A method, apparatus and electronic equipment for preparing Ti / Cu seed layers by magnetron sputtering
By adjusting the sputtering power ratio of the Ti/Cu target and forming a Ti/Cu atomic mixture or gradient structure, the problem of insufficient interfacial bonding strength in the Ti/Cu bilayer structure is solved, and the bonding strength and thermal stability of the seed layer are improved, making it suitable for semiconductor packaging and electroplating processes.
Patent Information
- Application Number
- CN202611278740.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-21
- Publication Date
- 2026-11-17
AI Technical Summary
In existing Ti/Cu bilayer structures, the interfacial bonding strength and long-term reliability between the Ti layer and the Cu layer are insufficient. In particular, stress concentration is easily generated on flexible or high thermal expansion coefficient substrates, leading to problems such as microcracks, delamination and metal layer desquamation.
By adjusting the sputtering power ratio of Ti target to Cu target, the percentage content of Ti atoms in the seed layer is controlled within the range of 15% to 35%. Co-sputtering or power gradient methods are used to form a Ti/Cu atom mixed structure or a continuous composition gradient structure, which increases the chemical bonding sites between Ti and the substrate and reduces the stress concentration at the interface.
It improves the bonding strength, thermal stability and long-term reliability between the seed layer and the substrate, while taking into account the conductivity of the seed layer and the compatibility with subsequent electroplating.
Smart Images

Figure CN123108485A_ABST
Abstract
Description
Technical Field
[0001] This disclosure relates to the field of semiconductor packaging technology, and more specifically, to a method, apparatus, and electronic device for preparing a Ti / Cu seed layer by magnetron sputtering. Background Technology
[0002] In applications such as semiconductor back-end interconnects, integrated circuit packaging substrates, flexible printed circuit boards, and ceramic substrate metallization, it is often necessary to form copper conductive lines or copper seed layers for subsequent electroplating on the surface of substrates such as silicon, silicon dioxide, polyimide, aluminum nitride ceramics, or epoxy glass fiber composites. Existing technologies typically employ magnetron sputtering to sequentially deposit a Ti adhesion layer and a Cu seed layer, forming a two-layer structure of substrate / Ti layer / Cu layer. The Ti layer improves the adhesion between the metal layer and the substrate, while the Cu layer provides lower conductivity and favorable nucleation conditions for subsequent electroplating.
[0003] However, in existing Ti / Cu bilayer structures, a relatively obvious interface usually forms between the Ti and Cu layers. The interface relies primarily on physical adsorption, limited interatomic interdiffusion, and partial chemical bonding for connection, easily leading to regions with relatively weak interfacial adhesion. When the seed layer undergoes subsequent thick copper plating, hot pressing, reflow soldering, or thermal cycling, stress concentration easily occurs at the interface due to the difference in thermal expansion coefficients between the Cu and Ti layers and the substrate. This can cause problems such as microcracks, delamination, blistering, or metal layer delamination. Especially for flexible substrates or substrates with high thermal expansion coefficients, the interfacial bonding strength and long-term reliability of existing bilayer structures still need improvement. Summary of the Invention
[0004] This disclosure provides at least one method, apparatus, and electronic device for preparing a Ti / Cu seed layer by magnetron sputtering. By adjusting the sputtering power ratio of the Ti target to the Cu target, the percentage content of Ti atoms in the seed layer is controlled within a preset range. A Ti / Cu atom mixed structure or a continuous composition gradient structure is formed by co-sputtering or power gradient. This can increase the chemical bonding sites between Ti and the substrate, reduce interfacial stress concentration, improve the bonding strength, thermal stability, and long-term reliability between the seed layer and the substrate, and take into account the conductivity of the seed layer and the compatibility of subsequent electroplating.
[0005] This disclosure provides a method for preparing a Ti / Cu seed layer by magnetron sputtering, including: The substrate to be deposited was placed in a vacuum chamber, and the relationship between the sputtering power ratio of Ti target and Cu target and the percentage content of Ti atoms was obtained. Ar working gas is introduced into the vacuum chamber, and independently adjustable sputtering power is applied to the Ti target and Cu target respectively; Adjust the power ratio between the Ti target and the Cu target according to the corresponding relationship, and form a Ti / Cu seed layer on the substrate surface by co-sputtering or power gradient method, so that the Ti / Cu seed layer forms an atomic mixed structure or a composition gradient structure that changes continuously along the thickness direction; The percentage content of Ti atoms in the Ti / Cu seed layer is controlled within the range of 15% to 35%, and the total thickness of the Ti / Cu seed layer is 40 to 150 nm.
[0006] In an optional implementation, the method further includes, before applying independently adjustable sputtering power to the Ti target and the Cu target respectively: The vacuum chamber is evacuated to a background pressure not exceeding 5 × 10⁻⁶. -5 Pa; Ar gas is introduced into the vacuum chamber, and the substrate is subjected to Ar plasma cleaning to remove oxides and organic contaminants from the surface of the substrate. The Ar plasma cleaning process involves a power of 50–150 W, a cleaning time of 5–15 min, and a cleaning pressure of 0.5–1 Pa.
[0007] In one optional implementation, obtaining the correspondence between the sputtering power ratio of the Ti target and the Cu target and the percentage content of Ti atoms includes: Under conditions of fixed total power or fixed total deposition time, multiple calibration samples were prepared according to different power ratios of Ti target to Cu target; Elemental analysis of the calibration sample was performed using energy-dispersive X-ray spectroscopy or X-ray photoelectron spectroscopy. A calibration curve was established based on the elemental analysis results, relating the power ratio of Ti targets to Cu targets and the percentage content of Ti atoms. The power ratio of the Ti target to the Cu target is 0.2 to 0.8, and the percentage content of Ti atoms is 20% to 30%.
[0008] In one optional embodiment, a Ti / Cu seed layer is formed on the substrate surface by co-sputtering, comprising: During the deposition process, the Ti target power and Cu target power are kept constant to form a Ti / Cu seed layer with a uniform mixture of Ti atoms and Cu atoms; The thickness of the Ti / Cu seed layer is 50–120 nm, and the deposition time is 1–5 min.
