to eliminate Lüdering, using a cryogenic temperature zone + low-temperature pre-stretching route. US patent US20250277295A1 discloses a recovery annealing scheme to eliminate Lüdering in 5-series alloys, but its process is a two-step method of recovery annealing + recrystallization annealing, and it does not use rare earth dispersed phases for long-term stability control.

[0013] In summary, there is an urgent need for a 5-series aluminum alloy sheet that combines resistance to intergranular corrosion with the absence of Lüders bands. Summary of the Invention

[0014] The present invention aims to solve the technical problem of how to provide a 5-series aluminum alloy sheet that has both resistance to intergranular corrosion and is free of Lüders bands.

[0015] To achieve the above objectives, the first aspect of the present invention provides a 5-series aluminum alloy sheet, wherein the components and their weight percentages in the 5-series aluminum alloy sheet are as follows:

[0016] Mg: 3.8~4.8%, Mn: 0.20~0.50%, Er: 0.05~0.09%, Zr: 0.12~0.15%, Zn: 0.05~0.15%, Fe≤0.25%, Si≤0.15%, Cu≤0.10%, Ti: 0.01~0.05%, other individual impurities ≤0.05%, total amount of other impurities ≤0.15%, balance Al;

[0017] The Er / Zr mass ratio is 0.34~0.75.

[0018] The second aspect of the present invention provides a method for preparing the above-mentioned 5-series aluminum alloy sheet, comprising the following steps: batching, melting and casting, homogenization heat treatment, hot rolling, first cold rolling, intermediate annealing, second cold rolling, finished product annealing, straightening and stretching, and stabilization heat treatment.

[0019] The melting and casting conditions include: melting temperature of 720~750℃, adding Al-Er, Al-Zr and Al-Zn master alloys sequentially at a temperature above 740℃, stirring, holding at the temperature for 15~30min, and after online degassing and filtration purification, semi-continuous casting at a rate of 40~70mm / min to obtain an ingot with a thickness of 500~600mm.

[0020] The beneficial effects of this invention are as follows:

[0021] (1) Completely eliminate the aging reproduction of Lüders bands. This invention uses core-shell nano-dispersed phases to anchor small-angle subgrain boundaries, low-temperature recovery to construct stable permanent dislocation sources, and bi-level stabilization to significantly reduce the free Mg concentration in the matrix, thereby cutting off the mechanism of Lüders band generation and aging reproduction from the metallurgical root.

[0022] (2) Low-cost rare earth ratio: The 5-series aluminum alloy sheet provided by this invention adopts an ultra-low Er ratio of 0.05~0.09wt%, which reduces the cost of rare earth raw materials by 40%~60%. Combined with the specific intermediate annealing, controllable straightening and other mass production adaptation processes provided by this invention, it has strong industrial applicability.

[0023] (3) Excellent resistance to intergranular corrosion. The 5-series aluminum alloy plate provided by the present invention introduces trace amounts of Zn elements to compete for segregation at grain boundaries, interrupting the continuous precipitation structure of the β-Al3Mg2 phase, and in conjunction with the two-stage stabilization to homogenize the distribution of matrix solutes. Attached Figure Description

[0024] Figure 1 This is a schematic diagram of the core-shell type Al3(Er,Zr) nano-precipitates uniformly dispersed in the matrix of Example 1 of the present invention.

[0025] Figure 2 This is a schematic diagram of the low-temperature recovery state tissues of Embodiment 1 and Comparative Example 3 of the present invention.

[0026] Figure 3 This is a comparison diagram of the engineering stress-strain curves of Embodiment 1, Comparative Example 1, and Comparative Example 2 of the present invention. Detailed Implementation

[0027] The endpoints and any values ​​of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of the various ranges, the endpoint values ​​of the various ranges and individual point values, and individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.

[0028] Existing technologies suffer from the technical bias that the low yield strength of 5-series aluminum alloys is inevitably accompanied by Lüders bands. This invention employs a preparation method that combines low-Er core-shell dispersed phase design, low-temperature recovery annealing, two-stage stabilization, and Zn microalloying to produce 5-series aluminum alloy sheets that possess excellent resistance to intergranular corrosion and are free of Lüders bands.

