A low-anisotropy, high-strength and high-toughness 5A90 aluminum-lithium alloy sheet and its preparation method
By combining pre-aging and pre-deformation processes, low-anisotropy, high-strength and high-toughness 5A90 aluminum-lithium alloy plates are prepared, solving the problems of insufficient material anisotropy and plasticity in traditional processes, and achieving a balance between high strength and toughness, which is suitable for key components in the aerospace field.
Patent Information
- Application Number
- CN202611252440.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-18
- Publication Date
- 2026-11-17
AI Technical Summary
Traditional 5A90 aluminum-lithium alloy plates exhibit strong anisotropy and insufficient plasticity and toughness during hot rolling, especially in the core of thick plates where the microstructure is severely uneven, making it difficult to meet the application requirements of the aerospace field.
By combining pre-aging and pre-deformation processes, and inducing uniform dislocation distribution through shearable second-phase particles, and combining forging, hot rolling, isothermal rolling, solution treatment, pre-aging and artificial aging processes, low anisotropy and high strength and toughness 5A90 aluminum-lithium alloy plates are prepared.
It effectively reduces the anisotropy of materials, improves strength and plasticity, and ensures the comprehensive mechanical properties of the alloy, making it suitable for manufacturing key components in the aerospace field.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] This invention belongs to the field of hot working technology of non-ferrous metal materials, specifically relating to a low anisotropy, high strength and toughness 5A90 aluminum-lithium alloy sheet and its preparation method. Background Technology
[0002] 5A90 aluminum-lithium alloy is a lightweight, high-strength metallic structural material that combines low density, high strength, corrosion resistance, and ease of forming, and has been widely used in the aerospace field. Adding 1% lithium to the alloy reduces its density by 3% and increases its elastic modulus by 6%. Replacing traditional high-strength aluminum alloys can reduce structural weight by 5%–15% and increase stiffness by 15%–20%, making it a promising material for aerospace applications.
[0003] The traditional manufacturing process for 5A90 aluminum-lithium alloy sheets involves forging, hot rolling, solution treatment, and artificial aging. However, sheets prepared using this process have the following problems: 1. During the hot rolling process of 5A90 aluminum-lithium alloy, the grains undergo directional plastic flow under the combined action of compressive and shear stresses, forming a banded structure with the rolling direction as the long axis. This process is accompanied by a rearrangement of specific crystallographic orientations, promoting the formation of strong deformation textures represented by S and Brass within the material. In this type of texture composition, the grain slip system differs significantly from the Schmidt factor and Taylor factor relative to different loading axis directions. When loaded along the rolling direction, most grains are in a soft orientation state that favors slip; while when loaded in the transverse direction, a large number of grains are in a hard orientation state that is unfavorable to slip. This difference in deformation resistance depending on the direction manifests as significant anisotropy in yield strength, tensile strength, and plasticity in macroscopic mechanical properties.
[0004] 2. In traditional hot rolling processes, the coarse primary phases and brittle impurity particles in the cast state are difficult to fully break down and dissolve during rolling. Instead, they are elongated along the rolling direction and distributed in a chain-like pattern. The interface between these brittle particles and the aluminum matrix becomes a stress concentration point and a source of micropore initiation during subsequent deformation or service, significantly reducing the material's fracture toughness and fatigue life. On the other hand, aluminum-lithium alloys have high stacking fault energies and strong dynamic recovery during hot deformation. While this is conducive to dislocation annihilation and subgrain formation, it inhibits the full progress of dynamic recrystallization, resulting in the retention of a large number of unrecrystallized or partially recrystallized banded structures composed of substructures and small-angle grain boundaries in the plate. This extreme inhomogeneity in grain size and morphology makes it difficult to coordinate micro-deformation, further deteriorating plasticity and fracture toughness. Especially in the core of thick plates, insufficient deformation and differences in heat dissipation exacerbate the inhomogeneity of the microstructure, forming performance-weak areas that are difficult to detect.
