A process for improving the microstructure and properties of H-beams for railway vehicles by refining grain size.
By combining stepwise deoxidation composite alloying and LF refining inclusion control with a two-stage controlled rolling and cooling process, the grain size of Q460 grade H-beams is refined, solving the problems of coarse grains and insufficient low-temperature toughness in existing technologies, and realizing the production of high-performance railway vehicle H-beams.
Patent Information
- Application Number
- CN202611402073.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-10
- Publication Date
- 2026-11-17
AI Technical Summary
The existing Q460 grade H-beams have coarse grains, poor uniformity of microstructure in the thickness direction, insufficient low-temperature toughness, and severe embrittlement of welded joints, making it difficult to meet the high-performance requirements of heavy-load and high-speed railway vehicles.
By employing stepwise deoxidation composite alloying, LF refining inclusion control, and two-stage controlled rolling and cooling processes, acicular ferrite nucleation is induced by the generation of dispersed composite inclusions, and the grain size is refined and the microstructure is optimized by combining the segmented controlled cooling process.
The method achieved a stable grain size of H-beams of grade 10.5 or higher, an IAF volume fraction of ≥45%, a banded structure of ≤0.5 grade, a yield strength of ≥480MPa, a tensile strength of ≥610MPa, a transverse impact energy of ≥120J at -40℃, and an impact energy of ≥80J in the heat-affected zone at -40℃ after welding with a high heat input of 100kJ/cm, significantly improving strength, toughness and weldability.
Abstract
Description
Technical Field
[0001] This invention belongs to the field of iron and steel metallurgy and controlled rolling and cooling technology, and particularly relates to a process for improving the microstructure and properties of H-beams for railway vehicles by refining grain size. Background Technology
[0002] With the development of my country's railway freight towards heavy-haul and passenger transport towards high-speed, the requirements for the strength, low-temperature toughness, fatigue resistance, and welding efficiency of H-beams in railway vehicle body structures are becoming increasingly stringent. Q460 grade high-strength H-beams are the core load-bearing material of railway vehicle bodies, and their microstructure and properties directly determine the operational safety and service life of the entire vehicle.
[0003] Currently, conventional Q460 grade H-beams are mostly produced using traditional microalloying + controlled rolling and controlled cooling processes, which generally suffer from the following technical shortcomings: First, the finished product has coarse grains, typically with a grain size of only 7.5~8.5, and poor uniformity of microstructure in the thickness direction, with severe banded microstructure in the core, resulting in insufficient low-temperature toughness, large fluctuations in transverse impact energy at -40℃, and a low pass rate, making it difficult to meet the service requirements of the frigid northern regions; Second, during high heat input welding, the grains in the heat-affected zone grow rapidly, exhibiting obvious embrittlement, and the impact energy of the welded joint decreases by more than 50%, limiting the improvement of welding construction efficiency; Third, the strengthening method of simply refining austenite grains has reached its bottleneck, making it difficult to achieve simultaneous improvement in strength and toughness, and failing to meet the lightweight and long-life design requirements of the new generation of railway vehicles.