[0009] In one optional implementation, a Ti / Cu seed layer is formed on the substrate surface in a power gradient manner, comprising: During the initial deposition phase, within a thickness range of 20% to 30% of the total thickness of the Ti / Cu seed layer, the Ti target power is increased and the Cu target power is decreased to form a Ti-rich region close to the substrate. Subsequently, the Ti target power is gradually reduced along the deposition time or thickness direction while the Cu target power is increased simultaneously to form a Cu-rich region near the surface of the seed layer; The percentage of Ti atoms in the Ti / Cu seed layer gradually decreases from 30% near the substrate to less than 10% near the surface.
[0010] In one alternative implementation, a negative bias is applied to the substrate during magnetron sputtering; The negative bias voltage is a DC bias voltage or pulse bias voltage of -60 to -150V, which promotes the intermixing of Ti atoms and Cu atoms at the substrate interface and improves the density of the seed layer.
[0011] In one optional implementation, after deposition is completed, the Ti target power supply, Cu target power supply and negative bias power supply are turned off, and the substrate is cooled to room temperature in a vacuum environment or a low-pressure Ar protective atmosphere. After the Ti / Cu seed layer is deposited and exits the cavity, the Ti / Cu seed layer is subjected to Ar plasma surface activation treatment. The power of the surface activation treatment is 20-50W and the treatment time is 1-3min.
[0012] This disclosure also provides a magnetron sputtering apparatus for preparing a Ti / Cu seed layer, comprising: The substrate loading module is used to place the substrate to be deposited in a vacuum chamber and obtain the relationship between the sputtering power ratio of Ti target and Cu target and the percentage content of Ti atoms. The sputtering power application module is used to introduce Ar working gas into the vacuum chamber and apply independently adjustable sputtering power to the Ti target and Cu target respectively. A co-sputtering or gradient deposition module is used to adjust the power ratio between the Ti target and the Cu target according to the corresponding relationship, and to form a Ti / Cu seed layer on the substrate surface in a co-sputtering mode or a power gradient mode, so that the Ti / Cu seed layer forms an atomic mixed structure or a composition gradient structure that changes continuously along the thickness direction; wherein, the percentage content of Ti atoms in the Ti / Cu seed layer is controlled in the range of 15% to 35%, and the total thickness of the Ti / Cu seed layer is 40 to 150 nm.
[0013] This disclosure also provides an electronic device, including: a processor, a memory, and a bus. The memory stores machine-readable instructions executable by the processor. When the electronic device is running, the processor communicates with the memory via the bus. When the machine-readable instructions are executed by the processor, they perform the steps of the above-described magnetron sputtering preparation method for Ti / Cu seed layers, or any possible implementation of the above-described magnetron sputtering preparation method for Ti / Cu seed layers.
[0014] This disclosure also provides a computer-readable storage medium storing a computer program that, when executed by a processor, performs the steps of the magnetron sputtering preparation method for the Ti / Cu seed layer described above, or any possible implementation of the magnetron sputtering preparation method for the Ti / Cu seed layer described above.
[0015] This disclosure also provides a computer program product, including a computer program / instructions, which, when executed by a processor, implements the magnetron sputtering preparation method for the Ti / Cu seed layer described above, or any possible implementation of the magnetron sputtering preparation method for the Ti / Cu seed layer described above.
[0016] This disclosure provides a magnetron sputtering preparation method, apparatus, and electronic device for Ti / Cu seed layers. By adjusting the sputtering power ratio of the Ti target to the Cu target, the percentage content of Ti atoms in the seed layer is controlled within a preset range. A Ti / Cu atom mixed structure or a continuous composition gradient structure is formed by co-sputtering or power gradient. This can increase the chemical bonding sites between Ti and the substrate, reduce interfacial stress concentration, improve the bonding strength, thermal stability, and long-term reliability between the seed layer and the substrate, and also take into account the conductivity of the seed layer and the compatibility of subsequent electroplating.
[0017] To make the above-mentioned objects, features and advantages of this disclosure more apparent and understandable, preferred embodiments are described below in detail with reference to the accompanying drawings. Attached Figure Description
[0018] To more clearly illustrate the technical solutions of the embodiments of this disclosure, the accompanying drawings used in the embodiments will be briefly described below. These drawings are incorporated in and constitute a part of this specification. They illustrate embodiments conforming to this disclosure and, together with the specification, serve to explain the technical solutions of this disclosure. It should be understood that the following drawings only show some embodiments of this disclosure and should not be considered as limiting the scope. Those skilled in the art can obtain other related drawings based on these drawings without creative effort.
[0019] Figure 1A flowchart of a magnetron sputtering method for preparing a Ti / Cu seed layer according to an embodiment of this disclosure is shown; Figure 2 A side view of a vacuum chamber provided in an embodiment of this disclosure is shown; Figure 3 A cross-sectional schematic diagram of a Ti / Cu seed layer prepared according to an embodiment of this disclosure is shown; Figure 4 A schematic diagram of a magnetron sputtering apparatus for preparing a Ti / Cu seed layer provided in an embodiment of this disclosure is shown; Figure 5 A schematic diagram of an electronic device provided in an embodiment of the present disclosure is shown. Detailed Implementation
[0020] To make the objectives, technical solutions, and advantages of the embodiments of this disclosure clearer, the technical solutions of the embodiments of this disclosure will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of this disclosure, and not all of them. The components of the embodiments of this disclosure described and shown in the accompanying drawings can generally be arranged and designed in various different configurations. Therefore, the following detailed description of the embodiments of this disclosure provided in the accompanying drawings is not intended to limit the scope of the claimed disclosure, but merely represents selected embodiments of this disclosure. All other embodiments obtained by those skilled in the art based on the embodiments of this disclosure without inventive effort are within the scope of protection of this disclosure.
[0021] It should be noted that similar labels and letters in the following figures indicate similar items. Therefore, once an item is defined in one figure, it does not need to be further defined and explained in subsequent figures.