[0005] Therefore, the key to the widespread application of this alloy lies in how to improve the mechanical properties of 5A90 aluminum-lithium alloy plates while ensuring their plasticity and reducing anisotropy. Summary of the Invention
[0006] This invention addresses the technical problems existing in the prior art by proposing a method for preparing low-anisotropy, high-strength and high-toughness 5A90 aluminum-lithium alloy plates. By combining pre-aging and pre-deformation processes, the method utilizes shearable second-phase particles to induce a uniform distribution of dislocations during the pre-deformation process, thereby reducing the anisotropy of the plate and maintaining high plasticity while improving the alloy strength.
[0007] To achieve the above objectives, the present invention adopts the following technical solution: A method for preparing a low-anisotropy, high-strength and high-toughness 5A90 aluminum-lithium alloy sheet includes the following steps: (1) Forging: After holding the 5A90 aluminum-lithium alloy ingot at 450~470℃ for 8-10h, it is forged at the same temperature (450~470℃) to obtain an aluminum-lithium alloy plate forging with a thickness of 55mm. (2) Hot rolling: The oxide layer on the surface of the aluminum-lithium alloy plate forging obtained in step (1) is milled off, and after being kept at 440~450℃ for 4~6h, it is hot rolled to a final thickness of 20mm to obtain aluminum-lithium alloy plate. (3) Isothermal rolling: The aluminum-lithium alloy plate obtained in step (2) is kept at 440~450℃ for 1~3h and then isothermal rolled to 3mm, wherein the roll temperature is 400~450℃. (4) Solution treatment: The 3mm thick plate obtained in step (3) is subjected to solution treatment at a temperature of 440~450℃ for 30~60min. (5) Pre-aging treatment: The plate after step (4) is subjected to pre-aging treatment. The pre-aging treatment temperature is 100~200℃ and the aging treatment time is 2~8h. Then it is air-cooled or water-cooled to room temperature to obtain an aluminum-lithium alloy plate with a thickness of 2~3mm. (6) Pre-deformation: The sheet obtained in step (5) is cold-rolled and pre-deformed at room temperature; (7) Artificial aging: The pre-deformed plate from step (6) is artificially aged at a temperature of 100~200℃ for 8~24h, and then air-cooled or water-cooled to room temperature to finally obtain a high-strength and tough 5A90 aluminum-lithium alloy plate.
[0008] Specifically, the 5A90 aluminum-lithium alloy ingot in step (1) is composed of the following components by mass percentage: magnesium 4.5~6.0%, lithium 1.9~2.3%, zirconium 0.08~0.16%, with the balance being aluminum.
[0009] Specifically, step (1) adopts a three-upsetting and three-drawing process for forging, with a forging ratio of (1.5~1.8):1, a forging pressing speed of 10~30mm / s, a single upsetting pressing amount of 30%, and forging in one fire without tempering in the middle. The total forging time is 10~30min.
[0010] Specifically, in step (2), the hot rolling temperature is 440~450℃.
[0011] Specifically, in step (2), the single-pass reduction during hot rolling is 10-20%, and no tempering is performed in between, with a total deformation of 60-70%.
[0012] Specifically, in step (3), the deformation amount per pass during isothermal rolling is 10~20% (preferably 20%), no tempering is performed in the middle, and the total deformation amount is 80~90% (preferably 85%).
[0013] Specifically, in step (3), the roll temperature is controlled at 420℃ during the isothermal rolling process.
[0014] Specifically, in step (4), the plate that has undergone solution treatment is subjected to water quenching at 35~50℃ for 1~3 minutes.
[0015] Specifically, in step (6), the obtained sheet material is cold-rolled and pre-deformed along the TD direction of the sheet material at room temperature.
[0016] Specifically, in step (6), during cold rolling pre-deformation, the single-pass reduction is 1~2%, and the total deformation is 2~8%.
[0017] Furthermore, the present invention also provides a method for preparing a low anisotropy, high strength and toughness 5A90 aluminum-lithium alloy sheet by means of the above-mentioned method through forging, hot rolling, isothermal rolling, solution treatment, pre-aging, pre-deformation, and artificial aging.
[0018] Specifically, this invention is based on 5A90 aluminum-lithium alloy and produces 5A90 aluminum-lithium alloy sheets, which are intended to be used in the processing and manufacturing of spacecraft or military and civilian aircraft parts.
[0019] Based on this, the present invention also provides the application of the low anisotropy, high strength and toughness 5A90 aluminum-lithium alloy sheet in the processing or manufacturing of spacecraft or military and civilian aircraft parts.