[0029] The first aspect of this invention provides a 5-series aluminum alloy sheet, wherein the components and their weight percentages in the 5-series aluminum alloy sheet are as follows:

[0030] Mg: 3.8~4.8%, Mn: 0.20~0.50%, Er: 0.05~0.09%, Zr: 0.12~0.15%, Zn: 0.05~0.15%, Fe≤0.25%, Si≤0.15%, Cu≤0.10%, Ti: 0.01~0.05%, other individual impurities ≤0.05%, total amount of other impurities ≤0.15%, balance Al;

[0031] The Er / Zr mass ratio is 0.34~0.75.

[0032] In this invention, an ultra-low Er content of 0.05~0.09 wt% is used, matched with a specific Zr content (0.12~0.15 wt%) and Er / Zr ratio (0.34~0.75), to precipitate an Al3Er core-Zr-rich shell core-shell structured dispersed phase through two-stage homogenization. This dispersed phase is uniformly distributed within the grains and at subgrain boundaries, which can permanently pin small-angle subgrain boundaries, stabilize the matrix microstructure, significantly reduce the matrix defect energy, inhibit the directional diffusion and segregation of Mg atoms towards dislocations and grain boundaries, reduce the number of Cottrell atmospheres generated from the source, and weaken the core driving force of dislocation pinning.

[0033] According to a preferred embodiment of the present invention, the Er / Zr mass ratio is 0.35~0.75.

[0034] The second aspect of the present invention provides a method for preparing the above-mentioned 5-series aluminum alloy sheet, characterized in that it includes the following steps: batching, melting and casting, homogenization heat treatment, hot rolling, first cold rolling, intermediate annealing, second cold rolling, finished product annealing, straightening and stretching, and stabilization heat treatment.

[0035] The melting and casting conditions include: melting temperature of 720~750℃, adding Al-Er, Al-Zr and Al-Zn master alloys sequentially at a temperature above 740℃, stirring, holding at the temperature for 15~30min, and after online degassing and filtration purification, semi-continuous casting at a rate of 40~70mm / min to obtain an ingot with a thickness of 500~600mm.

[0036] According to the present invention, the conditions for the homogenization heat treatment include: holding at 350~390℃ for 5~8h, then heating to 490~515℃ at a rate of 20~40℃ / h, holding at 490~515℃ for 5~8h, furnace cooling from 490~515℃ to 490~500℃ at a rate of 30~50℃ / h, and holding at 490~500℃ for 30~60min.

[0037] In this invention, Er atoms are activated by holding at 350~390℃ for 5~8h to precipitate pure Al3Er cores. Zr atoms have an extremely low diffusion coefficient at this temperature, and diffusion is effectively suppressed to avoid miscible precipitation. The temperature is increased to 490~515℃ at a rate of 20~40℃ / h with a gentle heating gradient to ensure that the Al3Er cores grow to the target size before the Zr shell precipitates, preventing the cores from dissolving or the shell structure from becoming disordered due to excessively rapid heating. During the heating process, the core continues to grow steadily without the formation of new phase nuclei. After holding at 490~515℃ for 5~8h, Zr atoms diffuse and activate at this temperature, growing epitaxially at the Al3Er core interface to form a Zr-rich shell. The core is then furnace-cooled to 490~500℃ at a rate of 30~50℃ / h and held at 490~500℃ for 30~60min to obtain a core-shell Al3(Er,Zr) nano-dispersed phase. The 490~500℃ mentioned above is a low-temperature sub-range within the high-temperature range of 490~515℃. Cooling down to this narrow temperature range and holding it is used to stabilize the already formed core-shell Al3(Er,Zr) nano-dispersed phase and avoid coarsening of the dispersed phase caused by prolonged high-temperature holding.

[0038] In this invention, during the homogenization heat treatment, the temperature is held at 490~515℃ for 5~8h, then furnace cooled from 490~515℃ to 490~500℃ at a rate of 30~50℃ / h, and then held at 490~500℃ for 30~60min. The temperature before furnace cooling is higher than the temperature after furnace cooling.

[0039] According to the present invention, the hot rolling conditions include: after the heat treatment for homogenization is completed, the ingot is not air-cooled out of the furnace and is hot-rolled, with an initial rolling temperature of 490~500℃, a final rolling temperature of 310~340℃, and hot-rolled to a billet with a thickness of 3.5mm. After rolling, the billet is air-cooled to 20~30℃.

[0040] According to the present invention, the conditions for the first cold rolling pass include: a reduction rate of 45.7% to 57.1% and a rolling thickness of 1.5 to 1.9 mm.

[0041] According to the present invention, the intermediate annealing conditions include: holding at 320~380℃ for 1~3 hours.

