A method for synergistically improving strength and ductility of a Cu-Ni-Si alloy plate strip

By combining high-temperature short-time annealing with two-stage deep cryogenic rolling, the problems of limited secondary deformation capacity and difficulty in introducing nanotwins caused by unreasonable intermediate annealing process in Cu-Ni-Si alloy strips and sheets were solved. This approach achieved a synergistic improvement in strength and plasticity, resulting in a synergistic strengthening effect of high-density nanotwins and δ-Ni2Si precipitates.

CN123108449APending Publication Date: 2026-11-17HENAN UNIV OF SCI & TECH +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611137199.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-29
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In the existing Cu-Ni-Si alloy sheet and strip preparation and processing technology, there are technical difficulties such as limited secondary deformation capacity due to unreasonable intermediate annealing process, difficulty in introducing nanotwins, and difficulty in balancing strength and plasticity.

Method used

A combined method of high-temperature short-time annealing and two-stage cryogenic rolling is adopted, including a first-stage cryogenic rolling in the liquid nitrogen temperature zone with a total deformation of 65%~85%, divided into 5~8 passes, with each pass followed by immersion in liquid nitrogen for heat preservation; high-temperature short-time annealing is carried out at 750℃~800℃ for 10~30 seconds followed by rapid cooling; the second-stage cryogenic rolling is carried out in the liquid nitrogen temperature zone with a total deformation of 40%~60%, divided into 1~3 passes, with each pass followed by immersion in liquid nitrogen for heat preservation; and low-temperature aging treatment is carried out at 400℃~450℃ for 2~4 hours.

Benefits of technology

The synergistic enhancement of strength and plasticity of Cu-Ni-Si alloy plates and strips was achieved, with tensile strength reaching 715.68 MPa, yield strength reaching 670 MPa, elongation reaching 13.61%, and electrical conductivity reaching 51.30% IACS. High-density nanotwins and δ-Ni2Si precipitates were successfully introduced to synergistically strengthen the material, significantly improving the overall performance of strength and plasticity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108449A_ABST
    Figure CN123108449A_ABST
Patent Text Reader

Abstract

The application discloses a method for improving the strength and plasticity of Cu-Ni-Si alloy strip and belongs to the technical field of copper alloy material preparation and processing. The method uses Cu-Ni-Si alloy plate after solid solution treatment as raw material, and sequentially carries out first-stage deep cold rolling, high-temperature short-time annealing, second-stage deep cold rolling and low-temperature aging treatment. The first-stage deep cold rolling changes the solid solution state structure into a deformed structure containing high-density dislocations and layer defect. The high-temperature short-time annealing retains part of the layer defect as a nanotwin nucleation precursor and eliminates part of the work hardening. The second-stage deep cold rolling induces the formation of high-density nanotwins on the precursor, the average width of the nanotwins is 2.13-3.47 nm, and the twin strengthening contribution is 80.5-93 MPa. The low-temperature aging treatment uniformly precipitates δ-Ni2Si precipitates in the matrix and near the twin boundaries and dislocation walls, and forms synergistic strengthening with the nanotwins. The obtained plate strip has a tensile strength of 715.68 MPa, a yield strength of 670 MPa, an elongation of 13.61%, and an electrical conductivity of 51.30% IACS, and the synergistic improvement of the strength and plasticity is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of copper alloy material preparation and processing technology, specifically a method for synergistically improving the strength and plasticity of Cu-Ni-Si alloy plates and strips. Background Technology

[0002] Cu-Ni-Si alloy is a typical precipitation-strengthened copper alloy, widely used in high-end connectors in aerospace, new energy vehicles, and other fields due to its combination of high strength and good conductivity. The strengthening of this alloy mainly comes from the δ-Ni₂Si phase precipitated during the aging process. The interaction between the precipitated phase and dislocations hinders dislocation movement, thus achieving precipitation strengthening. The typical thermomechanical treatment route for Cu-Ni-Si alloy is solution treatment → cold rolling → aging treatment. The aging treatment is usually carried out at 400-500℃ for several hours to promote the full precipitation of the δ-Ni₂Si phase, achieving precipitation strengthening.