[0004] Oxide metallurgy, by introducing beneficial non-metallic inclusions into steel to induce intragranular acicular ferrite (IAF) nucleation, and relying on the interpenetrating and segmenting effect of acicular ferrite to significantly refine the microstructure, is an effective way to simultaneously improve the strength and toughness of steel and its high heat input welding performance. Existing research shows that Al-Ti-O composite inclusions can effectively induce IAF nucleation, but current processes lack sufficient precision in controlling the composition, size, and distribution of inclusions. The proportion of inclusions with beneficial sizes (1~6μm) is low, and large-sized harmful inclusions cannot be effectively removed. Furthermore, the focus is only on inclusion design during the smelting stage, without coordination with rolling and cooling processes, resulting in low IAF nucleation rates and limited microstructure refinement effects, making stable application in the mass production of H-beams difficult. Therefore, developing a grain refinement process that precisely controls inclusions and coordinates with the rolling process is crucial for improving the overall performance of H-beams used in railway vehicles. Summary of the Invention
[0005] The purpose of this invention is to provide a process for improving the microstructure and properties of H-beams for railway vehicles by refining grain size. Q460 grade H-beams for railway vehicles prepared using this process exhibit a stable grain size of ≥10.5, an IAF volume fraction ≥45%, and a banded microstructure ≤0.5. The yield strength is ≥480MPa, tensile strength ≥610MPa, elongation after fracture ≥22%, and transverse V-notch impact energy at -40℃ ≥120J. The impact energy of the heat-affected zone after welding with a high heat input of 100kJ / cm at -40℃ is ≥80J, significantly improving the strength-toughness ratio and weldability. This process can be implemented using conventional steel smelting and rolling production lines without requiring additional specialized equipment. It offers strong stability in mass production and can be widely applied to the load-bearing structures of railway freight and passenger car bodies, greatly improving the service life and operational safety of components.
[0006] To solve the above-mentioned technical problems, the present invention adopts the following technical solution:
[0007] This invention discloses a process for improving the microstructure and properties of H-beams for railway vehicles by refining grain size. The process comprises six main steps: smelting composition design, converter-based stepwise deoxidation and alloying, LF refining and inclusion control, continuous casting, heating and two-stage controlled rolling, and post-rolling segmented cooling. Specific parameters for each step are as follows:
[0008] Step 1: Smelting Composition Design
[0009] Based on Q460 grade railway vehicle H-beams, the alloy element matching was optimized, and the chemical composition by mass fraction was as follows: C 0.06~0.10%, Si 0.20~0.40%, Mn 1.20~1.50%, P≤0.015%, S 0.005~0.012%, Alt 0.020~0.040%, Ti 0.012~0.025%, Nb 0.020~0.040%, V 0.030~0.060%, Ca 0.0010~0.0020%, with the balance being Fe and unavoidable impurities;
[0010] Composition design concept: Low carbon ensures toughness and weldability; Mn solid solution strengthening and S-based MnS formation; Ti and Al synergistically form composite oxide inclusions; Nb and V microalloying refines grains and provides additional strengthening; trace amounts of Ca modify the morphology of inclusions.
[0011] Step 2: Converter smelting and step-by-step deoxidation and alloying
[0012] Converter endpoint control: endpoint carbon mass fraction ≥ 0.05%, endpoint phosphorus ≤ 0.012%, tapping temperature 1620~1650℃, slag-blocking tapping adopted, slag discharge ≤ 5kg / t steel.
[0013] Stepwise deoxidation feeding sequence:
[0014] When the steel has been tapped to 1 / 3 of its original volume, aluminum blocks (or aluminum-manganese ferrooxide) are added for pre-deoxidation, with the amount of aluminum added being 60-70% of the total aluminum content.
[0015] When the steel is tapped to 1 / 2 capacity, ferrosilicon and ferromanganese are added sequentially for main alloying, and the Si and Mn are adjusted to the target range. At the same time, ferrotitanium and 30-40% of the total aluminum are added for composite deoxidation, and the Ti recovery rate is controlled at 60-70%.
[0016] Lime and refined pre-melted slag are added at the end of the steelmaking process to form slag and desulfurize it.
[0017] Step 3: Precise Control of Inclusions in LF Refining
[0018] Slag heating: After the ladle is put into the LF furnace, the furnace is heated by electricity to heat the slag. Lime is added to adjust the slag composition and control the slag to be CaO-SiO2-Al2O3 system with a binary basicity of 3.5~4.5 and a total mass fraction of FeO+MnO in the slag ≤0.5% to ensure a strong reducing atmosphere.
[0019] Composition fine-tuning: Based on the spectral analysis results, fine-tune elements such as C, Si, Mn, and Ti to the target range; if the S content is lower than the lower limit, add a small amount of FeS to adjust the S to 0.005~0.012% to ensure the formation of MnS composite inclusions.