[0042] In this invention, unlike conventional complete recrystallization, the small-angle subgrain boundaries retained during intermediate annealing serve as primary permanent dislocation sources. Unlike free dislocations that are easily pinned by Mg atoms, small-angle subgrain boundaries are thermodynamically stable interfaces and are unlikely to become core sites for the large-scale accumulation of Mg atoms; however, trace amounts of Mg atom segregation can still occur during long-term room temperature storage. This invention relies on the core-shell Al3(Er,Zr) dispersed phase to continuously pin the subgrain boundaries, combined with subsequent bi-stage stabilization to consume free Mg in the matrix, thus synergistically suppressing the large-scale accumulation of Mg atoms in pinned dislocations at the subgrain boundaries. During stamping deformation, the subgrain boundaries can continuously and uniformly emit mobile dislocations without needing to break through solute atom pinning, completely eliminating the stress-strain yield plateau and achieving zero Ae and no Lüders bands.

[0043] According to the present invention, the conditions for the second cold rolling pass include: rolling to a finished thickness of 0.95~1.05 mm and a total cold rolling reduction of 70~72.9%.

[0044] In this invention, the total cold rolling reduction rate is the reduction rate from hot-rolled billet to finished sheet.

[0045] According to the present invention, the conditions for annealing the finished product include: annealing the finished product in an air-cushion continuous annealing furnace, heating to 280~360°C at a rate of ≥50°C / s, holding at that temperature for 15~60s, and then cooling to 20~30°C at a rate of 5~15°C / s in an air-cushion cooling section.

[0046] According to the present invention, the conditions for the straightening stretch include: straightening elongation ≤ 0.3%.

[0047] According to the present invention, the conditions for the stabilization heat treatment include: holding at 100~130℃ for 45~90 min, air cooling to 20~30℃, and holding at 160~175℃ for 8~18 min followed by air cooling to 20~30℃.

[0048] In this invention, the highly active Mg atoms in the solid solution state of the matrix diffuse to the subgrain boundaries and the dispersed phase interface after being kept at 100~130℃ for 45~90min and then air-cooled, forming a low-concentration uniform gas cloud. This reduces the free Mg concentration in the matrix to below the room temperature aging threshold, effectively suppressing the secondary rearrangement and dislocation repinning of Mg atoms during long-term storage. It also activates the diffusion and segregation of Zn atoms to the grain boundaries (Zn has a significantly higher diffusion rate in Al at 100~130℃ than Mg), preferentially occupying active sites at the grain boundaries, constructing a grain boundary Zn enrichment layer, and competitively suppressing the grain boundary directional diffusion path of Mg atoms.

[0049] After holding at 160~175℃ for 8~18 minutes, air-cool to 20~30℃ to selectively eliminate large-angle metastable subgrain boundaries. The trace amounts of Mg atoms released by the relaxation of the subgrain boundary structure form GP region precursors in the crystal, resulting in trace baking hardening.

[0050] In this invention, after stabilization heat treatment, the grains exhibit a fibrous or elongated morphology along the rolling direction, with a grain size of 15-30 μm. No recrystallization occurs, and there are no equiaxed recrystallized grains. After annealing, the matrix retains a large number of small-angle subgrain boundaries. These subgrain boundaries are thermodynamically stable and can act as permanent dislocation sources to continuously emit mobile dislocations during subsequent stamping deformation. Unlike the non-substructure state of a fully recrystallized structure, the retention of restored subgrain boundaries is the microstructural basis for eliminating the yield plateau. Core-shell Al3(Er,Zr) nano-dispersed phases are uniformly pinned at the subgrain boundaries, stabilizing the subgrain boundary structure and inhibiting subgrain boundary migration and merging during long-term room temperature storage and subsequent stamping deformation. The microstructure is in a restored state, without large-angle recrystallized grains. After two-stage stabilization treatment, large-angle metastable subgrain boundaries are selectively eliminated, and the remaining small-angle stable subgrain boundaries do not evolve during long-term storage, ensuring long-term stability of the microstructure and properties.

[0051] In this invention, the high-density core-shell Al3(Er,Zr) nanophase precipitated by bi-stage homogenization significantly pins dislocation movement, resulting in a substantial increase in the cold rolling work hardening rate. This can easily lead to strip breakage and poor sheet shape. A specific intermediate annealing is added between the first and second cold rolling passes to eliminate work hardening accumulation, restore sheet plasticity, and ensure that the sheet shape and surface quality meet the standards under specific total reduction conditions.