[0003] However, the existing Cu-Ni-Si alloy sheet and strip preparation and processing technology still has the following shortcomings: (1) In order to further improve the strength of the alloy, researchers have tried to use a two-stage cold rolling process to increase the total deformation. Two-stage cold rolling refers to the introduction of intermediate annealing between two cold rolling deformations to eliminate the work hardening generated by the first stage of cold rolling, restore the material's deformation capacity, and thus achieve a larger cumulative deformation in the second stage of cold rolling. However, the existing intermediate annealing usually adopts low-temperature recovery annealing at 300-400℃. In this temperature range, the material mainly undergoes a recovery process, accompanied only by limited dislocation climb and annihilation. Work hardening is difficult to be fully eliminated, and plastic recovery is limited. Therefore, the amount of deformation that can be applied in the secondary rolling process is limited, which weakens the contribution of subsequent work hardening to the material strength. In contrast, if high-temperature solution treatment at 850-950℃ is used instead of low-temperature recovery annealing, although work hardening can be significantly eliminated and the plasticity of the material can be restored, it will usually induce complete recrystallization and subsequent grain growth, causing the deformation structure such as dislocations, deformation bands and substructures formed in the early stage to basically disappear, which is not conducive to the inheritance and control of microstructure in subsequent deformation process; (2) Copper alloys have high stacking fault energy, and dislocation slip dominates under conventional room temperature deformation conditions, making it difficult to initiate twin deformation. Even with low-temperature deformation, the density and uniformity of nanotwins are still very limited due to the lack of effective twin nucleation promotion methods. Studies have shown that nanotwins can effectively interfere with dislocation movement and have minimal impact on the resistivity of copper alloys, making them an ideal microstructure to break the strong plasticity inversion dilemma. However, there is still a lack of effective process methods for introducing high-density nanotwins into Cu-Ni-Si alloys; (3) The formation of nanotwins requires specific nucleation precursors (such as stacking faults and other defect structures), which are usually introduced through pre-deformation. If these precursors are to be introduced after the first-stage cold rolling and nanotwins are to be induced in the second-stage cold rolling, the intermediate annealing must retain a sufficient number of precursors while eliminating work hardening. However, although traditional low-temperature annealing (300-400℃) can retain precursors, work hardening is not sufficiently eliminated and the ability to undergo secondary deformation is insufficient; although traditional high-temperature solution treatment (850-950℃ / several hours) can eliminate work hardening, the precursors are completely eliminated and the grains are coarsened, which cannot create conditions for the subsequent formation of nanotwins. Existing processes have not been able to solve this contradiction; (4) In traditional processes, although aging treatment can improve strength through precipitation strengthening, it often comes at the cost of sacrificing plasticity. If a nanotwin strengthening mechanism can be introduced, the strength can be improved without significantly losing plasticity by utilizing the hindering effect of twin boundaries on dislocation movement. However, as mentioned above, existing processes cannot effectively introduce high-density nanotwins into Cu-Ni-Si alloys, so it is difficult to balance strength and plasticity.

[0004] In summary, the existing Cu-Ni-Si alloy sheet and strip manufacturing technologies have not yet effectively solved the technical problems of limited secondary deformation capacity due to unreasonable intermediate annealing processes, difficulty in introducing nanotwins, and difficulty in balancing strength and plasticity. Summary of the Invention

[0005] This invention provides a method for synergistically improving the strength and plasticity of Cu-Ni-Si alloy plates and strips, in order to solve the technical problems in the prior art, such as limited secondary deformation capacity due to unreasonable intermediate annealing process, difficulty in introducing nanotwins, and difficulty in balancing strength and plasticity.

