An aluminum alloy conductive busbar and its heat treatment method
Patent Information
- Application Number
- CN202611401158.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-10
- Publication Date
- 2026-11-17
AI Technical Summary
[0004]本发明要解决的技术问题是:现有铝合金导电母排在兼顾导电性能、机械强度及折弯性能时,存在铝合金组成与热处理状态难以稳定匹配,以及不同公称厚度母排缺少明确、可执行的人工时效制度对应关系的问题,为此提出一种铝合金导电母排及其热处理方法
Smart Images

Figure CN123108367A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of aluminum alloy materials and heat treatment technology, and in particular to an aluminum alloy conductive busbar and its heat treatment method. Background Technology
[0002] Aluminum alloy conductive busbars are characterized by their light weight, good conductivity, and good machinability, and are widely used in electrical equipment and power connection components. Al-Mg-Si aluminum alloys can achieve certain strengthening effects through solution treatment and aging treatment. However, the presence of alloying elements such as Mg and Si in the Al matrix after solution treatment increases the scattering of conduction electrons. Furthermore, the precipitation of related components during artificial aging simultaneously alters the material's strength, conductivity, and plasticity. Therefore, conductive busbars require a balance between conductivity and mechanical properties.
[0003] However, in actual production, existing aluminum alloy conductive busbars still face the challenge of consistently matching material composition with heat treatment conditions. On one hand, increasing the Mg-Si strengthening degree improves the mechanical properties of the busbar, but it increases the difficulty of controlling conductivity and bending performance. On the other hand, busbars of different nominal thicknesses have different cross-sectional dimensions, resulting in variations in temperature response and microstructure adjustment during heat treatment. A single artificial aging process cannot adequately cover the process requirements of different specifications. Furthermore, elements such as Fe, Ti, Mn, and Cr also affect the plasticity and conductivity of the material, necessitating continuous control over the aluminum alloy chemical composition, online solution treatment after hot extrusion, and artificial aging processes corresponding to different thicknesses. Summary of the Invention
[0004] The technical problem to be solved by the present invention is that existing aluminum alloy conductive busbars, when taking into account conductivity, mechanical strength and bending performance, have problems such as difficulty in stably matching aluminum alloy composition and heat treatment state, and lack of clear and executable artificial aging system correspondence for busbars with different nominal thicknesses. To this end, an aluminum alloy conductive busbar and its heat treatment method are proposed.
[0005] To achieve the above objectives, the first aspect of this application adopts the following technical solution: an aluminum alloy conductive busbar, wherein, by mass percentage, the aluminum alloy comprises 0.60%-0.65% Mg, 0.40%-0.45% Si, Fe≤0.15%, Cu≤0.05%, Mn≤0.03%, Cr≤0.03%, Zn≤0.05%, Ti≤0.01%, B 0.03%-0.05%, with the balance being Al.
[0006] Preferably, the width of the aluminum alloy conductive busbar is 20-400mm and the thickness is 2-20mm.
[0007] Preferably, the conductivity of the aluminum alloy conductive busbar at 20°C is not less than 58% IACS.
[0008] Preferably, the tensile strength of the aluminum alloy conductive busbar is not less than 140 MPa.
[0009] Preferably, the bending radius of the aluminum alloy conductive busbar when it is bent at 90° along the extrusion direction is 15mm, and there are no crack defects on the surface of the bending area.
[0010] The second aspect of this application adopts the following technical solution: a heat treatment method for aluminum alloy conductive busbars, wherein the nominal thickness of the aluminum alloy conductive busbars is 3.20-20.00 mm; the aluminum alloy conductive busbars formed by hot extrusion are subjected to online solution treatment, wherein the solution temperature of the aluminum alloy conductive busbars in the online solution treatment is 520℃, and after the online solution treatment, they are rapidly cooled so that the discharge temperature of the rapidly cooled aluminum alloy conductive busbars does not exceed 100℃, and then artificial aging treatment is performed according to the nominal thickness of the aluminum alloy conductive busbars.
[0011] When the nominal thickness of the aluminum alloy conductive busbar is 3.20-10.00mm, the artificial aging process shall be one of the following: 200℃×7h, 210℃×7h, 225℃×3h, or 280℃×6h.