[0022] In this document, the term "and / or" merely describes a relationship, indicating that three relationships can exist. For example, A and / or B can represent three cases: A alone, A and B simultaneously, and B alone. Furthermore, the term "at least one" in this document means any combination of at least two of any one or more elements. For example, including at least one of A, B, and C can mean including any one or more elements selected from the set consisting of A, B, and C.
[0023] Research has revealed that in existing Ti / Cu bilayer structures, a relatively distinct interface typically forms between the Ti and Cu layers. The interface relies primarily on physical adsorption, limited interatomic interdiffusion, and partial chemical bonding for connection, easily leading to regions with relatively weak interfacial adhesion. When the seed layer undergoes subsequent thick copper plating, hot pressing, reflow soldering, or thermal cycling, the difference in thermal expansion coefficients between the Cu and Ti layers and the substrate can easily cause stress concentration at the interface, leading to problems such as microcracks, delamination, blistering, or metal layer delamination. Especially for flexible substrates or substrates with high thermal expansion coefficients, the interfacial bonding strength and long-term reliability of existing bilayer structures still need improvement.
[0024] Based on the above research, this disclosure provides a magnetron sputtering preparation method, apparatus, and electronic device for Ti / Cu seed layers. By adjusting the sputtering power ratio of the Ti target to the Cu target, the percentage content of Ti atoms in the seed layer is controlled within a preset range. A Ti / Cu atom mixed structure or a continuous composition gradient structure is formed by co-sputtering or power gradient. This can increase the chemical bonding sites between Ti and the substrate, reduce interfacial stress concentration, improve the bonding strength, thermal stability, and long-term reliability between the seed layer and the substrate, and take into account the conductivity of the seed layer and the compatibility of subsequent electroplating.
[0025] To facilitate understanding of this embodiment, a magnetron sputtering method for preparing a Ti / Cu seed layer disclosed in this disclosure will first be described in detail. The execution entity of the magnetron sputtering method for preparing a Ti / Cu seed layer provided in this disclosure is generally a computer device with certain computing capabilities. This computer device may include, for example, a terminal device, a server, or other processing equipment. The terminal device can be a user equipment (UE), mobile device, user terminal, terminal, cellular phone, cordless phone, personal digital assistant (PDA), handheld device, computing device, vehicle-mounted device, wearable device, etc. In some possible implementations, the magnetron sputtering method for preparing a Ti / Cu seed layer can be implemented by a processor calling computer-readable instructions stored in memory.
[0026] See Figure 1 The diagram shows a flowchart of a magnetron sputtering method for preparing a Ti / Cu seed layer according to an embodiment of this disclosure. The method includes steps S101 to S103, wherein: S101. Place the substrate to be deposited in a vacuum chamber and obtain the relationship between the sputtering power ratio of Ti target and Cu target and the percentage content of Ti atoms.
[0027] In practice, before depositing the Ti / Cu seed layer, the substrate to be deposited is placed in the vacuum chamber of the magnetron sputtering equipment. The vacuum chamber is equipped with a substrate holder for supporting the substrate; this holder can be a rotating holder and / or a heated holder to rotate the substrate or regulate its temperature. The vacuum chamber also contains a Ti target, a Cu target, an Ar gas inlet assembly, and independent power control units for controlling the sputtering power of the Ti and Cu targets, respectively. The Ti and Cu targets can each use independent DC magnetron sputtering power supplies, or, depending on the thin film deposition requirements, a DC power supply, an RF power supply, or a combination of DC and RF power supplies.
[0028] Here, the substrate to be deposited can be selected according to the application scenario of the seed layer, including at least one of single-crystal silicon substrate, thermally oxidized silicon substrate, polyimide substrate, aluminum nitride ceramic substrate, and epoxy / glass fiber composite substrate. During substrate loading, the surface to be deposited on the substrate is oriented towards the Ti target and the Cu target so that Ti atoms generated by sputtering from the Ti target and Cu atoms generated by sputtering from the Cu target are co-deposited onto the substrate surface.
[0029] Furthermore, after the substrate is loaded, the mechanical pump and molecular pump corresponding to the vacuum chamber are activated to evacuate the vacuum chamber, so that the background pressure of the vacuum chamber does not exceed 5 × 10⁻⁶. -5 To reduce contamination of the deposition interface by water vapor, oxygen, and volatile organic compounds, a set background vacuum is established. After reaching this vacuum level, high-purity Ar gas is introduced into the vacuum chamber. The purity of the Ar gas can be no less than 99.999%.
[0030] In one embodiment, the substrate is cleaned with Ar plasma before formal deposition. Specifically, Ar gas is introduced into a vacuum chamber, and the cleaning power is set to 50–150 W, the cleaning time to 5–15 min, and the cleaning pressure to 0.5–1 Pa. The Ar plasma bombards the substrate surface to remove oxides, organic contaminants, and other adsorbed impurities, and to activate the substrate surface. The cleaned substrate surface has high surface activity, which is beneficial for the subsequent deposition of Ti atoms to form Ti-O bonds, Ti-N bonds, or other interfacial bonding structures with the substrate surface.
[0031] It should be noted that, in order to ensure that the percentage of Ti atoms in the Ti / Cu seed layer is within the target range, it is necessary to obtain the correspondence between the sputtering power ratio of the Ti target and the Cu target and the percentage of Ti atoms in the deposited film beforehand. Since factors such as the target size, magnetic field strength, target-substrate distance, target utilization status, and equipment structure of the Ti and Cu targets will affect the corresponding sputtering rate, the power ratio can be calibrated for specific magnetron sputtering equipment.
[0032] Specifically, while maintaining consistent substrate type, substrate location, working gas type, working pressure, and other deposition conditions, multiple different sputtering power ratios for Ti and Cu targets were set, and corresponding calibration samples were prepared for each. The power ratio of the Ti and Cu targets could be set within the range of 0.2 to 0.8. For each set of calibration samples, the total power of the Ti and Cu targets could be fixed, the total deposition time could be fixed, or both the total power and the total deposition time could be fixed simultaneously to reduce the influence of variables other than the power ratio on the calibration results.