[0006] To achieve the above objectives, the specific solution adopted by the present invention is as follows: A method for synergistically improving the strength and plasticity of Cu-Ni-Si alloy plates and strips includes the following steps: Cu-Ni-Si alloy sheet and strip after solid solution treatment are used as raw materials, and the matrix of the raw materials is a copper-based solid solution matrix; The raw material is subjected to a first-stage cryogenic rolling process in the liquid nitrogen temperature zone. The total deformation is 65% to 85%, and the process is divided into 5 to 8 passes. After each pass, the material is immersed in liquid nitrogen for 10 to 30 minutes. The first-stage cryogenic rolling process transforms the internal structure of the raw material from a solid solution state to a deformed structure containing high-density dislocations and stacking fault defects, resulting in a first-stage cryogenic rolled plate. The first-stage cryogenic rolled plate is subjected to high-temperature short-time annealing. The high-temperature short-time annealing is carried out at 750℃~800℃ for 10~30 seconds and then rapidly cooled. The high-temperature short-time annealing allows some of the stacking fault defects in the deformed structure inside the first-stage cryogenic rolled plate to be retained as precursors for nanotwin nucleation, while eliminating some of the work hardening in the deformed structure, thus obtaining a high-temperature short-time annealed plate. The high-temperature short-time annealed plate is subjected to two-stage cryogenic rolling in the liquid nitrogen temperature zone. The total deformation is 40% to 60%, and it is divided into 1 to 3 passes. After each pass, the plate is immersed in liquid nitrogen for 10 to 30 minutes. The two-stage cryogenic rolling induces the formation of high-density nanotwins on the nanotwin nucleation precursor. The average width of the nanotwins is 2.13 to 3.47 nm. The nanotwins have twin boundaries, and dislocation walls are also present inside the high-temperature short-time annealed plate, resulting in a two-stage cryogenic rolled plate. The secondary cryogenic rolled plate is subjected to low-temperature aging treatment, which is carried out at 400℃~450℃ for 2~4 hours. The low-temperature aging treatment causes δ-Ni2Si precipitates to precipitate uniformly and be distributed in the matrix, as well as near twin boundaries and dislocation walls, forming a synergistic strengthening with the nanotwins, resulting in Cu-Ni-Si alloy plate and strip with synergistic improvement in strength and plasticity.

[0007] Furthermore, the total deformation of the first-stage cryogenic rolling is 75%, divided into 5 passes, with liquid nitrogen holding for 30 minutes after each pass; the high-temperature short-time annealing temperature is 780℃, and the holding time is 20 seconds.

[0008] Furthermore, the cooling method for the high-temperature short-time annealing is air cooling or water cooling.

[0009] Furthermore, the secondary cryogenic rolling is completed in a single pass, with a total deformation of 50%.

[0010] Furthermore, the low-temperature aging treatment is performed at a temperature of 420°C for 3 hours.

[0011] Furthermore, the Cu-Ni-Si alloy strip has a tensile strength of 715.68 MPa, a yield strength of 670 MPa, an elongation of 13.61%, and an electrical conductivity of 51.30% IACS.

[0012] The core of this invention lies in the synergistic effect of "high-temperature short-time annealing" and "two-stage deep cryogenic rolling," a combination not previously reported in existing Cu-Ni-Si alloy processing technologies. Compared to traditional processes, the beneficial effects of this invention are as follows: (1) High-temperature short-time annealing (750-800℃ / 10-30 seconds) falls in the gap between traditional low-temperature annealing (300-400℃ / several hours) and high-temperature solution treatment (850-950℃ / several hours), and has unique technical effects. Compared with low-temperature annealing, this invention can more fully eliminate work hardening, allowing the secondary cryogenic rolling to proceed smoothly, while retaining the precursor of nanotwin nucleation, forming high-density nanotwins after the secondary cryogenic rolling; compared with high-temperature solution treatment, this invention avoids the elimination of grain coarsening and deformed structures, making nanotwin strengthening possible.

[0013] (2) The present invention successfully introduced high-density nanotwins into Cu-Ni-Si alloy. After treatment by the method of the present invention, the average width of nanotwins in the alloy is 2.13-3.47 nm, and the twin strengthening contribution is 80.5-93 MPa, while the twin width in the traditional room temperature rolling process is 6.37 nm, and the strengthening contribution is only 59.4 MPa.