[0020] Soft blowing argon purification: After the composition is qualified, adjust the argon flow rate to 80~120L / min and perform soft blowing argon treatment for 15~20min; the soft blowing process ensures that the steel liquid surface is slightly surging and not exposed, promotes the full floating of large inclusions, and at the same time retains small and dispersed beneficial composite inclusions.
[0021] Trace calcium treatment: 3-5 minutes before the end of soft blowing, feed in calcium-iron wire to control the Ca mass fraction in the steel at 0.0010-0.0020% to modify Al2O3 inclusions and avoid the formation of large clusters of inclusions.
[0022] Step 4: Continuous casting of irregularly shaped billets
[0023] Special H-beam billets are produced using a shaped billet continuous casting machine. The temperature of the molten steel in the tundish is controlled at 1530~1550℃, and the casting speed is 0.8~1.2m / min. Electromagnetic stirring in the crystallizer and electromagnetic stirring at the end are used to ensure uniform billet structure.
[0024] Full-process protective casting: long nozzle argon sealing and immersion nozzle protection to avoid secondary oxidation of molten steel and ensure the stability of inclusion composition and size.
[0025] After the billet is removed from the production line, it should be cooled for ≥48 hours to eliminate internal casting stress, promote hydrogen diffusion, and avoid white spot defects.
[0026] Step 5: Heating and Two-Stage Controlled Rolling
[0027] The billet is fed into a walking beam furnace for heating at a temperature of 1200~1250℃ and held for 2~3 hours to ensure austenite homogenization and full solid solution of alloying elements such as Nb and V, while avoiding the high-temperature growth of TiN inclusions.
[0028] The first stage is recrystallization zone rolling. The initial rolling temperature is 1100~1150℃. High reduction rolling is adopted, with a cumulative reduction rate of ≥60% and a single-pass reduction rate of ≥15%. Through repeated recrystallization, the original austenite grains are fully broken and the austenite size is refined.
[0029] Roller cooling: After rolling to the intermediate thickness, the roller is air-cooled and allowed to warm up. The roller insulation cover is turned on to reduce the temperature drop at the edges and ensure uniform cross-sectional temperature. When the steel temperature drops to 850~900℃, the second stage of rolling begins.
[0030] The second stage: rolling in the non-recrystallization zone with a cumulative reduction of ≥50% and a final rolling temperature controlled at 780~820℃; high-density deformation bands and dislocations are introduced through large deformation to increase IAF nucleation sites, while flattening austenite grains to provide a foundation for subsequent phase transformation refinement.
[0031] Step 6: Post-rolling segmented controlled cooling
[0032] A three-stage cooling process is adopted to precisely control the phase change process:
[0033] The first stage of rapid cooling: immediately after rolling, the grains enter an ultra-fast cooling device and are rapidly cooled to 680-720°C at a cooling rate of 15-20°C / s. This inhibits austenite grain growth and promotes the nucleation of ferrite within the grains and at grain boundaries.
[0034] The second stage of air cooling and heat preservation: after ultra-fast cooling, air cooling for 30~60s allows IAF to grow fully, and the grains are divided by the interpenetration of needle-like ferrite, while ensuring that the ferrite phase transformation is complete.
[0035] The third stage of controlled cooling: then cooling at a rate of 5~10℃ / s to 550~600℃, and finally air cooling to room temperature; controlling the pearlite transformation, avoiding pearlite growth and banded distribution, and ensuring uniform and fine tissue.
[0036] Furthermore, the chemical composition of the H-beam is as follows (mass fraction): C 0.08%, Si 0.30%, Mn 1.35%, P 0.012%, S 0.008%, Alt 0.030%, Ti 0.018%, Nb 0.030%, V 0.045%, Ca 0.0015%, with the balance being Fe and impurities.