[0020] Specifically, the improved low anisotropy, high strength and toughness 5A90 aluminum-lithium alloy sheet of this invention has a wide range of applications in the aerospace field. It is mainly used to manufacture structural frames, panels or skins for parts such as wings, or to manufacture fuel tanks or shells for rockets and missiles, and has broad application prospects.
[0021] This invention uses a low-density, high-Mg-content 5A90 aluminum-lithium alloy as a base and employs a combination of forging, hot rolling, isothermal rolling, solution treatment, pre-aging, pre-deformation, and artificial aging processes to prepare a low-anisotropy, high-strength, and high-toughness aluminum-lithium alloy sheet. The method of this invention combines pre-aging and pre-deformation processes, utilizing shearable second-phase particles to induce a uniform distribution of dislocations during pre-deformation, thereby reducing the anisotropy of the sheet. This improves the alloy's strength while maintaining high plasticity, providing a feasible path for the research and development and production of low-anisotropy, high-strength, and high-toughness aluminum-lithium alloy sheets. This invention offers a wide process window, controllable costs, and produces sheets with excellent comprehensive mechanical properties, demonstrating promising prospects for engineering applications.
[0022] Compared with the prior art, the present invention has the following technical advantages: 1. This invention precipitates a large number of shearable GP regions and fine δ′ phases in the matrix through short-time pre-aging, resulting in a uniform distribution of dislocations introduced by subsequent pre-deformation, thus avoiding dislocation entanglement and local stress concentration. This uniform dislocation structure provides a rapid diffusion channel for solute atoms during artificial aging, promoting the large-scale dispersion precipitation of the δ′ phase and achieving a synergistic contribution of precipitation strengthening and dislocation strengthening.
[0023] 2. This invention avoids coarsening of the δ′ phase due to excessive aging by precisely controlling the pre-aging time and pre-deformation amount, while suppressing the harmful transformation of the GP region to the β phase (Al3Mg2) under high deformation amount, ensuring that the strengthening effect is mainly based on the orderly strengthening mechanism, and guaranteeing the comprehensive performance of the alloy.
[0024] 3. The pre-aging temperature, time, and pre-deformation amount involved in this invention are all within the parameter range that are easy to control in industrial production. No special devices such as cryogenic equipment or pulse current are required. It can be realized on conventional heat treatment production lines and has good prospects for engineering applications.
[0025] 4. The low anisotropy, high strength and toughness aluminum-lithium alloy sheet of the present invention has a simple process, low cost, high comprehensive mechanical properties, and good application prospects. Attached Figure Description
[0026] Figure 1 EBSD image of the 55mm thick 5A90 aluminum-lithium alloy forging obtained in step (1) of Example 1; Figure 2 The stress-strain curve of the high-strength and high-toughness 5A90 aluminum-lithium alloy plate obtained in Example 1 at room temperature and strain rate of 2 mm / min; Figure 3 TEM image of the high-strength and high-toughness 5A90 aluminum-lithium alloy sheet obtained in Example 1; Figure 4 HRTEM image of the high-strength and high-toughness 5A90 aluminum-lithium alloy sheet obtained in Example 1; Figure 5 Photograph of the high-strength and high-toughness 5A90 aluminum-lithium alloy sheet obtained in Example 1; Figure 6 The stress-strain curve of the 5A90 aluminum-lithium alloy plate obtained in Comparative Example 1 is shown. Detailed Implementation
[0027] To make the technical objectives, technical solutions, and beneficial effects of the present invention clearer, the technical solutions of the present invention will be further described below in conjunction with specific embodiments. However, the embodiments are intended to explain the present invention and should not be construed as limiting the present invention. Where no specific technology or conditions are specified in the embodiments, the technology or conditions described in the literature in the field or the product manual shall apply.
[0028] Unless otherwise specified, the experimental methods used in the following examples are conventional methods; unless otherwise specified, the instruments and equipment used in the following examples are commercially available conventional instruments and equipment; unless otherwise specified, the reagents, raw materials, etc. used in the following examples are conventional commercial products and can be obtained through commercial channels.
[0029] In the following examples and comparative examples, room temperature or normal temperature refers to 25±5℃.