[0014] (3) This invention achieves a synergistic improvement in strength and plasticity. Tests show that the Cu-Ni-Si alloy treated by this method has a tensile strength of 715.68 MPa, an elongation of 13.61%, and an electrical conductivity of 51.30% IACS. Compared with the traditional room temperature rolling + low temperature annealing process, the tensile strength is increased by approximately 4.3%, the elongation by approximately 70%, and the electrical conductivity by approximately 2.5%. Particularly noteworthy is that while maintaining or even improving strength, the elongation is nearly doubled.

[0015] (4) The process of the present invention has good operability and stability, and is suitable for continuous and mass production of Cu-Ni-Si alloy strips. It can provide high-performance copper alloy materials for high-end connectors in fields such as new energy vehicles and aerospace. Attached Figure Description

[0016] Figure 1 This is a schematic diagram of the process route of the present invention.

[0017] Figure 2 These are HRTEM images of nanotwins in the Cu-Ni-Si alloy obtained in Example 1 of the present invention, wherein (a)-(d) are HRTEM images of nanotwins after secondary cryogenic rolling; and (e)-(h) are HRTEM images of nanotwins after low-temperature aging treatment.

[0018] Figure 3 These are TEM images of the high-density nanotwin structure in the Cu-Ni-Si alloy obtained in Example 1 of the present invention; wherein, (a) is a TEM image of the nanotwins after primary cryogenic rolling; (b)-(c) are TEM images of the nanotwins after secondary cryogenic rolling; and (d) is a TEM image of the nanotwins after low-temperature aging. Detailed Implementation

[0019] The technical solution of the present invention will be clearly and completely described below with reference to specific embodiments. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the protection scope of the present invention.

