A CNC engraving modification process for semiconductor electronic components

By removing microburrs from high-purity tantalum semiconductor workpieces through ion beam grazing etching and magnetron sputtering processes, the problem of surface damage after etching was solved, and the equipment stability and wafer yield were improved in a high vacuum environment.

CN123108474APending Publication Date: 2026-11-17SHIJU TECH (HEFEI) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611553818.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-09
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

High-purity tantalum semiconductor sputtering targets and baffle rings generate micron-level microburrs and subsurface residual tensile stress on their surfaces after CNC etching, leading to the risk of tip discharge. Existing deburring methods are prone to damaging the macroscopic etched structure or introducing chemical contamination.

Method used

A purely physical dry process combining ion beam grazing etching and magnetron sputtering is employed. Ion beam grazing etching is performed in a high-vacuum chamber to remove microburrs, and an amorphous conformal coating is deposited in situ to preserve the macroscopic engraved structure and avoid chemical contamination and grain coarsening.

Benefits of technology

It effectively removes microburrs, reduces the risk of tip discharge, maintains the integrity of the engraved structure, avoids chemical contamination and grain coarsening, and improves equipment stability and wafer yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108474A_ABST
    Figure CN123108474A_ABST
Patent Text Reader

Abstract

This invention discloses a CNC engraving modification process for semiconductor electronic workpieces. This invention relates to the field of semiconductor manufacturing equipment and consumables technology. High-purity tantalum workpieces, after CNC engraving, exhibit microburrs and subsurface damage on their surface, which can easily trigger tip discharge in physical vapor deposition equipment. This invention places the CNC-engraved workpiece in a high-vacuum cavity simultaneously equipped with an inert gas ion source and a magnetron sputtering target. First, the workpiece surface is grazed by ion beam etching at a grazing angle, selectively removing microburrs while preserving the macroscopic engraved groove structure using edge effects. Then, an amorphous conformal coating is deposited in situ to seal microcracks and shield the subsurface damage layer without breaking the vacuum. This invention can be used to prepare vacuum consumables such as semiconductor sputtering targets and baffle rings, reducing the probability of tip discharge and improving process yield.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of semiconductor manufacturing equipment and consumables technology, specifically to a CNC engraving modification process based on semiconductor electronic special workpieces. Background Technology

[0002] In the semiconductor and electronics field, high-purity tantalum with a purity of not less than 99.995% is used as a sputtering target and consumable such as baffle rings in semiconductor physical vapor deposition equipment due to its excellent conductivity, resistance to plasma corrosion, and chemical stability. This field has high requirements for the reliability of the surface treatment process of consumables. During sputtering, target atoms will be deposited in non-target areas such as baffle rings to form anti-sputtering film. In advanced integrated circuit manufacturing, deadly particles attached to the wafer surface can cause device short circuits or open circuits and failure. In order to avoid the formation of deadly particles by peeling off the film, the surface of tantalum workpieces is usually CNC engraved to form a macro-concave-convex groove structure. The film adhesion is improved through mechanical interlocking effect. However, high-purity tantalum has strong plasticity and is easy to stick to the tool. During the engraving process, micron-level microburrs are easy to be generated at the surface edge, and residual tensile stress and lattice distortion layer are formed on the subsurface. Microburrs are easy to trigger tip discharge in the high vacuum and high-energy plasma environment of physical vapor deposition equipment, resulting in wafer scrap. Existing deburring methods mainly include wet chemical etching and high-temperature thermal annealing. Wet chemical etching uses acidic etching solutions to dissolve surface protrusions, but the etching effect is difficult to control precisely, easily damaging the macroscopic engraving outline. Furthermore, tantalum materials are prone to hydrogen embrittlement in acidic environments, and residual etching solutions can cause chemical pollution. High-temperature thermal annealing releases residual stress through high temperatures, but the engraved surface has a high energy storage due to plastic deformation, and abnormal grain growth is prone to occur in this area during annealing, leading to a decrease in the uniformity of the sputtered film. Moreover, it lacks the ability to directly correct the morphology of the microburrs that have already formed. Neither of the above two methods can simultaneously achieve the preservation of the macroscopic engraving structure and the elimination of microburrs and subsurface damage. Summary of the Invention