[0052] The large-angle metastable subgrain boundaries retained during the annealing of finished products are prone to subgrain merging and interface migration during the subsequent aluminum alloy baking process at 175~185℃, resulting in excessive softening of the baking paint. Through stabilization heat treatment, the high-energy large-angle metastable substructure is consumed in advance, releasing the residual stress in the structure. At the same time, the trace amount of Mg released by the relaxation of subgrain boundaries is used to form GP precursors, and the baking hardening effect is used to precisely compensate for the softening of the structure.

[0053] The presence of numerous subgrain boundaries and interface defects provides diffusion channels for Mg atoms. Under long-term humid and hot conditions, the β-Al3Mg2 phase readily precipitates continuously at the grain boundaries, forming continuous corrosion channels. Introducing trace amounts of Zn (0.05~0.15wt%) induces competitive segregation at grain boundaries, preferentially occupying active sites and disrupting the continuous precipitation of the β-phase. Combined with specific homogenization of the solute distribution in the heat-treated matrix, nitric acid intergranular corrosion (NAMLT) tests were conducted according to ASTM G67 standards, controlling the intergranular corrosion mass loss per unit area to within 15 mg / cm². 2 Within.

[0054] Test methods

[0055] Chemical composition was determined according to GB / T 7999-2015.

[0056] Mechanical property testing: The yield strength Rp0.2 and elongation after fracture A50 of the plate were tested in accordance with GB / T 16865.

[0057] The yield point elongation Ae was determined according to GB / T 16865.

[0058] Intergranular corrosion performance was determined according to ASTM G67.

[0059] The technical solution of the present invention will be further described in detail below with reference to the accompanying drawings and embodiments. Obviously, the embodiments described herein are only some embodiments of the present invention and are not intended to limit the present invention. All other embodiments implemented by those skilled in the art based on the embodiments of the present invention without creative improvements are within the protection scope of the present invention.

[0060] Example 1

[0061] Raw materials and ingredients

[0062] Mg: 4.5%, Mn: 0.35%, Er: 0.07%, Zr: 0.12%, Zn: 0.10%, Fe: 0.15%, Si: 0.08%, Cu: 0.05%, Ti: 0.02%, other individual impurities ≤0.05%, total amount of other impurities ≤0.15%, balance Al, Er / Zr=0.58;

[0063] The melting temperature is 720-750℃. At a temperature above 740℃, Al-Er, Al-Zr, and Al-Zn master alloys are added sequentially, stirred, and held for 30 minutes. After online degassing and filtration purification, the ingot is semi-continuously cast at a rate of 60 mm / min to obtain an ingot with a thickness of 580 mm.

[0064] Two-stage homogenization at 370℃ for 6 hours, heating to 505℃ at 30℃ / h, heating to 505℃ for 6 hours, furnace cooling to 495℃ at a rate of 40℃ / h, and holding at that temperature for 30 minutes.

[0065] After the homogenization heat treatment is completed, the ingot is not air-cooled out of the furnace and is hot-rolled. The hot rolling starts at 495℃ and ends at 320℃, and is hot-rolled to a billet with a thickness of 3.5mm.

[0066] The first cold rolling pass achieves a thickness of 1.6 mm, with a reduction rate of 54.3%.

[0067] Intermediate annealing at 350℃ for 2 hours;

[0068] The second cold rolling process reduces the finished product thickness to 1.0 mm, with a total reduction rate of 72%.

[0069] The finished product is annealed at a rate of 65℃ / s to 330℃, 330℃×30s, and then air-cooled to 25℃ at a rate of 5~15℃ / s.

[0070] The straightening elongation rate was 0.15%;

[0071] Stabilization heat treatment: 120℃×60min, air-cooled to 25℃, 165℃×12min, air-cooled to 25℃.

[0072] A1 5-series aluminum alloy sheet was prepared.

[0073] Example 2

[0074] The raw material composition is Mg: 4.8%, Mn: 0.30%, Er: 0.05%, Zr: 0.13%, Zn: 0.08%, Fe: 0.18%, Si: 0.10%, Cu: 0.04%, Ti: 0.03%, other individual impurities ≤0.05%, total amount of other impurities ≤0.15%, balance Al, Er / Zr=0.38;

[0075] The 5-series aluminum alloy sheet A2 was prepared according to the method in Example 1.