[0037] Furthermore, the chemical composition of the H-beam is as follows (mass fraction): C 0.06%, Si 0.20%, Mn 1.20%, P 0.012%, S 0.005%, Alt 0.030%, Ti 0.012%, Nb 0.020%, V 0.045%, Ca 0.0015%, with the balance being Fe and impurities.
[0038] Furthermore, the chemical composition of the H-beam is as follows (mass fraction): C 0.10%, Si 0.40%, Mn 1.50%, P 0.012%, S 0.012%, Alt 0.030%, Ti 0.025%, Nb 0.040%, V 0.045%, Ca 0.0015%, with the balance being Fe and impurities.
[0039] Furthermore, specifically:
[0040] The converter tapping temperature is 1635℃, and the deoxidation is carried out in stages: 65% aluminum is added before tapping, and ferrotitanium is added at 1 / 2 of the tapping time.
[0041] LF refining: basicity 4.0, soft argon blowing 100L / min for 18min, Ca content controlled at 0.0015%;
[0042] Continuous casting: Tundish temperature 1540℃, casting speed 1.0m / min;
[0043] Rolling: Heating temperature 1220℃, first stage rolling 1120℃, cumulative reduction 65%; second stage rolling 880℃, cumulative reduction 55%, final rolling temperature 800℃;
[0044] Cooling: First stage cooling rate 18℃ / s, final temperature 700℃; air cooling 45s; Second stage cooling rate 8℃ / s, final temperature 580℃, air cooling to room temperature.
[0045] Further process parameters: heating temperature 1200℃, two-stage initial rolling 850℃, final rolling 780℃; first-stage cooling rate 15℃ / s.
[0046] Further process parameters: heating temperature 1250℃, two-stage initial rolling 900℃, final rolling 820℃; first-stage cooling rate 20℃ / s.
[0047] Overall technical approach:
[0048] This invention adopts "oxide metallurgy-induced IAF nucleation + controlled rolling and cooling synergistic refinement" as its core technical concept, constructing a full-process microstructure control system from smelting to rolling. First, through a stepwise deoxidation composite alloying process, the composition and size of inclusions in the steel are precisely controlled to generate a large number of 1~5μm Al2O3-Ti2O3-MnS dispersed composite inclusions, which serve as efficient nucleation cores for IAF. Then, through LF refining soft blowing argon and trace calcium treatment, large-sized harmful inclusions are removed, ensuring that beneficial inclusions are uniformly dispersed. Subsequently, a two-stage controlled rolling process is adopted, with high pressure applied in the non-recrystallization zone to introduce high-density deformation bands and dislocations, providing more nucleation sites for IAF. Finally, through a segmented controlled cooling process, the phase transformation temperature and cooling rate are controlled to promote the nucleation and growth of a large number of IAFs within the austenite grains. The interpenetration of acicular ferrite divides the grains, while the morphology and distribution of pearlite are optimized, ultimately achieving ultra-fine microstructure and comprehensive performance improvement.
[0049] Core innovations:
[0050] 1. Stepwise Deoxidation Composite Alloying Process: This process abandons the traditional one-time deoxidation alloying method and adopts a stepwise feeding sequence of "aluminum pre-deoxidation → silicon-manganese alloying → titanium composite deoxidation": First, aluminum is added to remove most of the oxygen, forming fine Al2O3 cores; then, titanium-iron is added, and Ti reacts with residual oxygen to generate Ti2O3, which then composites with Al2O3; subsequently, Mn and S elements are enriched on the inclusion surface to form a MnS outer layer, ultimately obtaining targeted Al2O3-Ti2O3-MnS composite inclusions. This process can increase the proportion of beneficial composite inclusions with a size of 1~5μm to over 95%, significantly improving IAF induction efficiency.