[0030] The aluminum-lithium alloy grades and alloy compositions involved in the embodiments and comparative examples of this invention are shown in Table 1.
[0031] Table 1. Grades and composition of aluminum-lithium alloys.
[0032]
[0033] Example 1 A method for preparing a low-anisotropy, high-strength, high-toughness aluminum-lithium alloy sheet, the specific steps of which are as follows: (1) Forging: The 5A90 aluminum-lithium alloy ingot was held at 450℃ for 8 hours and then forged at the same temperature (450℃). The forging process was three upsetting and three drawing, the forging ratio was 1.7, the forging speed was 30mm / s, the single upsetting reduction was 30%, and it was forged in one heat without tempering. The total forging time was 30min, and an aluminum-lithium alloy plate forging with a thickness of 55mm was obtained (e.g. Figure 1 (as shown) (2) Hot rolling: The oxide layer on the surface of the aluminum-lithium alloy plate forging obtained in step (1) is milled off, and after being kept at 450℃ for 5 hours, it is hot rolled at the same temperature (450℃). The single pass reduction is 20%, and no tempering is performed in the middle. Finally, it is rolled to 20mm to obtain aluminum-lithium alloy plate. (3) Isothermal rolling: The aluminum-lithium alloy sheet obtained in step (2) is held at 450℃ for 1.5h and then isothermally rolled to 3mm. The roll temperature is 420℃. The deformation per pass during rolling is 20%, and no tempering is performed in between. The total deformation is 85%. (4) Solution treatment: The 3mm thick plate obtained in step (3) is subjected to solution treatment at a temperature of 450℃ for 45min. Then, it is quickly transferred to a quenching water tank within 5s for water quenching and cooling treatment. The initial water temperature is 35℃ and the water quenching time is 3min. (5) Pre-aging treatment: The plate after quenching in step (4) is subjected to pre-aging treatment at a temperature of 120°C for 2 hours, and then air-cooled to room temperature. (6) Pre-deformation: The plate after pre-aging in step (5) is cold-rolled and pre-deformed along the TD direction of the plate at room temperature. The single-pass reduction during the cold rolling pre-deformation process is 2%, and the total deformation is 4%. (7) Artificial aging: The pre-deformed sheet material from step (6) is subjected to artificial aging at a temperature of 120℃ for 12 hours, followed by air cooling to room temperature, ultimately yielding a 5A90 aluminum-lithium alloy sheet material with dimensions of 3000mm*1500mm*2.9mm (e.g., Figure 5 (As shown).
[0034] The stress-strain curves of the high-strength and high-toughness 5A90 aluminum-lithium alloy sheet obtained in Example 1 after tensile testing at room temperature and a strain rate of 2 mm / min are shown below. Figure 2 As shown.
[0035] Figure 3 The image shows a TEM image of the low anisotropy, high strength and toughness 5A90 aluminum-lithium alloy sheet obtained in Example 1. Figure 3 It can be seen that the dislocations in the high-strength and tough 5A90 aluminum-lithium alloy plate prepared by this method are uniformly distributed.