[0003] The technical problem to be solved by this invention is that after high-purity tantalum semiconductor sputtering targets, baffle rings and other electronic special workpieces are formed into macroscopic mechanical interlocking gripping structures by CNC engraving, micron-level microburrs are inevitably generated on their surface and edges, and residual tensile stress and lattice distortion layers are formed on the subsurface. The above-mentioned microburrs are prone to induce tip discharge in the high vacuum and high-energy plasma environment of semiconductor physical vapor deposition equipment, resulting in wafer scrapping and unplanned equipment downtime. Existing wet chemical etching deburring processes easily damage the macroscopic etched geometry and introduce chemical contamination and hydrogen embrittlement risks. High-temperature thermal annealing to eliminate residual stress can lead to abnormal grain coarsening in this area and disrupt sputtering uniformity. Therefore, the core technical problem to be solved by this invention is: how to eliminate surface microburrs and subsurface processing damage layers using a purely physical dry process while preserving the macroscopic mechanical interlocking gripping geometry formed by CNC etching, fundamentally solving the hidden dangers of tip discharge in high-vacuum plasma environments, without introducing chemical contamination or causing grain coarsening and other side effects. To solve the above technical problems, the present invention provides a CNC engraving modification process based on semiconductor electronic special workpieces, comprising the following steps: A high-purity tantalum workpiece is subjected to CNC engraving to form a macroscopic engraved groove structure on the surface of the workpiece. The surface of the workpiece after processing has microburrs. The workpiece, after being CNC engraved, is loaded onto the workpiece support stage inside the high vacuum chamber. The high vacuum chamber is equipped with an inert gas ion source and a magnetron sputtering target. The high vacuum chamber is sealed and then evacuated. An inert working gas is introduced into the high vacuum chamber, the inert gas ion source is activated, and the ion beam generated by the inert gas ion source is controlled to be incident on the surface of the workpiece at a grazing angle. The surface of the workpiece is subjected to ion beam grazing etching treatment. The edge effect of the ion beam sputtering yield changing with the incident angle is used to selectively etch the microburrs while retaining the macroscopic engraved groove structure. After completing the ion beam grazing etching process, the high vacuum chamber is kept in a vacuum state without breaking the vacuum. The process is switched to the magnetron sputtering mode, and the sputtering power supply corresponding to the magnetron sputtering target is started. An amorphous conformal coating is deposited in situ on the surface of the workpiece. The amorphous conformal coating covers and fills the microcracks remaining on the surface of the workpiece after the ion beam grazing etching process.

[0004] Compared with the prior art, the beneficial effects of the present invention by adopting the above technical solution are as follows: 1. The present invention utilizes the edge effect of sputtering yield variation with local incident angle to selectively etch the microburr side wings by ion beam grazing etching, while basically not producing morphological changes to the macroscopic flat area and the outline of the engraved groove. Therefore, while removing microburrs, the macroscopic engraved groove outline can be basically preserved, avoiding the decrease in specific surface area and gripping ability of the mechanical interlock gripping structure. 2. Since ion beam grazing etching and magnetron sputtering deposition are completed in situ continuously within the same high-vacuum chamber without breaking the vacuum, the entire process is a purely physical dry process that does not involve any acidic chemical reagents. Therefore, the risks of chemical contamination, impurity residue, and hydrogen embrittlement of tantalum materials are avoided. 3. Since the in-situ deposited amorphous conformal coating does not have a long-range ordered lattice structure, it can continuously and uniformly cover and fill the microcracks and pits remaining on the surface after the removal of microburrs, and form a physical shield for the subsurface work hardening and lattice distortion layer below it. Therefore, the workpiece surface is in a relatively uniform and low-stress state. 4. Since the entire process does not involve high-temperature recrystallization, it avoids abnormal grain growth at high temperatures due to high energy storage during plastic deformation on the engraved surface, thus ensuring the uniformity of the thickness and composition of the subsequent sputtered film. 5. Since surface microburrs are effectively eliminated and the subsurface damage layer is effectively shielded, the local electric field concentration coefficient is significantly reduced. Therefore, the probability of tip discharge in the cavity of semiconductor physical vapor deposition equipment can be reduced, which is beneficial to extending the service life of consumables and improving the yield of wafer manufacturing process. Attached Figure Description