[0012] When the nominal thickness of the aluminum alloy conductive busbar is 10.01-12.50mm, the artificial aging process shall be one of 200℃×8h, 210℃×8h, 225℃×3h or 280℃×6h.
[0013] When the nominal thickness of the aluminum alloy conductive busbar is 12.51-20.00mm, the artificial aging process shall be one of 210℃×9h, 225℃×4h, 225℃×4.5h or 280℃×6h.
[0014] The artificial aging conditions of 200℃, 210℃, 225℃ and 280℃ mentioned above are respectively combined with the corresponding nominal thickness to form a heat dissipation treatment combination, and each artificial aging temperature and artificial aging time is implemented according to the corresponding combination.
[0015] The technical effects and advantages of this invention are as follows: In this invention, by controlling the main strengthening elements Mg and Si, along with elements such as Fe, Ti, Mn, Cr, and B, within corresponding ranges, the material composition basis of the aluminum alloy conductive busbar is established; after hot extrusion, online solution treatment at 520℃ and rapid cooling are adopted to ensure that the discharge temperature of the rapidly cooled aluminum alloy conductive busbar does not exceed 100℃; then, according to the nominal thickness of the busbar, artificial aging regimes of 200℃, 210℃, 225℃, or 280℃ are matched, so that different specifications of busbars have clear discrete aging process selection, which is conducive to coordinating the conductivity, tensile strength, and bending performance of the aluminum alloy conductive busbar. Attached Figure Description
[0016] The disclosure of this invention is illustrated with reference to the accompanying drawings. It should be understood that the drawings are for illustrative purposes only and are not intended to limit the scope of protection of this invention.
[0017] Figure 1 This is a schematic diagram of the aluminum alloy conductive busbar of the present invention;
[0018] Figure 2 This is a schematic diagram of the process flow for the heat treatment method of aluminum alloy conductive busbar of the present invention;
[0019] Figure 3 This is a schematic diagram comparing the conductivity and tensile strength at 20°C under different artificial aging regimes according to the present invention;
[0020] Figure 4 This is a schematic diagram of the bending performance test of the present invention. Detailed Implementation
[0021] It is readily understood that, based on the technical solution of this invention, those skilled in the art can propose various interchangeable implementations without altering the essential spirit of the invention. Therefore, the following specific embodiments are merely illustrative examples of the technical solution of this invention and should not be considered as the entirety of the invention or as limitations or restrictions on the technical solution of this invention.
[0022] This invention provides a heat treatment method for aluminum alloy conductive busbars, specifically including the following steps:
[0023] S1: The raw materials are prepared according to the target chemical composition. After melting, refining and pre-furnace testing, Al-Ti-B is used for online grain refinement during the casting process. After casting, post-furnace testing and low-magnification microstructure inspection are carried out to obtain aluminum alloy ingots.
[0024] S2: Hot extrusion of aluminum alloy ingots to obtain aluminum alloy conductive busbars. Online solution treatment of the hot-extruded aluminum alloy conductive busbars. The solution temperature of the aluminum alloy conductive busbars in the online solution treatment is 520℃. After the online solution treatment is completed, rapid cooling is performed so that the discharge temperature of the rapidly cooled aluminum alloy conductive busbars does not exceed 100℃.
[0025] S3: Select the corresponding artificial aging temperature and artificial aging time according to the nominal thickness of the aluminum alloy conductive busbar, and conduct physical and chemical tests after artificial aging.
[0026] In some specific embodiments, step S1 includes the following technical features:
[0027] By mass percentage, the chemical composition of the aluminum alloy is controlled as follows: Mg 0.60%-0.65%, Si 0.40%-0.45%, Fe≤0.15%, Cu≤0.05%, Mn≤0.03%, Cr≤0.03%, Zn≤0.05%, Ti≤0.01%, B 0.03%-0.05%, with the balance being Al.
[0028] Mg and Si are the main heat treatment strengthening elements in Al-Mg-Si aluminum alloys. When the Mg and Si contents are too low, the number of strengthening components that can participate in subsequent solid solution and aging precipitation is reduced, which is not conducive to obtaining a strengthened state that meets the mechanical load-bearing requirements of conductive busbars. When the Mg and Si contents continue to increase, the number of solute atoms dissolved in the Al matrix increases, which enhances the scattering effect on conduction electrons and increases the difficulty of coordinating the material's strength, conductivity and bending performance. Therefore, the Mg content is controlled at 0.60%-0.65% and the Si content is controlled at 0.40%-0.45%.