[0033] Furthermore, after completing the preparation of calibration samples, energy dispersive X-ray spectroscopy (EDS), X-ray photoelectron spectroscopy (XPS) or other component analysis methods are used to detect the Ti and Cu element content in each calibration sample, calculate the percentage Ti atom content in each calibration sample, and establish a calibration curve or corresponding relationship table between the sputtering power ratio of Ti target and Cu target and the percentage Ti atom content.
[0034] The percentage content of Ti atoms can be determined based on the ratio of the number of Ti atoms to the total number of Ti and Cu atoms.
[0035] Based on the calibration curve or corresponding table, the Ti target power and Cu target power corresponding to the target Ti atomic percentage are determined. In one embodiment, the target Ti atomic percentage is set to 20%–30%, the Ti target power can be set to 80–120 W, the Cu target power can be set to 180–280 W, and the deposition rate can be controlled at 0.4–0.8 nm / s.
[0036] It should be noted that the above power parameters are only a typical embodiment, and can be adjusted according to the target size, magnetic field strength, target-substrate distance, working pressure and equipment structure in actual use.
[0037] This allows for the establishment of a correlation between sputtering power parameters and the actual composition of the thin film before formal deposition. This enables subsequent control of the Ti atom percentage in the Ti / Cu seed layer by adjusting the power ratio of the Ti target to the Cu target. Compared to deposition based solely on a fixed Ti layer thickness, this calibration process reduces compositional deviations between different equipment and batch processes, providing a technological basis for the subsequent formation of Ti / Cu atom mixed structures or continuous compositional gradient structures.
[0038] As one possible implementation method, see Figure 2 The image shown is a side view of a vacuum chamber provided in an embodiment of this disclosure. Figure 2 As shown, the magnetron sputtering equipment includes a vacuum chamber and Ti target, Cu target, substrate fixture and substrate to be deposited disposed in the vacuum chamber.
[0039] In practice, Ti and Cu targets are positioned on opposite sides of the vacuum chamber, with both targets facing the substrate fixture in the center. This allows Ti atoms sputtered from the Ti target and Cu atoms sputtered from the Cu target to co-fly towards the substrate and deposit on the substrate surface. The Ti and Cu targets can be arranged at an angle relative to the substrate fixture, creating overlapping deposition areas on the substrate surface. This promotes the co-deposition of Ti and Cu atoms and ensures uniform mixing of their components.
[0040] Here, the substrate fixture is positioned in the central region between the Ti target and the Cu target, and the substrate to be deposited is fixedly mounted on the substrate fixture. The substrate fixture can be configured as a rotatable structure, driving the substrate to rotate around a preset rotation axis during the deposition process. This allows different regions of the substrate to sequentially pass through the sputtering regions corresponding to the Ti and Cu targets, thereby improving the deposition uniformity of Ti and Cu atoms on the substrate surface and reducing film thickness deviations caused by differences in target positions. The substrate fixture can also be equipped with a heating structure for temperature control of the substrate.
[0041] Here, a negative bias power supply is positioned below the substrate fixture and electrically connected to the substrate fixture and / or the substrate. During deposition, the negative bias power supply applies a negative DC bias or a pulsed negative bias to the substrate, causing Ar+ ions formed in the vacuum chamber to move towards the substrate under the influence of the electric field and bombard the substrate surface. Ar+ bombardment can enhance the migration ability of deposited atoms on the substrate surface, promote the mixing of Ti and Cu atoms at the substrate interface, and help improve the compactness of the Ti / Cu seed layer and reduce columnar crystal defects.
[0042] Furthermore, the Ar gas inlet and mass flow controller are located on the side of the vacuum chamber and communicate with the interior of the vacuum chamber. Ar gas enters the vacuum chamber after its flow rate is regulated by the mass flow controller to create a stable working atmosphere within the vacuum chamber. The mass flow controller can adjust the Ar gas supply according to the set working pressure and deposition process to maintain the working pressure within the vacuum chamber within a preset range.
[0043] Furthermore, independent power control units are located at the top or side of the vacuum chamber and connected to the Ti and Cu targets respectively. These independent power control units can be DC power control units, RF power control units, or a combination of DC and RF power control units, used to separately control the sputtering power of the Ti and Cu targets, enabling them to operate according to a set power ratio. By adjusting the power of the Ti and Cu targets separately, the relative content of Ti and Cu atoms deposited on the substrate surface can be controlled. In co-sputtering mode, the Ti and Cu target powers can be kept relatively stable; in power gradient mode, the Ti target power can be gradually decreased while the Cu target power is simultaneously increased according to a set time relationship.
[0044] Furthermore, a vacuum system is located at the bottom of the vacuum chamber or connected to the lower part of the vacuum chamber. The vacuum system may include mechanical pumps and molecular pumps, used to evacuate the vacuum chamber before deposition and maintain the working pressure inside the vacuum chamber during deposition. By evacuating the vacuum chamber to a preset base vacuum through the vacuum system, the impact of residual oxygen, water vapor, and organic contaminants on the substrate surface and the Ti / Cu seed layer interface can be reduced.
[0045] During operation, the vacuum chamber is first evacuated using a vacuum system, and Ar gas is introduced into the chamber through an Ar gas inlet and a mass flow controller. Subsequently, independent power control units provide sputtering power to the Ti and Cu targets respectively, forming plasma within the vacuum chamber. Ar+ ions in the plasma bombard the Ti and Cu targets, causing Ti and Cu atoms on their surfaces to travel along their respective sputtering trajectories towards the substrate. Simultaneously, a negative bias power supply applies a negative bias to the substrate, promoting Ar+ ions to move towards the substrate surface and enhancing surface migration and interfacial mixing of deposited atoms. The substrate is rotated by a substrate fixture, causing Ti and Cu atoms to form a uniform Ti / Cu atom mixed layer or a continuous composition gradient seed layer on the substrate surface.
[0046] S102. Ar working gas is introduced into the vacuum chamber to apply independently adjustable sputtering power to the Ti target and Cu target respectively.