[0051] 2. LF Refining Inclusion Precision Control Technology: Through optimizing the high-basicity refining slag system, controlling soft blowing argon parameters, and the synergistic effect of trace calcium treatment: High-basicity slag (basicity 3.5~4.5) based on the CaO-SiO2-Al2O3 system is used to ensure a deep desulfurization and reducing atmosphere; 15~20 min of long-term soft blowing argon promotes the full flotation and removal of large-sized (>10μm) inclusions; combined with 0.0010~0.0020% trace calcium treatment, the clustered Al2O3 inclusions are modified into spherical composite inclusions. Ultimately, this achieves the goal of "removing large harmful inclusions and retaining small beneficial inclusions," with the number of beneficial dispersed inclusions in the steel ≥320 / mm. 2 And the distribution is uniform.
[0052] 3. Synergistic process of controlled rolling and cooling with IAF nucleation: Targeting the unique cross-section characteristics of H-beams, a two-stage rolling process is optimized: In the recrystallization zone, a large reduction fully breaks down the original austenite grains; in the non-recrystallization zone, the cumulative reduction rate is ≥50%, introducing a high-density deformation band and increasing the number of non-uniform IAF nucleation sites. This is complemented by a three-stage cooling process: rapid cooling for nucleation, air cooling for growth, and slow cooling for stable microstructure. This precisely controls the phase transformation process, promoting full nucleation and uniform growth of IAF, ultimately forming an ultrafine-grained microstructure with needle-like ferrite interspersed throughout, avoiding the inhomogeneity and banded defects of traditional processes.
[0053] Compared with the prior art, the beneficial technical effects of the present invention are as follows:
[0054] 1. Significantly refined microstructure: The finished H-beams have a stable grain size of 10.5 or higher, which is more than 2 levels finer than the traditional process; the IAF volume fraction is ≥45%, the banded structure is ≤0.5, and the microstructure uniformity is greatly improved, eliminating the performance fluctuations caused by banded structure and mixed crystals from the root.
[0055] 2. Excellent strength and toughness: yield strength ≥480MPa, tensile strength ≥610MPa, elongation after fracture ≥22%, strength indicators far exceeding the requirements of Q460 grade standard; transverse V-shaped impact energy at -40℃ ≥120J, impact energy dispersion ≤8%, low temperature toughness is improved by more than 60% compared with traditional process, fully adapting to the service requirements of railway vehicles in cold regions.
[0056] 3. Outstanding high heat input welding performance: After welding with a heat input of 100kJ / cm, the impact energy of the heat-affected zone at -40℃ is ≥80J, which is more than twice that of traditional processes. The problem of welding embrittlement is effectively solved, which can support the adoption of high-efficiency welding processes in railway vehicle manufacturing and greatly improve production efficiency.
[0057] 4. Strong industrial adaptability: This process relies entirely on a conventional converter-LF refining-continuous casting of special-shaped billets-rolling of section steel production lines, without the need for additional special equipment. It has a wide process parameter window, good stability in batch production, and a steel qualification rate of over 99.5%. The increase in production costs is ≤3%, resulting in a significant cost-performance advantage.
[0058] 5. Significantly extended service life: The refined microstructure improves the fatigue resistance of steel by more than 25%. Combined with excellent low-temperature toughness and weldability, the service life of the vehicle body structure can be extended by more than 30%, and the maintenance cost throughout the entire life cycle is significantly reduced. Detailed Implementation
[0059] Example 1:
[0060] The composition of the test steel (mass fraction, %) is as follows: C 0.08, Si 0.30, Mn 1.35, P 0.012, S 0.008, Alt 0.030, Ti 0.018, Nb 0.030, V 0.045, Ca 0.0015, balance Fe.
[0061] Process parameters:
[0062] The converter tapping temperature is 1635℃, and the deoxidation is carried out in stages: 65% aluminum is added before tapping, and ferrotitanium and the remaining aluminum are added in half of the tapping process.