[0029] The Fe content is controlled to be no higher than 0.15%. When the Fe content increases, the number of Fe-Si-Al type second phases in the aluminum alloy structure increases. The coarser second phases will cause local deformation incoordination in the Al matrix during plastic deformation. When the conductive busbar is bent at 90°, the outer arc area of the bend is in a state of tensile deformation. A high Fe content will increase the tendency for local cracks to form in this area. Therefore, the plasticity and bending performance of the aluminum alloy conductive busbar are maintained by limiting the Fe content.
[0030] The Ti content is controlled to be no higher than 0.01%, the Mn and Cr contents are both controlled to be no higher than 0.03%, and the B content is controlled to be 0.03%-0.05%. When trace elements such as Ti, Mn, and Cr exist in solid solution in the Al matrix, they will have an adverse effect on electronic conduction. By controlling the contents of Ti, Mn, Cr, and B together, the adverse effects of these trace elements on the electrical conductivity of aluminum alloys can be reduced.
[0031] After the raw materials are batched according to the target chemical composition, they are added to the melting equipment for melting, ensuring complete melting and forming a homogeneous aluminum alloy melt. After melting, the aluminum alloy melt is refined, degassed, deslag-removed, and filtered to reduce gas and non-metallic inclusions, improving the purity of the melt entering the casting process. Production research shows that effective refining can improve the electrical conductivity of 6101 aluminum alloy by approximately 0.2%-0.3% IACS. Therefore, for aluminum alloy conductive busbars with high conductivity requirements, the quality of the preceding melt will affect the final conductivity.
[0032] After refining, samples are taken before the furnace and chemical composition is analyzed. Mg, Si, Fe, Cu, Mn, Cr, Zn and Ti are detected by X-ray fluorescence spectroscopy, and B content is detected by corresponding chemical analysis methods. When the content of each element meets the above chemical composition control range, the aluminum alloy melt enters the grain refinement and casting process.
[0033] Al-Ti-B grain refiner is added to the molten aluminum during the casting process to refine the grains online. The grain refinement process is controlled by ensuring that the Ti content in the final aluminum alloy is no higher than 0.01% and the low-magnification grain size of the ingot is no greater than grade II. The molten aluminum after online grain refinement is then cast. After casting, post-furnace analysis and low-magnification microstructure inspection are performed to confirm that the chemical composition meets the above control range, the low-magnification grain size of the ingot is no greater than grade II, and there are no obvious cracks, severe porosity, or large inclusions that would affect subsequent hot extrusion. The ingot can then proceed to the hot extrusion process. For ingots that require improvement in as-cast segregation and as-cast second-phase distribution, homogenization treatment can be performed before hot extrusion.
[0034] In some specific embodiments, step S2 includes the following technical features:
[0035] The qualified aluminum alloy ingots are hot-extruded to form aluminum alloy conductive busbars. The conventional width of the aluminum alloy conductive busbars is 20-400mm and the thickness is 2-20mm.
[0036] During hot extrusion, aluminum alloys undergo plastic deformation, which increases crystal defects such as dislocations, vacancies, and lattice distortions within the material and enhances the scattering of conduction electrons. Production studies show that when the processing rate is 92.5%, the conductivity decreases by about 0.4% IACS, and when the processing rate is increased to 95.98%, the conductivity decreases by about 1% IACS. Therefore, there is a continuous influence between the material state formed by hot extrusion and the subsequent online solution treatment and artificial aging processes.
[0037] After hot extrusion, the aluminum alloy conductive busbar is subjected to online solution treatment. The 520℃ is the material temperature control value reached by the aluminum alloy conductive busbar in the online solution treatment section. Under this temperature condition, Mg-Si related components enter the Al matrix, establishing a solution basis for subsequent rapid cooling and artificial aging.
[0038] After the online solution treatment is completed, rapid cooling is performed to cool the aluminum alloy conductive busbar to a discharge temperature not exceeding 100°C. The rapid cooling referred to in this application means a continuous cooling process performed after the 520°C online solution treatment, ensuring that the Mg-Si related components remain in a supersaturated solution state before entering the artificial aging process. Specific cooling equipment and cooling media can be selected according to the configuration of the continuous production line to meet the requirements of continuous cooling and the aforementioned discharge temperature control.