[0076] Example 3

[0077] The raw material composition is Mg: 4.2%, Mn: 0.40%, Er: 0.05%, Zr: 0.14%, Zn: 0.12%, Fe: 0.18%, Si: 0.08%, Cu: 0.04%, Ti: 0.02%, other individual impurities ≤0.05%, total amount of other impurities ≤0.15%, balance Al, Er / Zr=0.36;

[0078] The preparation method is the same as in Example 1, except that the homogenization heat treatment is 390℃×8h, heated to 505℃ at 30℃ / h, 505℃×6h, furnace cooled to 495℃ at a rate of 40℃ / h, and held for 30min.

[0079] A3 5-series aluminum alloy sheet was obtained.

[0080] Comparative Example 1

[0081] Standard 5182-O fully recrystallized board.

[0082] Standard 5182 aluminum alloy (Mg: 4.5%, Mn: 0.35%, without Er, Zr, Zn).

[0083] Single-stage homogenization, complete recrystallization annealing at 490-520℃, holding for 60-90 seconds, and then directly rolled up without straightening after annealing.

[0084] DA1 5-series aluminum alloy sheet was prepared.

[0085] Comparative Example 2

[0086] The existing H111 pre-deformation process.

[0087] Standard 5182 aluminum alloy, Mg: 4.5%, Mn: 0.35%, free of Er, Zr, and Zn.

[0088] Air cushion furnace 490~520℃×60~90s, complete recrystallization annealing, online stretch bending and straightening, elongation 1.0~1.5%, i.e. industry standard H111 pre-deformation process, then winding after straightening.

[0089] DA2 5-series aluminum alloy sheet was prepared.

[0090] Comparative Example 3

[0091] The raw material composition and preparation method are the same as in Example 1, except that in the preparation method, the finished product is annealed at 500°C for complete recrystallization and held for 65 seconds, without stabilization heat treatment.

[0092] DA3 5-series aluminum alloy sheet was prepared.

[0093] Comparative Example 4

[0094] The alloy composition and preparation method are the same as in Example 1, except that Er is 0.03%.

[0095] DA4 5-series aluminum alloy sheet was produced.

[0096] Comparative Example 5

[0097] The alloy composition and preparation method are the same as in Example 1, except that the composition does not contain Er and Zr, and the preparation method does not include homogenization heat treatment.

[0098] DA5 5-series aluminum alloy sheet was produced.

[0099] Comparative Example 6

[0100] The raw material composition and preparation method are the same as in Example 1, except that there is no stabilization heat treatment in the preparation method.

[0101] DA6 5-series aluminum alloy sheet was produced.

[0102] Comparative Example 7

[0103] The raw material composition and preparation method are the same as in Example 1, except that the composition does not contain Zn.

[0104] DA7 5-series aluminum alloy sheet was produced.

[0105] Comparative Example 8

[0106] The raw material composition and preparation method are the same as in Example 1, except that the stabilization heat treatment is 120°C × 60 min, followed by air cooling to 25°C.

[0107] DA8 5-series aluminum alloy sheet was produced.

[0108] Performance tests were performed on A1-A3 and DA1-DA8, as shown in Table 1.

[0109] Table 1

[0110]

[0111] By comparing the examples and the comparative examples, it can be seen that, compared with Example 1, Comparative Example 5 has Ae=0.3% in 6 months when there is no dispersed phase, which proves the irreplaceable role of dispersed phase pinning subgrain boundaries in long-term stability.

[0112] Comparing Comparative Example 3 and Example 1, the Ae value was 1.1% in 6 months without recovery annealing, demonstrating the irreplaceable role of low-temperature recovery annealing in the initial elimination of Lüders bands.

[0113] Comparing Example 6 and Example 1, Ae=0.5% without bi-stage stabilization for 6 months demonstrates the dual non-substitutability of bi-stage stabilization.

[0114] Comparison of Example 7 and Example 1: Mass loss reached 28 mg / cm³ without Zn. 2 This demonstrates the irreplaceable role of Zn microalloying in corrosion resistance.

[0115] Figure 3In Example 1 of this invention, the plate has no yield plateau and Ae=0; in Comparative Example 1, the conventional 5182-O aluminum alloy has Ae≈2.0%; and in Comparative Example 2, the H111 pre-deformed aluminum alloy has Ae=0.8%.

[0116] The above embodiments and comparative examples illustrate that only when the internal micro-dispersed phase generated by specific homogenization, recovery annealing, two-stage stabilization, and Zn microalloying work synergistically can all performance indicators be achieved simultaneously.