[0063] LF refining: basicity 4.0, soft argon blowing 100L / min for 18min, Ca content controlled at 0.0015%;
[0064] Continuous casting: Tundish temperature 1540℃, casting speed 1.0m / min;
[0065] Rolling: Heating temperature 1220℃, first stage rolling 1120℃, cumulative reduction 65%; second stage rolling 880℃, cumulative reduction 55%, final rolling temperature 800℃;
[0066] Cooling: First stage cooling rate 18℃ / s, final temperature 700℃; air cooling 45s; Second stage cooling rate 8℃ / s, final temperature 580℃, air cooling to room temperature.
[0067] Finished product specifications: H-beam H500×300×11×18.
[0068] Example 2:
[0069] Composition (mass fraction, %): C 0.06, Si 0.20, Mn 1.20, S 0.005, Ti 0.012, Nb 0.020, the rest are the same as in Example 1.
[0070] Process: Heating temperature 1200℃, two-stage rolling 850℃, final rolling 780℃; first stage cooling rate 15℃ / s, the rest is the same as in Example 1.
[0071] Example 3:
[0072] Composition (mass fraction, %): C 0.10, Si 0.40, Mn 1.50, S 0.012, Ti 0.025, Nb 0.040, the rest are the same as in Example 1.
[0073] Process: Heating temperature 1250℃, two-stage initial rolling 900℃, final rolling 820℃; first stage cooling rate 20℃ / s, the rest is the same as in Example 1.
[0074] Comparative Example 1:
[0075] The traditional Q460H steel production process was adopted: no Ti addition, one-time aluminum deoxidation, conventional LF refining, ordinary two-stage rolling, and air cooling after rolling. Composition (mass fraction, %): C 0.08, Si 0.30, Mn 1.35, Ti none, the rest are similar to Example 1.
[0076] Comparative Example 2:
[0077] Al and Ti were added at once for deoxidation, without stepwise feeding, with a soft blowing time of 10 minutes and conventional rolling and cooling; the Ti content was 0.018%, and the remaining components were the same as in Example 1.
[0078] All samples underwent microstructural observation and mechanical property testing, and the results are shown in the table below:
[0079] Testing items Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Grain size / grade 11.0 10.5 10.5 8.0 9.0 IAF volume fraction / % 48 45 46 0 28 Banded tissue / grade 0.5 0.5 1.0 2.5 1.5 Percentage of beneficial inclusions in the 1~5μm range / % 96.2 95.1 95.7 / 82.3 Yield strength / MPa 495 482 502 425 458 Tensile strength / MPa 625 612 638 570 595 Elongation after fracture / % 24.5 23.0 22.5 21.0 21.5 Transverse impact energy at -40℃ / J (average) 132 121 126 75 92 100kJ / cm welding HAZ-40℃ impact energy / J 88 81 85 36 58 <![CDATA[Fatigue strength (10 7 cycles) / MPa]]> 235 228 232 185 205
[0080] The comparison results show that the process of this invention achieves ultra-fine microstructure by inducing IAF nucleation, improving the grain size by 3 levels compared with the traditional process, and increasing the low-temperature impact energy by more than 75%. The toughness of the heat-affected zone of high heat input welding is increased by 1.4 times, and the fatigue strength is increased by 27%. The overall performance is far superior to the traditional process and the ordinary oxide metallurgical process, and fully meets the high-performance requirements of H-beams for railway vehicles.
[0081] The embodiments described above are merely preferred embodiments of the present invention and are not intended to limit the scope of the present invention. Various modifications and improvements made by those skilled in the art to the technical solutions of the present invention without departing from the spirit of the present invention should fall within the protection scope defined by the claims of the present invention.