[0005] Figure 1 This is a flowchart illustrating the overall process of CNC engraving modification in an embodiment of the present invention. Figure 2 This is a flowchart of the ion beam grazing etching process in an embodiment of the present invention; Figure 3 This is a flowchart of the system processing logic in an embodiment of the present invention. Detailed Implementation

[0006] The following is in conjunction with the appendix Figure 1 -Appendix Figure 3 The specific embodiments of the present invention will be further described below. It should be noted that the description of these embodiments is for the purpose of helping to understand the present invention, but does not constitute a limitation of the present invention.

[0007] To make the technical solutions and advantages of the present invention clearer, the present invention will be further described in detail below with reference to specific embodiments. It should be understood that the specific embodiments described herein are only for explaining the present invention and are not intended to limit the scope of protection of the present invention.

[0008] The composite modification process system upon which this embodiment relies mainly consists of a high vacuum chamber, a workpiece loading and transmission mechanism, an inert gas ion source module, a magnetron sputtering target module, a vacuum pumping system, and a process control system. The high vacuum chamber has a vacuum sealing structure and can be configured with an auxiliary loading chamber connected to the main chamber, which is used to complete the loading and unloading of workpieces without opening the main chamber, thereby reducing the frequency of vacuum failure in the main chamber. An inert gas ion source is installed above or to the side of the high vacuum cavity, with its emission direction pointing towards the surface of the workpiece support stage and forming an adjustable grazing angle with the reference plane of the workpiece support stage. The inert gas ion source has an ion generation region and a grid acceleration structure to control the emission energy and beam density of the ions. The magnetron sputtering target assembly is installed on the other side or above the high vacuum cavity, facing the workpiece support stage. Its target material is high-purity tantalum and is equipped with a magnetron structure and cooling water circuit. The workpiece support stage is located in the center of the high vacuum cavity, used to support the workpiece, and is connected to an external drive motor to achieve rotational motion, so as to ensure uniform coverage of the workpiece surface by the ion beam and sputtered particle stream. A vacuum pumping system is connected to the high vacuum chamber and includes a combination of molecular pumps and mechanical pumps as well as a vacuum gauge to monitor and maintain the vacuum level inside the chamber. The process control system is connected to the inert gas ion source, the sputtering power supply corresponding to the magnetron sputtering target, and the drive mechanism of the workpiece carrier stage, respectively. It is used to perform closed-loop adjustment of parameters such as ion energy, ion beam current, grazing angle, sputtering power, gas partial pressure and processing time. It can also be equipped with a quartz crystal film thickness monitoring device for real-time monitoring of coating deposition thickness.

[0009] The core physical mechanism utilized in this invention is the angle dependence of ion beam physical sputtering, i.e., the edge effect. When low-energy inert gas ions are incident on the engraved surface at a grazing angle relative to the macroscopically flat surface of the workpiece, the engraved surface is not an ideal plane, but is covered with microburr protrusions formed by plastic tearing. The microburr tips have a local slope angle relative to the macroscopically flat surface, which makes the actual incident angle of the ion beam at the microburr side wings different from the actual incident angle at the macroscopically flat area. This leads to a difference in sputtering yield at the two locations, achieving selective etching of the microburrs, while producing basically no observable morphological changes to the macroscopically flat area and the macroscopic engraved groove contour.