[0039] In some specific embodiments, step S3 uses the nominal thickness of the aluminum alloy conductive busbar as the grading parameter for the artificial aging regime. The cross-sectional temperature response and subsequent microstructure adjustment differ for busbars with different nominal thicknesses; specifically, the following discrete temperature-time combinations are used:
[0040] When the nominal thickness of the aluminum alloy conductive busbar is 3.20-10.00mm, the artificial aging process shall be one of the following: 200℃×7h, 210℃×7h, 225℃×3h, or 280℃×6h.
[0041] When the nominal thickness of the aluminum alloy conductive busbar is 10.01-12.50mm, the artificial aging process shall be one of 200℃×8h, 210℃×8h, 225℃×3h or 280℃×6h.
[0042] When the nominal thickness of the aluminum alloy conductive busbar is 12.51-20.00mm, the artificial aging process adopts one of the following: 210℃×9h, 225℃×4h, 225℃×4.5h, or 280℃×6h. For thicker materials, the heat treatment process also includes a treatment regime of 225℃×4.5h or 280℃×7h for materials with a thickness of 20.01-25.00mm, and 225℃×5h for materials with a thickness of 25.01-40.00mm.
[0043] During artificial aging, the Mg-Si components dissolved in the Al matrix gradually transform from a supersaturated solid solution state to a precipitated state. On the one hand, the precipitation strengthens the material; on the other hand, as Mg and Si transform from the solid solution state in the Al matrix to the second phase, the concentration of solid solution elements in the matrix decreases, the scattering effect on conduction electrons weakens, and the conductivity recovers accordingly. Therefore, the artificial aging process needs to consider the conductivity, tensile strength, and bending performance of the aluminum alloy conductive busbar simultaneously.
[0044] The aforementioned artificial aging regimes of 200℃, 210℃, 225℃, and 280℃ constitute specific heat treatment combinations corresponding to the corresponding nominal thicknesses. Each artificial aging temperature and artificial aging time is implemented in pairs according to the corresponding combinations, and different artificial aging temperatures and artificial aging times are not separated and arbitrarily combined. Among them, 225℃×4h and 225℃×4.5h are two independent optional aging regimes for the 12.51-20.00mm thickness range.
[0045] The following will explain the solution of the present invention with reference to the embodiments. It should be noted that the embodiments are only used to illustrate the present invention and should not be regarded as limiting the scope of the present invention. Unless otherwise specified, the instruments used in the embodiments are all conventional products that can be obtained commercially.
[0046] Example 1
[0047] This embodiment provides a heat treatment method for aluminum alloy conductive busbars, specifically including the following steps:
[0048] S1: Melting and Composition Control
[0049] The ingredients are prepared according to the following chemical composition: Mg 0.60%-0.65%, Si 0.40%-0.45%, Fe≤0.15%, Cu≤0.05%, Mn≤0.03%, Cr≤0.03%, Zn≤0.05%, Ti≤0.01%, B 0.03%-0.05%, with the balance being Al.
[0050] The prepared furnace charge is added to the smelting equipment for melting. After the furnace charge is completely melted, it is refined, degassed, slag removed and filtered. After refining, samples are taken in front of the furnace to test the chemical composition of Mg, Si, Fe, Cu, Mn, Cr, Zn, Ti and B. If the test results meet the above target composition range, it enters the casting process.
[0051] Al-Ti-B grain refiner is added to the molten aluminum during the casting process to refine the grains online, controlling the Ti content in the final aluminum alloy to be no higher than 0.01%. The grain-refined molten aluminum is then cast to obtain an aluminum alloy ingot.
[0052] After casting, post-furnace analysis and low-magnification microstructure inspection were carried out. The grain size of the ingot was grade II under low-magnification microstructure. No obvious cracks, severe porosity or large inclusions that would affect subsequent hot extrusion were observed.
[0053] S2: Hot extrusion and online solution treatment
[0054] The qualified aluminum alloy ingots were hot-extruded to obtain aluminum alloy conductive busbars with rectangular cross sections; Examples 1-3 used the same width specifications and the nominal thickness was 12.0 mm.
[0055] The hot-extruded aluminum alloy conductive busbar is subjected to online solution treatment, so that the material temperature of the aluminum alloy conductive busbar in the online solution treatment section reaches 520℃; after the online solution treatment is completed, it is immediately rapidly cooled so that the discharge temperature of the rapidly cooled aluminum alloy conductive busbar does not exceed 100℃.