Claims
1. A process for improving the microstructure and properties of H-beams for railway vehicles by refining grain size, characterized in that, Specifically, it includes six major steps: smelting composition design, converter step-by-step deoxidation and alloying, LF refining inclusion control, continuous casting, heating and two-stage controlled rolling, and post-rolling segmented cooling. The specific parameters for each process are as follows: Step 1: Smelting Composition Design Based on Q460 grade railway vehicle H-beams, the alloy element matching was optimized, and the chemical composition by mass fraction was as follows: C 0.06~0.10%, Si 0.20~0.40%, Mn 1.20~1.50%, P≤0.015%, S 0.005~0.012%, Alt 0.020~0.040%, Ti 0.012~0.025%, Nb 0.020~0.040%, V 0.030~0.060%, Ca 0.0010~0.0020%, with the balance being Fe and unavoidable impurities; Step 2: Converter smelting and step-by-step deoxidation and alloying Converter endpoint control: endpoint carbon mass fraction ≥ 0.05%, endpoint phosphorus ≤ 0.012%, tapping temperature 1620~1650℃, slag-blocking tapping adopted, slag discharge ≤ 5kg / t steel; Stepwise deoxidation feeding sequence: When the steel has been tapped to 1 / 3 of its capacity, aluminum blocks are added for pre-deoxidation, with the amount of aluminum added being 60-70% of the total aluminum content. When the steel is tapped to 1 / 2, ferrosilicon and ferromanganese are added sequentially for main alloying, and Si and Mn are adjusted to the target range; at the same time, ferrotitanium and 30-40% of the total aluminum are added for composite deoxidation. Lime and refined pre-melted slag are added at the end of the steelmaking process to form slag and desulfurize it. Step 3: Precise Control of Inclusions in LF Refining Slag heating: After the ladle is put into the LF furnace, the power is supplied to heat up the slag, and lime is added to adjust the slag composition. The slag is controlled to be CaO-SiO2-Al2O3 system with a binary basicity of 3.5~4.5 and the total mass fraction of FeO+MnO in the slag is ≤0.5% to ensure a strong reducing atmosphere. Composition fine-tuning: Based on the spectral analysis results, fine-tune the C, Si, Mn, and Ti elements to the target range; if the S content is lower than the lower limit, add a small amount of FeS to adjust the S to 0.005~0.012% to ensure the formation of MnS composite inclusions; Soft blowing argon purification: After the composition is qualified, adjust the argon flow rate to 80~120L / min and perform soft blowing argon treatment for 15~20min; The soft blowing process ensures that the molten steel surface surges slightly and is not exposed, promoting the full floating of large inclusions while retaining small, dispersed, and beneficial composite inclusions. Trace calcium treatment: 3-5 minutes before the end of soft blowing, feed in calcium-iron wire to control the Ca mass fraction in the steel at 0.0010-0.0020% to modify Al2O3 inclusions and avoid the formation of large clusters of inclusions; Step 4: Continuous casting of irregularly shaped billets Special H-beam billets are produced using a shaped billet continuous casting machine. The temperature of the molten steel in the tundish is controlled at 1530~1550℃, and the casting speed is 0.8~1.2m / min. Electromagnetic stirring in the crystallizer and electromagnetic stirring at the end are used to ensure uniform billet structure. Full-process protective casting: long nozzle argon sealing and immersion nozzle protection to avoid secondary oxidation of molten steel and ensure the stability of inclusion composition and size; After the billet is removed from the production line, it should be cooled for ≥48 hours to eliminate casting internal stress, promote hydrogen diffusion, and avoid white spot defects. Step 5: Heating and Two-Stage Controlled Rolling The billet is fed into a walking beam furnace for heating at a temperature of 1200~1250℃ and held for 2~3 hours to ensure austenite homogenization and full solid solution of alloying elements such as Nb and V, while avoiding the high-temperature growth of TiN inclusions. First stage: Rolling in the recrystallization zone, with an initial rolling temperature of 1100~1150℃, using high reduction rolling, with a cumulative reduction rate ≥60% and a single-pass reduction rate ≥15%. Through repeated recrystallization, the original austenite