[0010] This mechanism can be illustrated by the following sputtering yield angle-dependent model: ; In the formula, Indicates the angle of incidence as Physical sputtering yield at time, i.e., the average number of target atoms sputtered per incident ion; The baseline sputtering yield, representing the vertical incidence of ions, is determined by the ion type, ion energy, and target material. The angle between the direction of ion incident and the direction of the normal to the local surface being bombarded is called the local incident angle. and Empirical fitting parameters related to ion energy and the ion-to-target atom mass ratio can be obtained from publicly available sputtering yield data or experimental calibration.

[0011] Local angle of incidence Macroscopic grazing angle set by the process and the slope angle of local surface morphology The relationship between them can be represented as: ; In the formula, Indicates the surface number The local actual angle of incidence at that location; This indicates the grazing angle set by the ion beam relative to the macroscopically flat surface of the workpiece; Indicates the first The local slope angle of a local surface relative to a macroscopically flat reference surface, when the local surface is tilted toward the ion source. Take positive values ​​in macroscopically flat regions. Approximately zero.

[0012] From the above two equations, it can be seen that the local incident angle at the microburr flank is closer to the higher yield range of the sputtering yield curve than the local incident angle in the macroscopically flat region. Therefore, the edge selective erosion ratio is defined as follows: ; In the formula, This represents the ratio of sputtering yield at microburrs to sputtering yield in macroscopically flat areas, i.e., the edge selectivity coefficient. This represents the sputtering yield calculated based on the local incident angle of the microburr flanks; This represents the sputtering yield calculated based on the local incident angle in a macroscopically flat region. The larger the value, the stronger the selective abrasion ability of the ion beam on microburrs under this set of process parameters, and the better the ability to preserve the morphology of the macroscopic engraved outline.

[0013] Based on the above system and physical mechanism, the specific implementation steps of this embodiment are as follows: First, high-purity tantalum workpiece blanks (sputtering targets or baffle rings) with a purity of not less than 99.995% are subjected to conventional CNC engraving to form a macroscopic engraving groove structure with a set depth and spacing on its surface, forming an initial mechanical interlocking gripping geometry. After processing, the workpiece surface has micron-level microburrs and a subsurface work hardening layer.

[0014] Subsequently, the workpiece that has undergone the above-mentioned engraving process is loaded onto the workpiece support stage of a high-vacuum cavity equipped with an inert gas ion source and a magnetron sputtering target. After sealing the cavity, the vacuum pumping system is activated to evacuate the cavity to a vacuum level not exceeding 5 × 10⁻⁶. -4 The basic vacuum level is set to reduce the interference of residual gas on subsequent processes.

[0015] Next, an inert working gas (argon or krypton) of a set flow rate is introduced into the cavity to maintain the process gas pressure within the cavity at 1×10⁻⁶. -2 Pa to 5×10 -2 Within the Pa range, activate the inert gas ion source, set the ion energy to the range of 500 electron volts to 2000 electron volts, and adjust the grazing angle of the ion beam exit direction relative to the macroscopic surface of the workpiece to the range of 15 degrees to 30 degrees.

[0016] Then, the workpiece support stage is driven to rotate so that the ion beam can uniformly cover the entire engraved surface of the workpiece. According to the process parameter window calculated or experimentally calibrated by the aforementioned edge effect model, the workpiece surface is subjected to ion beam grazing etching treatment, so that the surface microburrs are selectively smoothed and the edge contour tends to be rounded, while the depth and shape of the macroscopic engraved groove remain basically unchanged.

[0017] After completing the above-mentioned ion beam grazing etching, the cavity is kept in a vacuum state without breaking the vacuum or exposing the atmosphere. The process is then switched directly to the magnetron sputtering mode. The sputtering power supply corresponding to the magnetron sputtering target is started, and parameters such as sputtering power, working gas partial pressure, and deposition rate are set. Under the set deposition rate and deposition time conditions, an amorphous conformal coating with a thickness ranging from 20 nanometers to 500 nanometers is deposited in situ on the entire etched surface of the workpiece. This coating has no grain boundaries and no specific crystal orientation. It can continuously and uniformly cover and fill the microcracks and pits remaining on the surface after the aforementioned ion beam etching treatment, and form a physical shield for the subsurface work hardening and lattice distortion layer below it. In this embodiment, the magnetron sputtering target is a high-purity tantalum target, the introduced working gas is argon, and the deposited amorphous conformal coating is a high-purity tantalum coating with the same material as the workpiece. In another embodiment, the magnetron sputtering target is a tantalum target, and the introduced working gas contains nitrogen, so that the deposited amorphous conformal coating is a tantalum nitride coating.