[0056] S3: Artificial aging
[0057] The rapidly cooled aluminum alloy conductive busbar was subjected to artificial aging treatment at a temperature of 225°C for 3 hours. After artificial aging, it was cooled to room temperature to obtain the aluminum alloy conductive busbar of Example 1.
[0058] Example 2
[0059] This embodiment provides a heat treatment method for aluminum alloy conductive busbars, which differs from Embodiment 1 in that:
[0060] During the artificial aging stage, the artificial aging temperature is adjusted to 200℃ and the artificial aging time is adjusted to 8 hours.
[0061] Example 3
[0062] This embodiment provides a heat treatment method for aluminum alloy conductive busbars, which differs from Embodiment 1 in that:
[0063] During the artificial aging stage, the artificial aging temperature is adjusted to 280℃ and the artificial aging time is adjusted to 6 hours.
[0064] Comparative Example 1
[0065] This comparative example provides a heat treatment method for aluminum alloy conductive busbars, which differs from Example 1 in that:
[0066] The Fe content was adjusted to 0.25% during the ingredient preparation process.
[0067] Comparative Example 2
[0068] This comparative example provides a heat treatment method for aluminum alloy conductive busbars, which differs from Example 1 in that:
[0069] The artificial aging temperature remains constant at 225℃, and the artificial aging time is extended from 3 hours to 8 hours.
[0070] The aluminum alloy conductive busbars prepared in Examples 1-3 and Comparative Examples 1-2 were sampled and subjected to performance tests. The specific test details are as follows:
[0071] The contents of Mg, Si, Fe, Cu, Mn, Cr, Zn, and Ti were determined by X-ray fluorescence spectrometry, following the method specified in YS / T806-2020 "Chemical Analysis Methods for Aluminum and Aluminum Alloys - Determination of Elemental Content - X-ray Fluorescence Spectrometry". The boron (B) content was determined according to GB / T20975.15-2020 "Chemical Analysis Methods for Aluminum and Aluminum Alloys - Part 15: Determination of Boron Content". The results are shown in Table 1.
[0072] Table 1
[0073] Group Mg / % Si / % Fe / % Cu / % Mn / % Cr / % Zn / % Ti / % B / % Example 1 0.63 0.43 0.12 0.03 0.01 0.02 0.02 0.008 0.04 Example 2 0.63 0.43 0.12 0.03 0.01 0.02 0.02 0.008 0.04 Example 3 0.63 0.43 0.12 0.03 0.01 0.02 0.02 0.008 0.04 Comparative Example 1 0.63 0.43 0.25 0.03 0.01 0.02 0.02 0.008 0.04 Comparative Example 2 0.63 0.43 0.12 0.03 0.01 0.02 0.02 0.008 0.04
[0074] Examples 1-3 and Comparative Example 2 use the same chemical composition system, and the content of each element is within the range specified in this invention. In Comparative Example 1, the Fe content is increased to 0.25%, while the content of the other elements remains the same as in Example 1. Therefore, the performance difference between Example 1 and Comparative Example 1 mainly reflects the influence of the change in Fe content on the performance of the aluminum alloy conductive busbar.
[0075] The conductivity of aluminum alloy conductive busbars at 20℃ was tested according to GB / T 12966-2022 "Eddy Current Test Method for Conductivity of Aluminum and Aluminum Alloys". Three busbar samples were randomly selected from each group, and five measurement positions were selected for each sample. The average value of each sample was calculated first, and then the average value of each group was calculated. Tensile specimens were prepared according to GB / T 16865-2023, with the longitudinal axis of the specimen along the extrusion direction of the busbar. Tensile tests were conducted at room temperature according to GB / T 228.1-2021 "Metallic Materials - Tensile Testing - Part 1: Test Method at Room Temperature" to determine the tensile strength and elongation after fracture. Three parallel specimens were tested in each group. The results are shown in Table 2.