[0047] In practice, after the vacuum chamber reaches the set background vacuum, high-purity Ar gas is introduced into the vacuum chamber through the gas inlet assembly. The purity of the Ar gas can be no less than 99.999%, and the supply of Ar gas is adjusted by a mass flow controller to maintain a stable gas environment within the vacuum chamber.
[0048] Preferably, before the formal deposition of the Ti / Cu seed layer, the substrate to be deposited is plasma-cleaned using introduced Ar gas. Specifically, the pressure in the vacuum chamber is adjusted to 0.5–1 Pa, and a cleaning power of 50–150 W is applied for continuous cleaning for 5–15 minutes, causing the Ar gas to form plasma within the vacuum chamber. The Ar+ ions in the plasma bombard the substrate surface to remove oxides, organic contaminants, and other adsorbed impurities, while simultaneously activating the substrate surface to form an active surface conducive to Ti atom deposition and interfacial bonding.
[0049] Here, after substrate cleaning is completed, the working pressure in the vacuum chamber is adjusted to 0.4–0.7 Pa, preferably 0.5 Pa, and independently adjustable sputtering power is applied to the Ti target and Cu target respectively. The Ti target and Cu target are respectively connected to independent power control units, which can be DC power control units, RF power control units, or a combination of DC and RF power control units.
[0050] Specifically, during the sputtering process, Ar+ ions in the Ar plasma bombard the Ti and Cu targets, causing Ti atoms on the Ti target surface and Cu atoms on the Cu target surface to be sputtered from their respective target surfaces and move towards the substrate, eventually depositing on the substrate surface. By adjusting the sputtering power of the Ti and Cu targets respectively, the sputtering rates of Ti and Cu atoms and the atomic flux reaching the substrate surface can be changed, thereby adjusting the relative content of Ti and Cu atoms in the Ti / Cu seed layer.
[0051] During co-sputtering, the Ti and Cu targets operate simultaneously, with their respective power levels maintained at set values. This allows Ti and Cu atoms to be deposited synchronously on the substrate surface, forming a Ti / Cu atom hybrid structure. The power ratio of the Ti to Cu targets can be determined based on a pre-established relationship between sputtering power ratio and Ti atom percentage, and can be set within the range of 0.2 to 0.8. By adjusting the power ratio of the Ti to Cu targets, the Ti atom percentage in the formed Ti / Cu seed layer is controlled within the range of 15% to 35%, preferably within the range of 20% to 30%.
[0052] In a typical embodiment, the sputtering power of the Ti target is set to 80–120 W, and the sputtering power of the Cu target is set to 180–280 W, with the deposition rate of the resulting thin film controlled at 0.4–0.8 nm / s. These power parameters can be adjusted according to the target size of the Ti and Cu targets, the magnetic field strength, the target-substrate distance, the target condition, and the structure of the magnetron sputtering equipment.
[0053] During power gradient deposition, the Ti and Cu targets employ independent power control methods. In the initial deposition phase, the sputtering power of the Ti target is increased, or maintained at a relatively high level, while the Cu target power is kept at a relatively low level, to ensure a higher Ti content in the deposition region near the substrate. As deposition progresses, the sputtering power of the Ti target is gradually decreased, while the sputtering power of the Cu target is simultaneously increased, creating a continuous compositional gradient in the Ti / Cu seed layer along its thickness, transitioning from a Ti-rich region to a Cu-rich region.
[0054] Thus, by performing Ar plasma cleaning on the substrate before formal deposition and independently adjusting the sputtering power of the Ti and Cu targets during the deposition process, precise control of the Ti / Cu seed layer composition and composition gradient can be achieved while improving the cleanliness and activity of the substrate surface.
[0055] Therefore, a higher Ti content near the substrate side is beneficial for increasing the interfacial bonding sites between Ti and the substrate, while a higher Cu content near the seed layer surface is beneficial for reducing surface resistance and improving nucleation and filling performance in subsequent electroplating processes.
[0056] S103. Adjust the power ratio between the Ti target and the Cu target according to the corresponding relationship, and form a Ti / Cu seed layer on the substrate surface by co-sputtering or power gradient method, so that the Ti / Cu seed layer forms an atomic mixed structure or a composition gradient structure that changes continuously along the thickness direction; wherein, the percentage content of Ti atoms in the Ti / Cu seed layer is controlled in the range of 15% to 35%, and the total thickness of the Ti / Cu seed layer is 40 to 150 nm.
[0057] In practice, after the sputtering power ratio of Ti target and Cu target is calibrated, the power combination of Ti target and Cu target is determined from the calibration curve or corresponding table according to the percentage content of Ti atoms in the target. The sputtering power of Ti target and Cu target is adjusted by an independent power control unit to form a Ti / Cu seed layer on the substrate surface.
[0058] Here, in co-sputtering, both the Ti and Cu targets are activated simultaneously, allowing Ti and Cu atoms to reach the substrate surface together in the same deposition stage. By maintaining the power ratio of the Ti and Cu targets within a preset range, Ti and Cu atoms form an atomically hybrid structure or a nanoscale mixed grain structure during deposition, rather than forming Ti and Cu layers with abrupt interfaces. During co-sputtering, the power of the Ti and Cu targets can be kept constant or finely adjusted within permissible process fluctuations to maintain the overall compositional stability of the Ti / Cu seed layer.
[0059] Preferably, the deposition time is 1 to 5 minutes.
[0060] Here, under the power gradient mode, the sputtering power of the Ti target and Cu target is changed according to a preset power change curve, so that the Ti / Cu seed layer forms a continuously varying compositional gradient structure along the thickness direction. Specifically, in the initial stage of deposition, the Ti target power is increased and the Cu target power is decreased, so that a Ti-rich region with a relatively high Ti content is formed on the side closer to the substrate; as the deposition thickness increases, the Ti target power is gradually decreased and the Cu target power is increased simultaneously, so that a Cu-rich region with a relatively high Cu content is gradually formed on the side farther from the substrate.