[0018] Finally, after the coating deposition is completed, the inert gas ion source and magnetron sputtering power supply are turned off, and the workpiece is cooled under vacuum or inert gas protection. After cooling to the set temperature, the cavity is opened, the workpiece is unloaded, and the finished product quality is tested for surface morphology, film thickness, and adhesion. The final product is obtained after passing the test. The surface morphology and coating cross-section before and after treatment are compared. After treatment, the cross-section of the workpiece is arranged in layers from the high-purity tantalum substrate layer, the subsurface work hardening and lattice distortion layer that is shielded and covered after treatment, and the in-situ deposited amorphous conformal coating. The layers are physically covered and sealed.

[0019] As a specific example, after CNC engraving of a high-purity tantalum baffle ring workpiece, it is loaded onto the workpiece support stage of the aforementioned high-vacuum cavity and evacuated to a vacuum level of 3×10⁻⁶. -4 Argon gas is then introduced after the pressure is applied, and the process gas pressure in the chamber is controlled to be 2 × 10⁻⁶.-2 Pa, set the ion energy to 1000 electron volts, set the grazing angle to 20 degrees, drive the workpiece carrier to rotate at the set speed, and perform ion beam grazing etching on the workpiece surface. After processing, the process is switched to magnetron sputtering mode without breaking the vacuum. High-purity tantalum target material is used, and sputtering power and deposition rate are set to deposit a 100-nanometer thick high-purity tantalum amorphous conformal coating. Scanning electron microscopy revealed that the microburrs on the surface of the treated workpiece were largely eliminated, the macroscopic engraved groove outlines were preserved intact, and the coating was continuously and uniformly applied to the groove surface and microcrack areas.

[0020] As a preferred embodiment of this invention, before performing ion beam grazing etching on the surface of the workpiece, online surface morphology detection methods (such as laser scattering roughness detection or image recognition detection) can be used to detect and statistically analyze the microburr height parameters on the surface of the CNC-etched workpiece. Based on the obtained height parameters, and according to the aforementioned edge selectivity coefficient calculation model, the grazing angle and ion energy and other process parameters are adjusted in reverse to maintain the edge selectivity coefficient within the set selective etching range. This allows for adaptive ion beam processing window settings for different batches and workpieces with different etching parameters, further improving the consistency of burr removal and the stability of macroscopic structure retention.

[0021] In other alternative implementations, during the ion beam grazing etching stage, the working gas is not limited to pure inert gas, but can also be a mixed atmosphere of inert gas and a small amount of reactive gas (such as nitrogen), so that the ion beam can physically sputter away microburrs while producing an in-situ nitriding modification effect on the newly exposed surface, as a supplement to the in-situ conformal coating deposition process. In the in-situ conformal coating deposition stage, conventional DC magnetron sputtering can be substituted for pulsed high-power magnetron sputtering or ion beam assisted deposition to prepare amorphous layers, thereby obtaining conformal coatings with higher density and stronger adhesion to the substrate. Ion beam bombardment and sputtering deposition particle streams can also be introduced into the cavity simultaneously, so that deburring and leveling and thin film deposition are carried out synchronously in time, as an equivalent alternative to the sequential two-step processing method.

[0022] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit them; Although the present invention has been described in detail through the above embodiments, those skilled in the art should understand that modifications can still be made to the specific embodiments of the present invention, or equivalent substitutions can be made to some technical features, without departing from the spirit and scope of the technical solution of the present invention.