[0076] Table 2
[0077] Group Conductivity at 20℃ / %IACS Tensile strength / MPa Elongation after fracture / % Example 1 59.22±0.05 171±2 12.4±0.3 Example 2 58.63±0.04 184±3 10.6±0.2 Example 3 60.18±0.05 146±2 14.5±0.3 Comparative Example 1 59.02±0.06 166±3 8.7±0.4 Comparative Example 2 59.85±0.06 136±2 15.0±0.3
[0078] The conductivity of the aluminum alloy conductive busbars in each embodiment at 20℃ was 58.63%-60.18% IACS, and the tensile strength was 146-184 MPa, all meeting the control requirements of conductivity not less than 58% IACS and tensile strength not less than 140 MPa at 20℃. Among them, Example 2, which used artificial aging at 200℃ for 8 hours, had a tensile strength of 184 MPa, which was relatively high among the embodiments. Example 3, which used artificial aging at 280℃ for 6 hours, had a conductivity of 60.18% IACS, which was also relatively high among the embodiments. Example 1, which used artificial aging at 225℃ for 3 hours, had a conductivity of 59.22% IACS at 20℃, a tensile strength of 171 MPa, and an elongation after fracture of 12%. The Fe content was 0.4%, and the electrical conductivity, tensile strength, and plasticity remained in harmony. In Comparative Example 1, after increasing the Fe content to 0.25%, the electrical conductivity at 20°C was 59.02% IACS, which was relatively similar to that of Example 1, while the elongation after fracture decreased to 8.7%, indicating that the increase in Fe content mainly affected the continuous plastic deformation ability of the material. In Comparative Example 2, after extending the artificial aging time at 225°C to 8 hours, the electrical conductivity at 20°C increased to 59.85% IACS, while the tensile strength decreased to 136 MPa. This indicates that increasing the degree of aging is beneficial for the further precipitation of solid solution elements in the Al matrix and the recovery of electrical conductivity, but it will change the strengthening state of the material. The artificial aging process needs to take into account both electrical conductivity and mechanical properties.
[0079] Bending performance tests were conducted on Examples 1-3 and Comparative Examples 1-2 according to GB / T 232-2024 "Metallic Materials - Bending Test Method". The bending specimens were prepared along the extrusion direction of the busbar, with a specimen length of 180±0.3 mm, a width of 15±0.2 mm, and R7.5 arcs at both ends. The bending radius was 15 mm, and the bending angle was 90°. Five independent specimens were tested in each group. After bending, penetrant testing was performed on the outer arc area of the bend according to GB / T 18851.1-2024 "Non-destructive Testing - Penetrant Testing - Part 1: General Rules". The results are shown in Table 3.
[0080] Table 3
[0081] Group Number of bending samples / piece No visible cracks / piece Penetrant testing without linear crack indicator / part Overall Results Example 1 5 5 5 5 / 5 passed Example 2 5 5 5 5 / 5 passed Example 3 5 5 5 5 / 5 passed Comparative Example 1 5 3 3 3 / 5 passed Comparative Example 2 5 5 5 5 / 5 passed
[0082] In Examples 1-3, none of the five bending samples showed surface cracking after being bent at 90° along the extrusion direction (R15mm), and no continuous linear crack indications were found in the penetrant test. In Comparative Example 1, only three of the five samples passed both the bending and penetrant tests. Combined with the result that the elongation after fracture decreased to 8.7%, it indicates that the continuous plastic deformation capacity of the material decreased after the Fe content was increased, and cracks were more likely to occur in the tensile region of the outer arc of the bend. In Comparative Example 2, all five samples passed both the bending and penetrant tests, but their tensile strength had decreased to 136 MPa, indicating that the main performance limitation under this treatment was the reduction in tensile strength, rather than bending cracking.
[0083] According to GB / T 3246.2-2012 "Methods for Inspection of Microstructure of Wrought Aluminum and Aluminum Alloy Products Part 2: Low Magnification Microstructure Inspection Method", the ingots corresponding to Examples 1-3 and Comparative Examples 1-2 were subjected to low magnification microstructure inspection. The low magnification grain size and macroscopic microstructure defects were recorded. The results are shown in Table 4.
[0084] Table 4
[0085] Group Low grain size Obvious cracks Severely loose Large-size inclusions Example 1 Level 2 none none none Example 2 Level 2 none none none Example 3 Level 2 none none none Comparative Example 1 Level 2 none none none Comparative Example 2 Level 2 none none none
[0086] The low-magnification grain size of the ingots in all embodiments and comparative examples was grade II, and no obvious cracks, severe porosity, or large-sized inclusions were found, indicating that each group had a similar pre-casting microstructure. The performance differences between the embodiments and comparative examples were not caused by obvious casting macroscopic defects.