[0117] The above description is merely a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the scope of the technology disclosed in the present invention, based on the technical solution and inventive concept of the present invention, should be covered within the scope of protection of the present invention.

Claims

1. A 5-series aluminum alloy sheet, characterized in that, The components and their weight percentages in the 5-series aluminum alloy sheet are as follows: Mg: 3.8~4.8%, Mn: 0.20~0.50%, Er: 0.05~0.09%, Zr: 0.12~0.15%, Zn: 0.05~0.15%, Fe≤0.25%, Si≤0.15%, Cu≤0.10%, Ti: 0.01~0.05%, other individual impurities ≤0.05%, total amount of other impurities ≤0.15%, balance Al; The Er / Zr mass ratio is 0.34~0.

75.

2. The 5-series aluminum alloy sheet according to claim 1, characterized in that, The Er / Zr mass ratio is 0.35~0.

75.

3. The method for preparing the 5-series aluminum alloy sheet according to claim 1 or 2, characterized in that, The process includes the following steps: batching, melting and casting, homogenization heat treatment, hot rolling, first cold rolling, intermediate annealing, second cold rolling, finished product annealing, straightening and stretching, and stabilization heat treatment. The melting and casting conditions include: melting temperature of 720~750℃, adding Al-Er, Al-Zr and Al-Zn master alloys sequentially at a temperature above 740℃, stirring, holding at the temperature for 15~30min, and after online degassing and filtration purification, semi-continuous casting at a rate of 40~70mm / min to obtain an ingot with a thickness of 500~600mm.

4. The method for preparing 5-series aluminum alloy sheet according to claim 3, characterized in that, The homogenization heat treatment conditions include: holding at 350~390℃ for 5~8h, then heating to 490~515℃ at a rate of 20~40℃ / h, holding at 490~515℃ for 5~8h, furnace cooling from 490~515℃ to 490~500℃ at a rate of 30~50℃ / h, and holding at 490~500℃ for 30~60min.

5. The method for preparing 5-series aluminum alloy sheet according to claim 3, characterized in that, The hot rolling conditions include: after the heat treatment for homogenization is completed, the ingot is not air-cooled out of the furnace and is hot-rolled. The initial rolling temperature is 490~500℃, the final rolling temperature is 310~340℃, and the billet is hot-rolled to a thickness of 3.5mm. After rolling, the billet is air-cooled to 20~30℃.

6. The method for preparing 5-series aluminum alloy sheet according to claim 3, characterized in that, The conditions for the first cold rolling pass include: a reduction rate of 45.7% to 57.1% and a rolling thickness of 1.5 to 1.9 mm.

7. The method for preparing 5-series aluminum alloy sheet according to claim 3, characterized in that, The intermediate annealing conditions include: holding at 320~380℃ for 1~3 hours.

8. The method for preparing 5-series aluminum alloy sheet according to claim 3, characterized in that, The conditions for the second cold rolling pass include: rolling to a finished thickness of 0.95~1.05 mm, and a total cold rolling reduction of 70~72.9%.

9. The method for preparing 5-series aluminum alloy sheet according to claim 3, characterized in that, The conditions for annealing the finished product include: annealing the finished product using an air cushion continuous annealing furnace, heating to 280~360℃ at a rate of ≥50℃ / s, holding at that temperature for 15~60s, and then cooling to 20~30℃ at a rate of 5~15℃ / s through an air cushion cooling section. The conditions for straightening and stretching include: straightening elongation ≤ 0.3%.

10. The method for preparing 5-series aluminum alloy sheet according to claim 3, characterized in that, The conditions for the stabilization heat treatment include: holding at 100~130℃ for 45~90 min, air cooling to 20~30℃, and holding at 160~175℃ for 8~18 min followed by air cooling to 20~30℃.

Citation Information

Patent Citations

  • Stabilization heat treatment process for high-Mg aluminum alloy sheet containing Zn and Er and capable of resisting long-term intergranular corrosion

    CN103938038A

  • A manufacturing method for eliminating Lüders bands on the surface of 5754 aluminum alloy plate

    CN104988441B

  • 5xxx aluminum alloy board for automobile body and manufacturing method thereof

    CN105908026A

  • Erbium-containing oceangraphic engineering and goods stock aluminum alloy and plate manufacturing method thereof

    CN108342626A

  • AlMg wrought aluminum alloy and low-temperature prestretching control method for improving surface quality

    CN118563230A