[0023] Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art can make possible changes and modifications without departing from the spirit and scope of the present invention. Therefore, any modifications, equivalent changes and alterations made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention shall fall within the protection scope defined by the claims of the present invention.

Claims

1. A CNC engraving modification process for semiconductor electronic special workpieces, characterized in that: Includes the following steps: A high-purity tantalum workpiece is subjected to CNC engraving to form a macroscopic engraved groove structure on the surface of the workpiece. The surface of the workpiece after processing has microburrs. The workpiece, after being CNC engraved, is loaded onto the workpiece support stage inside the high vacuum chamber. The high vacuum chamber is equipped with an inert gas ion source and a magnetron sputtering target. The high vacuum chamber is sealed and then evacuated. An inert working gas is introduced into the high vacuum chamber, the inert gas ion source is activated, and the ion beam generated by the inert gas ion source is controlled to be incident on the surface of the workpiece at a grazing angle. The surface of the workpiece is subjected to ion beam grazing etching treatment. The edge effect of the ion beam sputtering yield changing with the incident angle is used to selectively etch the microburrs while retaining the macroscopic engraved groove structure. Before performing ion beam grazing etching on the surface of the workpiece, the surface morphology of the workpiece is inspected to obtain the height parameter of the microburrs on the workpiece surface. Based on the height parameter, the grazing angle of the ion beam and the energy of the ions generated by the inert gas ion source are adjusted so that the ratio of the sputtering yield at the microburrs to the sputtering yield in the macroscopic flat area, i.e., the edge selectivity coefficient, is maintained within a preset selective ablation range. After completing the ion beam grazing etching process, the high vacuum chamber is kept in a vacuum state without breaking the vacuum. The process is switched to the magnetron sputtering mode, and the sputtering power supply corresponding to the magnetron sputtering target is started. An amorphous conformal coating is deposited in situ on the surface of the workpiece. The amorphous conformal coating covers and fills the microcracks remaining on the surface of the workpiece after the ion beam grazing etching process.

2. The CNC engraving modification process according to claim 1, characterized in that, The grazing angle of the ion beam is 15 to 30 degrees, and the energy of the ions generated by the inert gas ion source is 500 electron volts to 2000 electron volts.

3. The CNC engraving modification process according to claim 1, characterized in that, The high-vacuum chamber is evacuated to ensure that its vacuum level does not exceed 5 × 10⁻⁶. -4 Pa; the inert working gas is one of argon and krypton; after the inert working gas is introduced, the process gas pressure in the high vacuum chamber is 1×10 Pa. -2 Pa to 5×10 -2 Pa.

4. The CNC engraving modification process according to claim 1, characterized in that, The thickness of the amorphous conformal coating is 20 nanometers to 500 nanometers.

5. The CNC engraving modification process according to claim 1, characterized in that, The magnetron sputtering target is a high-purity tantalum target, and the amorphous conformal coating is a high-purity tantalum coating. The material of the high-purity tantalum coating is the same as that of the workpiece.

6. The CNC engraving modification process according to claim 1, characterized in that, The magnetron sputtering target is a tantalum target, and the working gas introduced after switching to the magnetron sputtering working mode contains nitrogen. The amorphous conformal coating is a tantalum nitride coating.

7. The CNC engraving modification process according to claim 1, characterized in that, During the ion beam grazing etching process on the surface of the workpiece, the workpiece stage is driven to rotate so that the ion beam covers the entire etched surface of the workpiece.

8. The CNC engraving modification process according to claim 1, characterized in that, After CNC engraving of the workpiece and before ion beam grazing etching of the workpiece surface, the surface morphology of the workpiece is inspected to obtain the height parameter of the microburrs; the grazing angle of the ion beam and the energy of the ions generated by the inert gas ion source are adjusted according to the obtained height parameter.

9. The CNC engraving modification process according to any one of claims 1 to 8, characterized in that, The workpiece is at least one of a semiconductor sputtering target and a baffle ring, and the purity of the high-purity tantalum workpiece is not less than 99.995%.