grains are fully broken down, and the austenite size is refined. Roller cooling: After rolling to the intermediate thickness, the roller is air-cooled and allowed to warm up. The roller insulation cover is turned on to reduce the temperature drop at the edges and ensure uniform cross-sectional temperature. When the steel temperature drops to 850~900℃, the second stage of rolling begins. The second stage: rolling in the non-recrystallization zone, with a cumulative reduction rate of ≥50%, and the final rolling temperature controlled at 780~820℃; high-density deformation bands and dislocations are introduced through large deformation to increase IAF nucleation sites, while flattening austenite grains to provide a foundation for subsequent phase transformation refinement. Step 6: Post-rolling segmented controlled cooling A three-stage cooling process is adopted to precisely control the phase change process: The first stage is rapid cooling: immediately after rolling, the grains enter an ultra-rapid cooling device and are rapidly cooled to 680-720°C at a cooling rate of 15-20°C / s. This inhibits austenite grain growth and promotes the nucleation of ferrite within the grains and at grain boundaries. The second stage is air cooling and heat preservation: after ultra-rapid cooling, the grains are air-cooled for 30-60 seconds to allow IAF to grow fully. The grains are divided by the interpenetrating effect of acicular ferrite, while ensuring sufficient ferrite phase transformation. The third stage of controlled cooling: then cooling at a rate of 5~10℃ / s to 550~600℃, and finally air cooling to room temperature; controlling the pearlite transformation, avoiding pearlite growth and banded distribution, and ensuring uniform and fine tissue.
2. The process for improving the microstructure and properties of H-beams for railway vehicles by refining grain size according to claim 1, characterized in that, The chemical composition of the H-beam is as follows (mass fraction): C 0.08%, Si 0.30%, Mn 1.35%, P 0.012%, S 0.008%, Alt 0.030%, Ti 0.018%, Nb 0.030%, V 0.045%, Ca 0.0015%, with the balance being Fe and impurities.
3. The process for improving the microstructure and properties of H-beams for railway vehicles by refining grain size according to claim 1, characterized in that, The chemical composition of the H-beam is as follows (mass fraction): C 0.06%, Si 0.20%, Mn 1.20%, P 0.012%, S 0.005%, Alt 0.030%, Ti 0.012%, Nb 0.020%, V 0.045%, Ca 0.0015%, with the balance being Fe and impurities.
4. The process for improving the microstructure and properties of H-beams for railway vehicles by refining grain size according to claim 1, characterized in that, The chemical composition of the H-beam is as follows (mass fraction): C 0.10%, Si 0.40%, Mn 1.50%, P 0.012%, S 0.012%, Alt 0.030%, Ti 0.025%, Nb 0.040%, V 0.045%, Ca 0.0015%, with the balance being Fe and impurities.
5. The process for improving the microstructure and properties of H-beams for railway vehicles by refining grain size according to claim 2, characterized in that, Specifically: The converter tapping temperature is 1635℃, and the deoxidation is carried out in stages: 65% aluminum is added before tapping, and ferrotitanium is added at 1 / 2 of the tapping time. LF refining: basicity 4.0, soft argon blowing 100L / min for 18min, Ca content controlled at 0.0015%; Continuous casting: Tundish temperature 1540℃, casting speed 1.0m / min; Rolling: Heating temperature 1220℃, first stage rolling 1120℃, cumulative reduction 65%; second stage rolling 880℃, cumulative reduction 55%, final rolling temperature 800℃; Cooling: First stage cooling rate 18℃ / s, final temperature 700℃; air cooling 45s; Second stage cooling rate 8℃ / s, final temperature 580℃, air cooling to room temperature.
6. The process for improving the microstructure and properties of H-beams for railway vehicles by refining grain size according to claim 3, characterized in that, Process parameters: heating temperature 1200℃, two-stage initial rolling 850℃, final rolling 780℃; first-stage cooling rate 15℃ / s.
7. The process for improving the microstructure and properties of H-beams for railway vehicles by refining grain size according to claim 4, characterized in that, Process parameters: heating temperature 1250℃, two-stage initial rolling 900℃, final rolling 820℃; first stage cooling rate 20℃ / s.