[0061] In one embodiment, the initial deposition corresponds to 20%–30% of the total thickness of the Ti / Cu seed layer. Within this thickness range, a higher Ti target power is set to achieve a Ti content of approximately 30% or higher than that in the middle of the seed layer near the substrate. Subsequently, the Ti target power is linearly reduced along the deposition time or deposition thickness direction, while the Cu target power is simultaneously increased, causing the Ti content to gradually decrease and the Cu content to gradually increase. A Cu-rich region with a Ti content of less than 10% can be formed near the surface of the seed layer to meet the requirements of subsequent electroplating for conductivity and copper nucleation performance.
[0062] In the co-sputtering or power gradient methods, the percentage of Ti atoms in the Ti / Cu seed layer is controlled within the range of 15% to 35%, preferably within the range of 20% to 30%, by adjusting the power ratio between the Ti target and the Cu target. For the compositional gradient structure formed by power gradient, the percentage of Ti atoms can be determined based on the overall composition of the seed layer, the average composition within a preset thickness range, or the compositional distribution along the thickness direction, so that the seed layer as a whole meets the preset Ti content requirements.
[0063] It should be noted that the total thickness of the Ti / Cu seed layer is 40–150 nm, preferably 50–120 nm. The specific thickness of the seed layer can be set according to the substrate material, subsequent electroplating thickness, conductivity requirements, and interface bonding strength requirements. When the seed layer is formed using a power gradient method, the Ti-rich region near the substrate, the Ti / Cu mixed region in the middle, and the Cu-rich region near the surface together constitute the Ti / Cu seed layer within the total thickness range.
[0064] Furthermore, during the deposition process, a DC negative bias voltage of -60 to -150V or a pulsed negative bias voltage can be applied to the substrate to promote Ar+ bombardment of the substrate surface and the deposited area, thereby improving the surface migration ability of Ti and Cu atoms and the degree of interfacial mixing. Negative bias-assisted deposition can form an atomic mixing transition region of approximately 2–8 nm between the substrate and the Ti / Cu seed layer, improving the density of the seed layer and reducing columnar crystal defects.
[0065] The resulting Ti / Cu seed layer has a higher Ti content on the side closer to the substrate, which is beneficial for Ti to form interfacial bonding structures such as Ti-O bonds and Ti-N bonds with oxygen or nitrogen elements on the substrate surface. The Ti / Cu mixed region in the middle can buffer the thermal expansion mismatch stress between the substrate and the Cu layer. The side closer to the seed layer surface has a higher Cu content, which can provide a lower surface resistance and a nucleation surface suitable for subsequent copper electroplating, thus taking into account the interfacial bonding performance, stress buffering performance, conductivity and electroplating compatibility of the seed layer.
[0066] As one possible implementation, after accumulation, the target power supply and bias voltage are turned off, and the surface is naturally cooled to room temperature in a vacuum or low-pressure Ar protective atmosphere to avoid surface oxidation. After 10–20 minutes, the vacuum is broken and the seed layer is removed. The resulting seed layer is an alloy or gradient structure with controllable Ti content, forming a strong chemically bonded transition region with the substrate at the bottom, a stress-buffered mixed phase in the middle, and a Cu-rich low-resistivity surface at the top. After exiting the cavity, low-power Ar plasma surface activation can be performed, with a power of 20–50 W and a processing time of 1–3 minutes.
[0067] See Figure 3 The diagram shown is a cross-sectional schematic of a Ti / Cu seed layer prepared according to an embodiment of this disclosure.
[0068] like Figure 3 As shown, the seed layer formed in this embodiment is disposed on the substrate surface and consists of a Ti-Cu mixing region and / or a Ti-Cu composition gradient region. Unlike the conventional abrupt bilayer structure of substrate / Ti / Cu layer, the seed layer is disposed on the substrate surface and consists of a Ti-Cu mixing region and / or a Ti-Cu composition gradient region. Unlike the conventional abrupt bilayer structure of substrate / Ti / Cu layer, the Ti and Cu elements exhibit atomic-level mixing or continuous variation along the thickness direction of the seed layer, and there is no obvious Ti / Cu abrupt interface between the substrate and the Cu-rich surface.
[0069] On the side closer to the substrate, a Ti-rich region with a relatively high Ti content is formed. This region can be formed by co-sputtering to create a mixed Ti and Cu atom structure, or by power gradient deposition to create a bottom region with a high Ti content. In one embodiment, the Ti content on the side closer to the substrate is approximately 30 at%, so that more Ti atoms are distributed near the substrate interface. For substrates containing oxygen or nitrogen, Ti atoms can form Ti-O bonds, Ti-N bonds, and other chemical bonding structures with oxygen or nitrogen elements on the substrate surface, thereby improving the interfacial bonding strength between the seed layer and the substrate.
[0070] An interfacial mixing transition region is formed at the interface between the substrate and the Ti / Cu seed layer. This interfacial mixing transition region is formed by the interdiffusion or mixing of substrate material, Ti atoms, and Cu atoms, and its thickness can be approximately 2–8 nm. This transition region can reduce the abrupt change in composition between the substrate and the metal seed layer, reduce stress concentration at traditional abrupt interfaces, and buffer the thermal expansion mismatch stress between the substrate and the upper metal layer.
[0071] Along the direction away from the substrate, the Ti content gradually decreases while the Cu content gradually increases, thus forming a continuous Ti-Cu composition gradient. In the power-gradient deposition method, by gradually decreasing the Ti target power while simultaneously increasing the Cu target power, the percentage of Ti atoms gradually decreases from a higher value near the substrate to less than 10 at% near the surface, while the Cu content correspondingly increases. This results in a compositional distribution within the seed layer that continuously transitions from a Ti-rich region to a Cu-rich region.
[0072] A Cu-rich surface region is formed at the top of the seed layer. This Cu-rich surface region has a high Cu content and a low Ti content, which can reduce the contact resistance of the seed layer surface and provide a continuous and uniform conductive surface and electroplating nucleation interface for subsequent copper electroplating, thereby improving the uniformity of copper layer deposition and reducing defects such as voids.