[0036] Figure 4 The image shows the HRTEM image of the low anisotropy, high strength and toughness 5A90 aluminum-lithium alloy sheet obtained in Example 1. Figure 4 It can be seen that a large number of GP regions were precipitated during pre-aging. Example 2
[0037] A method for preparing a low-anisotropy, high-strength, high-toughness aluminum-lithium alloy sheet, the specific steps of which are as follows: (1) Forging: After holding the 5A90 aluminum-lithium alloy ingot at 450℃ for 8 hours, it was forged at the same temperature (450℃). The forging process of three upsetting and three drawing was adopted, the forging ratio was 1.7, the forging speed was 30mm / s, the single upsetting reduction was 30%, and it was forged in one fire without tempering in the middle. The total forging time was 30min, and an aluminum-lithium alloy plate forging with a thickness of 55mm was obtained. (2) Hot rolling: The oxide layer on the surface of the aluminum-lithium alloy plate forging obtained in step (1) is milled off, and after being kept at 450℃ for 5 hours, it is hot rolled at the same temperature (450℃). The single pass reduction is 20%, and no tempering is performed in the middle. Finally, it is rolled to 20mm to obtain aluminum-lithium alloy plate. (3) Isothermal rolling: The aluminum-lithium alloy sheet obtained in step (2) is held at 450℃ for 1.5h and then isothermally rolled to 3mm. The roll temperature is 420℃. The deformation per pass during rolling is 20%, and no tempering is performed in between. The total deformation is 85%. (4) Solution treatment: The 3mm thick plate obtained in step (3) is subjected to solution treatment at a temperature of 450℃ for 45min. Then, it is quickly transferred to a quenching water tank within 5s for water quenching and cooling treatment. The initial water temperature is 35℃ and the water quenching time is 3min. (5) Pre-aging treatment: The plate after quenching in step (4) is subjected to pre-aging treatment at a temperature of 120°C for 2 hours, and then air-cooled to room temperature to obtain an aluminum-lithium alloy plate with a thickness of 2-3 mm. (6) Pre-deformation: The plate after pre-aging in step (5) is cold-rolled and pre-deformed along the TD direction of the plate at room temperature. The single-pass reduction during the cold rolling pre-deformation process is 2%, and the total deformation is 6%. (7) Artificial aging: The pre-deformed plate from step (6) is artificially aged at a temperature of 120°C for 12 hours, and then air-cooled to room temperature to obtain a 5A90 aluminum-lithium alloy plate with dimensions of 3000mm*1500mm*2.8mm. Example 3
[0038] Example 3 provides a method for preparing a low-anisotropy, high-strength, high-toughness aluminum-lithium alloy sheet. The difference between Example 3 and Example 1 is that: After solution treatment, no pre-aging treatment is performed; instead, pre-deformation and artificial aging are carried out directly.
[0039] Comparative Example 1 Comparative Example 1 provides a method for preparing 5A90 aluminum-lithium alloy, the specific steps of which are as follows: (1) Forging: After holding the 5A90 aluminum-lithium alloy ingot at 460℃ for 10h, it was forged at the same temperature (460℃). The forging process of three upsetting and three drawing was adopted, the forging ratio was 1.7, the forging speed was 30mm / s, the single upsetting reduction was 30%, and it was forged in one fire without tempering in the middle. The total forging time was 30min, and an aluminum-lithium alloy plate forging with a thickness of 55mm was obtained. (2) Hot rolling: The oxide layer on the surface of the aluminum-lithium alloy plate forging obtained in step (1) is milled off, and after being kept at 450℃ for 6 hours, it is hot rolled at the same temperature (450℃). The single pass reduction is 20%, and no tempering is performed in the middle. Finally, it is rolled to 20mm to obtain aluminum-lithium alloy plate. (3) Isothermal rolling: The aluminum-lithium alloy sheet obtained in step (2) is held at 450℃ for 1.5h and then isothermally rolled to 3mm. The roll temperature is 400℃. The deformation per pass during rolling is 20%. Tempering is not performed in the middle. The total deformation is 85%. (4) Solution treatment: The 3mm thick plate obtained in step (3) is subjected to solution treatment at a temperature of 450℃ for 30 minutes. Then, it is quickly transferred to a quenching water tank within 5 seconds for water quenching. The initial water temperature is 35℃ and the water quenching time is 3 minutes. (5) Artificial aging: The plate obtained in step (4) is artificially aged at a temperature of 120°C for 12 hours and then air-cooled to room temperature to obtain a 5A90 aluminum-lithium alloy plate with a size of 3000mm*1500mm*3mm.
[0040] The tensile results of Comparative Example 1 are as follows Figure 6 As shown.
[0041] Performance testing The room temperature mechanical properties were tested according to GB / T 16865-2023. The specimens were subjected to tensile testing on an MTS Landmark electro-hydraulic servo testing machine, with the tensile direction along the RD and TD directions of the sample. An extensometer was used during the tensile process for more accurate deformation measurement. The clamp movement speed was 2 mm / min. Three parallel specimens were tested for each condition, and the average value was taken. The properties of the aluminum-lithium alloy sheets obtained in the examples and comparative examples are shown in Table 2.
[0042] Table 2 is a summary table of the performance of the high-strength and tough 5A90 aluminum-lithium alloy sheet in the examples and the comparative examples.