[0020] This invention provides a method for synergistically improving the strength and plasticity of Cu-Ni-Si alloy plates and strips, comprising the following steps: Step (1), Material Selection: Take the Cu-Ni-Si alloy plate after solution treatment as raw material. Solution treatment allows the Ni and Si elements in the alloy to fully dissolve in the copper matrix, forming a supersaturated solid solution, which provides the material basis for the precipitation of δ-Ni2Si precipitate phase during the subsequent aging process; Step (2), First-stage cryogenic rolling: The raw material is subjected to first-stage cryogenic rolling in the liquid nitrogen temperature zone (-196℃), with a total deformation of 65%~85%, divided into 5~8 passes. After each pass, the material is immersed in liquid nitrogen for 10~30 minutes. The first-stage cryogenic rolling transforms the internal structure of the raw material from a solid solution state to a deformed structure containing high-density dislocations and stacking faults, resulting in a first-stage cryogenic rolled plate. The purpose of first-stage cryogenic rolling is to significantly suppress dynamic recovery during deformation in the liquid nitrogen temperature zone, allowing for the accumulation of higher-density dislocations and stacking faults within the alloy, transforming the solid solution state into a deformed structure containing high-density dislocations and stacking faults. These defects serve as "nucleation precursors" for subsequent nanotwin formation. If the total deformation is less than 65%, the dislocation and stacking fault density is insufficient, failing to provide enough precursors for subsequent nanotwin formation; if the total deformation is greater than 85%, the work hardening is too severe, and even high-temperature short-time annealing cannot fully restore the deformation capacity, affecting the smooth progress of the second-stage cryogenic rolling. Immersing the sample in liquid nitrogen for 10-30 minutes after each rolling pass is to ensure that the sample temperature drops sufficiently to the liquid nitrogen temperature range, ensuring that the next rolling pass is carried out under cryogenic conditions. Step (3), High-Temperature Short-Time Annealing: The first-stage cryogenic rolled plate is subjected to high-temperature short-time annealing. The high-temperature short-time annealing is carried out at 750℃~800℃ for 10~30 seconds and then rapidly cooled. The high-temperature short-time annealing allows some of the stacking fault defects in the deformed structure inside the first-stage cryogenic rolled plate to be retained as precursors for nanotwin nucleation, while eliminating some of the work hardening in the deformed structure, resulting in a high-temperature short-time annealed plate. This step is the core feature that distinguishes this invention from the prior art. Its unique function is that, on the one hand, the annealing temperature (750-800℃) is sufficient to eliminate most of the work hardening introduced by the first-stage cryogenic rolling. Dislocations rearrange and partially annihilate through climb and slip, restoring the deformability of the alloy and providing good processing conditions for the second-stage cryogenic rolling. On the other hand, due to the extremely short holding time (only 10-30 seconds), grain growth and recrystallization are effectively suppressed. The stacking fault defects introduced by the first-stage cryogenic rolling are not completely eliminated, but are partially retained as precursors for nanotwin nucleation. If the annealing temperature is below 750℃ or the holding time is insufficient, work hardening will not be adequately eliminated; if the annealing temperature is above 800℃ or the holding time is too long, stacking fault precursors will be completely eliminated, and grain coarsening will occur. Rapid cooling (air cooling or water cooling) is to avoid unnecessary precipitation or microstructural changes during the cooling process. Step (4), Secondary Cryogenic Rolling: The high-temperature short-time annealed plate is subjected to secondary cryogenic rolling in the liquid nitrogen temperature zone. The total deformation is 40%~60%, divided into 1~3 passes. After each pass, the plate is immersed in liquid nitrogen for 10~30 minutes. The secondary cryogenic rolling induces the formation of high-density nanotwins on the nanotwin nucleation precursor. The average width of the nanotwins is 2.13~3.47 nm. The nanotwins have twin boundaries, and dislocation walls are also present inside the high-temperature short-time annealed plate, resulting in a secondary cryogenic rolled plate. The purpose of this step is that during secondary cryogenic rolling in the liquid nitrogen temperature zone, dislocation slip is suppressed due to the extremely low deformation temperature, and the deformation mechanism is dominated by twinning deformation. The stacking fault defects retained after high-temperature short-time annealing serve as "nucleation precursors," providing low-energy-barrier nucleation sites for the formation of nanotwins, and inducing the formation of high-density nanotwins under external stress. Nanotwins possess twin boundaries, and dislocation walls also exist within the alloy. If the total deformation in the second-stage cryogenic rolling is less than 40%, the nanotwin density is insufficient, resulting in limited strengthening effect; if it exceeds 60%, it may cause excessive work hardening, affecting the subsequent aging treatment effect. Immersing the sample in liquid nitrogen for 10-30 minutes after each rolling pass is to ensure that the sample temperature drops sufficiently to the liquid nitrogen temperature range, ensuring that the next rolling pass is carried out under cryogenic conditions. Step (5), Low-temperature aging treatment: The secondary cryogenic rolled plate is subjected to low-temperature aging treatment at 400℃~450℃ for 2~4 hours. The low-temperature aging treatment causes δ-Ni2Si precipitates to precipitate uniformly and distribute in the matrix, as well as near twin boundaries and dislocation walls, forming synergistic strengthening with the nanotwins, resulting in Cu-Ni-Si alloy strip with synergistic improvement in strength and plasticity. The purpose of this step is: During the low-temperature aging treatment, Ni and Si atoms in the supersaturated solid solution precipitate in the form of δ-Ni2Si phase. Since there are a large number of twin boundaries and dislocation walls inside the alloy after secondary cryogenic rolling, these defect regions have high distortion energy, providing preferential nucleation and growth sites for δ-Ni2Si precipitates. Therefore, in addition to being distributed outside the matrix, the δ-Ni2Si precipitates are mainly distributed near twin boundaries and dislocation walls, forming synergistic strengthening with the nanotwins. If the aging temperature is below 400℃ or the holding time is insufficient, the precipitated phase will not precipitate sufficiently, and the strengthening effect will be limited; if the aging temperature is above 450℃ or the holding time is too long, the precipitated phase will coarsen, weakening the strengthening effect.

[0021] The Cu-Ni-Si alloy strip after the above treatment has a high-density nanotwin structure. The average width of the nanotwins is 2.13-3.47 nm, and the twin strengthening contribution is 80.5-93 MPa. The δ-Ni2Si precipitate is uniformly distributed in the matrix and near the twin boundaries and dislocation walls, forming a synergistic strengthening with the nanotwins. Finally, the tensile strength of the strip reaches 715.68 MPa, the yield strength reaches 670 MPa, the elongation reaches 13.61%, and the conductivity reaches 51.30% IACS.