[0073] The total thickness of the seed layer in this application is 40–150 nm, preferably 50–120 nm, and the percentage of Ti atoms is controlled within the range of 15%–35%, preferably 20%–30%. When co-sputtering is used, Ti and Cu form an atomic-level mixed structure in the seed layer; when power gradient is used, Ti and Cu form a continuous composition gradient along the thickness direction of the seed layer.
[0074] Those skilled in the art will understand that, in the above-described method of the specific implementation, the order in which each step is written does not imply a strict execution order and does not constitute any limitation on the implementation process. The specific execution order of each step should be determined by its function and possible internal logic.
[0075] Based on the same inventive concept, this disclosure also provides a magnetron sputtering preparation apparatus for Ti / Cu seed layers corresponding to the magnetron sputtering preparation method for Ti / Cu seed layers. Since the principle of the apparatus in this disclosure for solving the problem is similar to the magnetron sputtering preparation method for Ti / Cu seed layers described above, the implementation of the apparatus can refer to the implementation of the method, and the repeated parts will not be described again.
[0076] Please see Figure 4 , Figure 4 This is a schematic diagram of a magnetron sputtering apparatus for preparing a Ti / Cu seed layer according to an embodiment of this disclosure. Figure 4 As shown in the figure, the magnetron sputtering preparation apparatus 400 for Ti / Cu seed layers provided in this embodiment includes: The substrate loading module 410 is used to place the substrate to be deposited in a vacuum chamber and obtain the correspondence between the sputtering power ratio of Ti target and Cu target and the percentage content of Ti atoms.
[0077] The sputtering power application module 420 is used to introduce Ar working gas into the vacuum chamber and apply independently adjustable sputtering power to the Ti target and Cu target respectively.
[0078] The co-sputtering or gradient deposition module 430 is used to adjust the power ratio between the Ti target and the Cu target according to the corresponding relationship, and to form a Ti / Cu seed layer on the substrate surface in a co-sputtering mode or a power gradient mode, so that the Ti / Cu seed layer forms an atomic mixed structure or a composition gradient structure that changes continuously along the thickness direction; wherein, the percentage content of Ti atoms in the Ti / Cu seed layer is controlled in the range of 15% to 35%, and the total thickness of the Ti / Cu seed layer is 40 to 150 nm.
[0079] The processing flow of each module in the device and the interaction flow between each module can be referred to the relevant descriptions in the above method embodiments, and will not be detailed here.
[0080] This disclosure provides a magnetron sputtering method and apparatus for preparing a Ti / Cu seed layer. By adjusting the sputtering power ratio of the Ti target to the Cu target, the percentage content of Ti atoms in the seed layer is controlled within a preset range. A Ti / Cu atom mixed structure or a continuous composition gradient structure is formed by co-sputtering or power gradient. This can increase the chemical bonding sites between Ti and the substrate, reduce interfacial stress concentration, improve the bonding strength, thermal stability and long-term reliability between the seed layer and the substrate, and take into account the conductivity of the seed layer and the compatibility of subsequent electroplating.
[0081] Corresponding to Figure 1 The present disclosure also provides an electronic device 500, such as a magnetron sputtering method for preparing Ti / Cu seed layers. Figure 5 The diagram shown is a structural schematic of an electronic device 500 provided in an embodiment of this disclosure, including: Processor 51, memory 52, and bus 53; memory 52 is used to store execution instructions, including main memory 521 and external memory 522; the main memory 521, also called internal memory, is used to temporarily store the computational data in processor 51, as well as the data exchanged with external memory 522 such as hard disk. Processor 51 exchanges data with external memory 522 through main memory 521. When the electronic device 500 is running, processor 51 and memory 52 communicate through bus 53, enabling processor 51 to execute... Figure 1 The steps of the magnetron sputtering method for preparing Ti / Cu seed layers.
[0082] This disclosure also provides a computer-readable storage medium storing a computer program. When executed by a processor, the computer program performs the steps of the magnetron sputtering preparation method for the Ti / Cu seed layer described in the above method embodiments. The storage medium can be a volatile or non-volatile computer-readable storage medium.
[0083] This disclosure also provides a computer program product, which includes computer instructions. When the computer instructions are executed by a processor, they can perform the steps of the magnetron sputtering preparation method for the Ti / Cu seed layer described in the above method embodiments. For details, please refer to the above method embodiments, which will not be repeated here.
[0084] The aforementioned computer program product can be implemented through hardware, software, or a combination thereof. In one optional embodiment, the computer program product is specifically embodied in a computer storage medium; in another optional embodiment, the computer program product is specifically embodied in a software product, such as a software development kit (SDK), etc.
[0085] Those skilled in the art will clearly understand that, for the sake of convenience and brevity, the specific working process of the device described above can be referred to the corresponding process in the foregoing method embodiments, and will not be repeated here. In the several embodiments provided in this disclosure, it should be understood that the disclosed device and method can be implemented in other ways. The device embodiments described above are merely illustrative. For example, the division of units is only a logical functional division, and in actual implementation, there may be other division methods. Furthermore, multiple units or components may be combined or integrated into another system, or some features may be ignored or not executed. Another point is that the displayed or discussed mutual coupling or direct coupling or communication connection may be through some communication interfaces; the indirect coupling or communication connection of devices or units may be electrical, mechanical, or other forms.
[0086] The units described as separate components may or may not be physically separate. The components shown as units may or may not be physical units; that is, they may be located in one place or distributed across multiple network units. Some or all of the units can be selected to achieve the purpose of this embodiment according to actual needs.
[0087] In addition, the functional units in the various embodiments of this disclosure can be integrated into one processing unit, or each unit can exist physically separately, or two or more units can be integrated into one unit.
[0088] If the aforementioned functions are implemented as software functional units and sold or used as independent products, they can be stored in a processor-executable, non-volatile, computer-readable storage medium. Based on this understanding, the technical solution of this disclosure, in essence, or the part that contributes to the prior art, or a portion of the technical solution, can be embodied in the form of a software product. This computer software product is stored in a storage medium and includes several instructions to cause a computer device (which may be a personal computer, server, or network device, etc.) to execute all or part of the steps of the methods described in the various embodiments of this disclosure. The aforementioned storage medium includes various media capable of storing program code, such as USB flash drives, portable hard drives, read-only memory (ROM), random access memory (RAM), magnetic disks, or optical disks.