[0087] The technical scope of this invention is not limited to the content described above. Those skilled in the art can make various modifications and variations to the above embodiments without departing from the technical concept of this invention, and all such modifications and variations should fall within the protection scope of this invention.
Claims
1. An aluminum alloy conductive busbar, characterized in that, The aluminum alloy comprises, by mass percentage, 0.60%-0.65% Mg, 0.40%-0.45% Si, ≤0.15% Fe, ≤0.05% Cu, ≤0.03% Mn, ≤0.03% Cr, ≤0.05% Zn, ≤0.01% Ti, 0.03%-0.05% B, with the balance being Al.
2. The aluminum alloy conductive busbar according to claim 1, characterized in that, The width of the aluminum alloy conductive busbar is 20-400mm and the thickness is 2-20mm.
3. The aluminum alloy conductive busbar according to claim 1, characterized in that, The conductivity of the aluminum alloy conductive busbar at 20°C is not less than 58% IACS.
4. The aluminum alloy conductive busbar according to claim 1, characterized in that, The tensile strength of the aluminum alloy conductive busbar is not less than 140 MPa.
5. The aluminum alloy conductive busbar according to claim 1, characterized in that, The bending radius of the aluminum alloy conductive busbar when it is bent at 90° along the extrusion direction is 15mm, and there are no cracks on the surface of the bending area.
6. A heat treatment method for an aluminum alloy conductive busbar, characterized in that, The aluminum alloy conductive busbar comprises, by mass percentage, Mg 0.60%-0.65%, Si 0.40%-0.45%, Fe≤0.15%, Cu≤0.05%, Mn≤0.03%, Cr≤0.03%, Zn≤0.05%, Ti≤0.01%, B 0.03%-0.05%, with the balance being Al. The nominal thickness of the aluminum alloy conductive busbar is 3.20-20.00 mm. The aluminum alloy conductive busbar formed by hot extrusion is subjected to online solution treatment. The solution temperature of the aluminum alloy conductive busbar in the online solution treatment is 520°C. After the online solution treatment, it is rapidly cooled so that the discharge temperature of the rapidly cooled aluminum alloy conductive busbar does not exceed 100°C, and then artificial aging treatment is performed. The artificial aging treatment adopts one of the following treatment systems according to the nominal thickness of the aluminum alloy conductive busbar: When the nominal thickness is 3.20-10.00mm, it is artificially aged at 200℃ for 7 hours, at 210℃ for 7 hours, at 225℃ for 3 hours, or at 280℃ for 6 hours. When the nominal thickness is 10.01-12.50mm, it shall be artificially aged at 200℃ for 8 hours, at 210℃ for 8 hours, at 225℃ for 3 hours, or at 280℃ for 6 hours. When the nominal thickness is 12.51-20.00mm, it is artificially aged at 210℃ for 9 hours, at 225℃ for 4 hours, at 225℃ for 4.5 hours, or at 280℃ for 6 hours.
7. The heat treatment method according to claim 6, characterized in that, When the nominal thickness of the aluminum alloy conductive busbar is 3.20-10.00mm, it shall be artificially aged at 200℃ for 7 hours; when the nominal thickness is 10.01-12.50mm, it shall be artificially aged at 200℃ for 8 hours.
8. The heat treatment method according to claim 6, characterized in that, When the nominal thickness of the aluminum alloy conductive busbar is 3.20-12.50mm, it shall be artificially aged at 225℃ for 3 hours; when the nominal thickness is 12.51-20.00mm, it shall be artificially aged at 225℃ for 4 hours or 4.5 hours.
9. The heat treatment method according to claim 6, characterized in that, When the nominal thickness of the aluminum alloy conductive busbar is 3.20-10.00mm, it shall be artificially aged at 210℃ for 7 hours; when the nominal thickness is 10.01-12.50mm, it shall be artificially aged at 210℃ for 8 hours; when the nominal thickness is 12.51-20.00mm, it shall be artificially aged at 210℃ for 9 hours.
10. The heat treatment method according to claim 6, characterized in that, When the nominal thickness of the aluminum alloy conductive busbar is 3.20-20.00mm, it is artificially aged at 280℃ for 6 hours.