[0043]
[0044] From Table 2 and Figure 2As can be seen, the low-anisotropy, high-strength and high-toughness 5A90 aluminum-lithium alloy sheet prepared by this invention exhibits a tensile strength of 453.7 MPa, a yield strength of 283.4 MPa, and an elongation of 12% in the RD direction at room temperature; and a tensile strength of 467.7 MPa, a yield strength of 304 MPa, and an elongation of 9.5% in the TD direction. The low-anisotropy, high-strength and high-toughness 5A90 aluminum-lithium alloy sheet prepared by this invention has wide applications in the aerospace field. It is mainly used to manufacture structural frames, panels, or skins for components such as wings, or for manufacturing fuel tanks and shells for rockets and missiles, demonstrating broad application prospects.
[0045] The specific embodiments of the present invention have been described above. It should be understood that the present invention is not limited to the specific embodiments described above. Those skilled in the art can make various modifications or variations within the scope of the claims, which do not affect the essence of the present invention.
Claims
1. A method for preparing a low-anisotropy, high-strength, high-toughness aluminum-lithium alloy sheet, characterized in that, Includes the following steps: (1) Forging: The 5A90 aluminum-lithium alloy ingot is held at 450~470℃ for 8-10h and then forged to obtain aluminum-lithium alloy plate forgings. (2) Hot rolling: The oxide layer on the surface of the aluminum-lithium alloy plate forging obtained in step (1) is milled off, and the plate is held at 440~450℃ for 4~6h before hot rolling to obtain aluminum-lithium alloy plate. (3) Isothermal rolling: The aluminum-lithium alloy plate obtained in step (2) is kept at 440~450℃ for 1~3h and then isothermal rolling is carried out, wherein the roll temperature is 400~450℃. (4) Solution treatment: The board obtained in step (3) is subjected to solution treatment at a temperature of 440~450℃ for 30~60min. (5) Pre-aging treatment: The plate obtained in step (4) is subjected to pre-aging treatment at a temperature of 100~200℃ and an aging treatment time of 2~8h. Then it is air-cooled or water-cooled to room temperature to obtain an aluminum-lithium alloy plate with a thickness of 2~3mm. (6) Pre-deformation: The sheet obtained in step (5) is cold-rolled and pre-deformed at room temperature; (7) Artificial aging: The plate from step (6) is artificially aged at a temperature of 100~200℃ for 8~24h, and then air-cooled or water-cooled to room temperature to finally obtain a low anisotropy, high strength and toughness 5A90 aluminum-lithium alloy plate.
2. The preparation method according to claim 1, characterized in that, The 5A90 aluminum-lithium alloy ingot in step (1) is composed of the following components by mass percentage: magnesium 4.5~6.0%, lithium 1.9~2.3%, zirconium 0.08~0.16%, with the balance being aluminum.
3. The preparation method according to claim 1, characterized in that, In step (2), the single-pass reduction during hot rolling is 10-20%, and no tempering is performed in between, with a total deformation of 60-70%.
4. The preparation method according to claim 1, characterized in that, In step (3), the deformation amount per pass during isothermal rolling is 10~20% (preferably 20%), no tempering is performed in the middle, and the total deformation amount is 80~90% (preferably 85%).
5. The preparation method according to claim 1, characterized in that, In step (4), the solution-treated plate is subjected to water quenching at 35~50℃.
6. The preparation method according to claim 1, characterized in that, In step (6), the obtained sheet is cold-rolled and pre-deformed along the TD direction of the sheet at room temperature.
7. The preparation method according to claim 1, characterized in that, In step (6), during cold rolling pre-deformation, the single-pass reduction is 1~2%, and the total deformation is 2~8%.
8. A low-anisotropy, high-strength and high-toughness 5A90 aluminum-lithium alloy sheet prepared by any one of the methods described in claims 1 to 7.
9. The application of the low anisotropy, high strength and toughness 5A90 aluminum-lithium alloy sheet of claim 8 in the processing or manufacturing of spacecraft or military and civilian aircraft parts.
10. The application of the low anisotropy, high strength and toughness 5A90 aluminum-lithium alloy sheet of claim 8 in the manufacture of structural frames, panels or skins for parts such as wings, or in the manufacture of fuel tanks or shells for rockets and missiles.