[0022] Example 1

[0023] This embodiment describes a method for synergistically improving the strength and plasticity of Cu-Ni-Si alloy plates and strips. The specific steps are as follows: Step (1): Take the Cu-Ni-Si alloy plate after solution treatment as raw material; Step (2), First-stage cryogenic rolling: The raw material is subjected to first-stage cryogenic rolling in the liquid nitrogen temperature zone (-196℃), with a total deformation of 75%, divided into 5 passes. After each pass, the material is immersed in liquid nitrogen for 30 minutes to obtain a first-stage cryogenic rolled plate. Step (3), high temperature short time annealing: The first-level cryogenic rolled plate is subjected to rapid annealing at 780°C for 20 seconds, and then air-cooled to room temperature to obtain a high temperature short time annealed plate; Step (4), Secondary cryogenic rolling: The high-temperature short-time annealed plate is cryogenically rolled again in the liquid nitrogen temperature zone. The total deformation is 50%, and it is completed in a single pass. Before rolling, the sample is immersed in liquid nitrogen for 30 minutes to obtain the secondary cryogenic rolled plate. Step (5), Low temperature aging treatment: The secondary cryogenic rolled plate is subjected to isothermal aging treatment at 420℃ for 3 hours to obtain Cu-Ni-Si alloy plate and strip with synergistic improvement in strength and plasticity.

[0024] Comparative Example 1 The only difference from Example 1 is that in step (2), a low-temperature annealing of 400℃ / 3h is used instead of the high-temperature short-time annealing of the present invention, that is, the first-stage cryogenic rolled plate is annealed by holding it at 400℃ for 3 hours.

[0025] Comparative Example 2 The only difference from Example 1 is that in step (2), the high-temperature short-time annealing of the present invention is replaced by high-temperature solution treatment at 850℃ / 1h, that is, the first-stage cryogenic rolled plate is kept at 850℃ for 1 hour for solution treatment.

[0026] Comparative Example 3 The only difference from Example 1 is that step (2) is omitted, i.e., after the first-stage cryogenic rolling, high-temperature short-time annealing is not performed, and the second-stage cryogenic rolling is performed directly. In this comparative example, the sample cracked during the second-stage cryogenic rolling process and could not complete the subsequent processes.

[0027] Comparative Example 4 The process employs room temperature rolling followed by low-temperature annealing, meaning that both the first and second stages of room temperature rolling are performed at room temperature, while the intermediate annealing uses traditional low-temperature annealing (400℃ / 3h). The total deformation during the first stage of room temperature rolling is 75%, and the total deformation during the second stage is 50%. The remaining steps are the same as in Example 1.

[0028] Performance testing methods (1) Tensile property test: The room temperature tensile test was carried out in accordance with GB / T 228.1-2021 "Metallic materials, tensile testing - Part 1: Test at room temperature" using an Instron universal testing machine with an initial strain rate of 1.4 × 10⁻⁶. -3 s -1 The tensile strength (Rm), yield strength (Rp0.2), and elongation after fracture (A50) were tested.

[0029] (2) Conductivity test: The conductivity was determined at room temperature using the four-terminal potential difference method. The test standard was GB / T 3048.2-2007, and the results were expressed as International Annealed Copper Standard (%IACS).

[0030] (3) Microscopic organizational characterization: Transmission electron microscopy (TEM) observation: The nanotwin structure of the alloy was observed using a JEM-2100F field emission transmission electron microscope with an accelerating voltage of 200 kV. High-resolution TEM (HRTEM) observation was used to measure the width of the nanotwins; at least 100 twins were counted for each sample, and the average value was taken. Electron backscatter diffraction (EBSD) analysis: The grain boundary characteristics and dislocation distribution of the alloy were analyzed using a scanning electron microscope equipped with an EBSD probe. The scanning step size was 0.1 μm. Small-angle grain boundaries were defined as grain boundaries with an orientation difference of 2° to 15°.

[0031] Performance Test Results and Analysis (1) Mechanical properties and electrical conductivity The alloy plates and strips obtained in Examples 1-2 and Comparative Examples 1-3 were tested according to the above test methods, and the results are shown in Table 1.

[0032] Table 1 Performance comparison between the examples and comparative examples

[0033] As shown in Table 1, after treatment with the method of the present invention, Example 1 achieved a tensile strength of 715.68 MPa, a yield strength of 670 MPa, an elongation of 13.61%, and an electrical conductivity of 51.30% IACS. Comparative Example 1 used a low-temperature annealing process of 400℃ / 3h instead of the high-temperature short-time annealing of the present invention, resulting in a tensile strength of 672.35 MPa and an elongation of 9.23%. Compared to Comparative Example 1, the tensile strength of Example 1 increased by approximately 6.4%, and the elongation increased by approximately 47.5%. This indicates that low-temperature annealing cannot fully eliminate work hardening, and the low nanotwin density leads to unsatisfactory strength and plasticity. Comparative Example 2 used a high-temperature solution treatment process of 850℃ / 1h instead of the high-temperature short-time annealing of the present invention, resulting in a tensile strength of 625.41 MPa and an elongation of 14.52%. Compared to Comparative Example 2, the tensile strength of Example 1 increased by approximately 14.4%, while the elongation was essentially the same. This indicates that while high-temperature solution treatment can fully restore deformability and achieve better plasticity, it completely eliminates the deformable structure and precursors, making it impossible to introduce nanotwin reinforcement, resulting in insufficient strength. Comparative Example 3, without intermediate annealing, underwent a second-stage cryogenic rolling directly after the first-stage rolling. The sample cracked during the second-stage rolling process, making subsequent processing impossible. This demonstrates that without appropriate annealing between the two stages of cryogenic rolling to eliminate some work hardening, the material will lose its deformability due to excessive work hardening. Comparative Example 4 exhibited a tensile strength of 686.2 MPa, an elongation of 8.0%, and an electrical conductivity of 52.5% IACS. Compared to Comparative Example 4, Example 1 showed an increase in tensile strength of approximately 4.3%, a significant increase in elongation of approximately 70%, and essentially the same electrical conductivity. This indicates that under room temperature rolling conditions, due to the high stacking fault energy of copper alloys, dislocation slip dominates, making it difficult to fully initiate twinning deformation. This results in nanotwins with larger widths and lower densities. Furthermore, insufficient elimination of work hardening during low-temperature annealing further limits the deformation capacity of secondary rolling and the introduction of nanotwins, leading to poor strength-plasticity matching. Comparative Examples 1-4 show that only the synergistic combination of cryogenic rolling and high-temperature short-time annealing in this invention can ensure the smooth progress of secondary rolling while introducing high-density, narrow-width nanotwins. This achieves a significant simultaneous improvement in both strength and plasticity while maintaining relatively stable conductivity, resulting in significantly superior overall performance compared to the comparative examples.

[0034] (2) Microstructure analysis Depend on Figure 2 and Figure 3It is evident that a high-density nanotwin structure is formed in the alloy treated by the method of this invention, with an average twin width of approximately 2.13-3.47 nm. The high-density nanotwins exhibit uniform width distribution, straight and clear twin boundaries, and extremely small spacing between adjacent twins (only 2.13-3.47 nm), indicating a very large twin interface per unit volume and a significant hindering effect on dislocation movement. Calculations show that the twinning strengthening contribution of the nanotwins reaches 80.5-93 MPa. Comparative Example 4, using room temperature rolling followed by low-temperature annealing, has an average nanotwin width of 6.37 nm and a twinning strengthening contribution of only 59.4 MPa. Compared to Example 1, Comparative Example 4 has a larger twin width and a lower twinning strengthening contribution. A larger twin width results in a larger twin boundary spacing, weakening the hindering effect on dislocation movement and thus limiting the strengthening effect. The present invention reduces the nanotwin width by approximately 45%-59% and increases the twinning strengthening contribution by approximately 35%-57%.

[0035] Meanwhile, the δ-Ni2Si precipitates are uniformly distributed in the matrix and near twin boundaries and dislocation walls, forming a synergistic strengthening effect with the nanotwins. EBSD analysis shows that after high-temperature short-time annealing, the proportion of small-angle grain boundaries in the alloy reaches 83.76%, and the dislocation distribution is more uniform. The high proportion of small-angle grain boundaries means that the deformed structure has been partially restored but not completely recrystallized. This is the microscopic evidence of the "selective retention" of precursors by high-temperature short-time annealing. The grains have not grown significantly, but the dislocations have rearranged to form subgrain boundaries, providing an ideal microstructure that has both a certain degree of deformability and retains the precursors for subsequent second-stage cryogenic rolling.

[0036] In summary, this invention achieves precise control of the microstructure of Cu-Ni-Si alloys through the synergistic combination of high-temperature short-time annealing and two-stage deep cryogenic rolling, successfully introducing a microstructure that is synergistically strengthened by high-density nanotwins and δ-Ni2Si precipitates, ultimately achieving a synergistic improvement in strength and plasticity.

[0037] The above description is merely a preferred embodiment of the present invention and is not intended to limit the scope of the invention in any way. All equivalent transformations or modifications made in accordance with the essence of the present invention should be covered within the protection scope of the present invention.

Claims

1. A method for synergistically improving the strength and plasticity of Cu-Ni-Si alloy plates and strips, characterized in that, Includes the following steps: Cu-Ni-Si alloy sheet and strip after solid solution treatment are used as raw materials, and the matrix of the raw materials is a copper-based solid solution matrix; The raw material is subjected to a first-stage cryogenic rolling process in the liquid nitrogen temperature zone. The total deformation is 65% to 85%, and the process is divided into 5 to 8 passes. After each pass, the material is immersed in liquid nitrogen for 10 to 30 minutes. The first-stage cryogenic rolling process transforms the internal structure of the raw material from a solid solution state to a deformed structure containing high-density dislocations and stacking fault defects, resulting in a first-stage cryogenic rolled plate. The first-stage cryogenic rolled plate is subjected to high-temperature short-time annealing. The high-temperature short-time annealing is carried out at 750℃~800℃ for 10~30 seconds and then rapidly cooled. The high-temperature short-time annealing allows some of the stacking fault defects in the deformed structure inside the first-stage cryogenic rolled plate to be retained as precursors for nanotwin nucleation, while eliminating some of the work hardening in the deformed structure, thus obtaining a high-temperature short-time annealed plate. The high-temperature short-time annealed plate is subjected to two-stage cryogenic rolling in the liquid nitrogen temperature zone. The total deformation is 40% to 60%, and it is divided into 1 to 3 passes. After each pass, the plate is immersed in liquid nitrogen for 10 to 30 minutes. The two-stage cryogenic rolling induces the formation of high-density nanotwins on the nanotwin nucleation precursor. The average width of the nanotwins is 2.13 to 3.47 nm. The nanotwins have twin boundaries, and dislocation walls are also present inside the high-temperature short-time annealed plate, resulting in a two-stage cryogenic rolled plate. The secondary cryogenic rolled plate is subjected to low-temperature aging treatment, which is carried out at 400℃~450℃ for 2~4 hours. The low-temperature aging treatment causes δ-Ni2Si precipitates to precipitate uniformly and be distributed in the matrix, as well as near twin boundaries and dislocation walls, forming a synergistic strengthening with the nanotwins, resulting in Cu-Ni-Si alloy plate and strip with synergistic improvement in strength and plasticity.

2. The method according to claim 1, characterized in that, The total deformation of the first-stage cryogenic rolling is 75%, divided into 5 passes, with liquid nitrogen holding for 30 minutes after each pass; the high-temperature short-time annealing temperature is 780℃, and the holding time is 20 seconds.

3. The method according to claim 1, characterized in that, The cooling method for the high-temperature short-time annealing is air cooling or water cooling.

4. The method according to claim 1, characterized in that, The secondary cryogenic rolling is completed in a single pass, with a total deformation of 50%.

5. The method according to claim 1, characterized in that, The low-temperature aging treatment was performed at a temperature of 420°C for 3 hours.

6. The method according to claim 1, characterized in that, The Cu-Ni-Si alloy strip has a tensile strength of 715.68 MPa, a yield strength of 670 MPa, an elongation of 13.61%, and an electrical conductivity of 51.30% IACS.