[0089] Finally, it should be noted that the above-described embodiments are merely specific implementations of this disclosure, used to illustrate the technical solutions of this disclosure, and not to limit it. The protection scope of this disclosure is not limited thereto. Although this disclosure has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that any person skilled in the art can still modify or easily conceive of changes to the technical solutions described in the foregoing embodiments, or make equivalent substitutions for some of the technical features, within the scope of the technology disclosed in this disclosure. Such modifications, changes, or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of this disclosure, and should all be covered within the protection scope of this disclosure. Therefore, the protection scope of this disclosure should be determined by the protection scope of the claims.
Claims
1. A method for preparing a Ti / Cu seed layer by magnetron sputtering, characterized in that, include: The substrate to be deposited was placed in a vacuum chamber, and the relationship between the sputtering power ratio of Ti target and Cu target and the percentage content of Ti atoms was obtained. Ar working gas is introduced into the vacuum chamber, and independently adjustable sputtering power is applied to the Ti target and Cu target respectively; Adjust the power ratio between the Ti target and the Cu target according to the corresponding relationship, and form a Ti / Cu seed layer on the substrate surface by co-sputtering or power gradient method, so that the Ti / Cu seed layer forms an atomic mixed structure or a composition gradient structure that changes continuously along the thickness direction; The percentage content of Ti atoms in the Ti / Cu seed layer is controlled within the range of 15% to 35%, and the total thickness of the Ti / Cu seed layer is 40 to 150 nm.
2. The method according to claim 1, characterized in that, Before applying independently adjustable sputtering power to the Ti target and Cu target respectively, the method further includes: The vacuum chamber is evacuated to a background pressure not exceeding 5 × 10⁻⁶. -5 Pa; Ar gas is introduced into the vacuum chamber, and the substrate is subjected to Ar plasma cleaning to remove oxides and organic contaminants from the surface of the substrate. The Ar plasma cleaning process involves a power of 50–150 W, a cleaning time of 5–15 min, and a cleaning pressure of 0.5–1 Pa.
3. The method according to claim 1, characterized in that, The relationship between the sputtering power ratio of Ti and Cu targets and the percentage content of Ti atoms was obtained, including: Under conditions of fixed total power or fixed total deposition time, multiple calibration samples were prepared according to different power ratios of Ti target to Cu target; Elemental analysis of the calibration sample was performed using energy-dispersive X-ray spectroscopy or X-ray photoelectron spectroscopy. A calibration curve was established based on the elemental analysis results, relating the power ratio of Ti targets to Cu targets and the percentage content of Ti atoms. The power ratio of the Ti target to the Cu target is 0.2 to 0.8, and the percentage content of Ti atoms is 20% to 30%.
4. The method according to claim 1, characterized in that, Forming a Ti / Cu seed layer on the substrate surface by co-sputtering includes: During the deposition process, the Ti target power and Cu target power are kept constant to form a Ti / Cu seed layer with a uniform mixture of Ti atoms and Cu atoms; The thickness of the Ti / Cu seed layer is 50–120 nm, and the deposition time is 1–5 min.
5. The method according to claim 1, characterized in that, Forming a Ti / Cu seed layer on the substrate surface using a power gradient method includes: During the initial deposition phase, within a thickness range of 20% to 30% of the total thickness of the Ti / Cu seed layer, the Ti target power is increased and the Cu target power is decreased to form a Ti-rich region close to the substrate. Subsequently, the Ti target power is gradually reduced along the deposition time or thickness direction while the Cu target power is increased simultaneously to form a Cu-rich region near the surface of the seed layer; The percentage of Ti atoms in the Ti / Cu seed layer gradually decreases from 30% near the substrate to less than 10% near the surface.
6. The method according to claim 1, characterized in that: A negative bias voltage is applied to the substrate during magnetron sputtering; The negative bias voltage is a DC bias voltage or pulse bias voltage of -60 to -150V, which promotes the intermixing of Ti atoms and Cu atoms at the substrate interface and improves the density of the seed layer.
7. The method according to claim 1, characterized in that: After deposition, the Ti target power supply, Cu target power supply and negative bias power supply are turned off, and the substrate is cooled to room temperature in a vacuum environment or a low-pressure Ar protective atmosphere. After the Ti / Cu seed layer is deposited and exits the cavity, the Ti / Cu seed layer is subjected to Ar plasma surface activation treatment. The power of the surface activation treatment is 20-50W and the treatment time is 1-3min.
8. A magnetron sputtering apparatus for preparing a Ti / Cu seed layer, characterized in that, include: The substrate loading module is used to place the substrate to be deposited in a vacuum chamber and obtain the relationship between the sputtering power ratio of Ti target and Cu target and the percentage content of Ti atoms. The sputtering power application module is used to introduce Ar working gas into the vacuum chamber and apply independently adjustable sputtering power to the Ti target and Cu target respectively. A co-sputtering or gradient deposition module is used to adjust the power ratio between the Ti target and the Cu target according to the corresponding relationship, and to form a Ti / Cu seed layer on the substrate surface in a co-sputtering mode or a power gradient mode, so that the Ti / Cu seed layer forms an atomic mixed structure or a composition gradient structure that changes continuously along the thickness direction; wherein, the percentage content of Ti atoms in the Ti / Cu seed layer is controlled in the range of 15% to 35%, and the total thickness of the Ti / Cu seed layer is 40 to 150 nm.
9. An electronic device, characterized in that, include: The device includes a processor, a memory, and a bus. The memory stores machine-readable instructions executable by the processor. When the electronic device is running, the processor communicates with the memory via the bus. When the machine-readable instructions are executed by the processor, the steps of the magnetron sputtering preparation method for the Ti / Cu seed layer as described in any one of claims 1 to 7 are performed.
10. A computer-readable storage medium, characterized in that, The computer-readable storage medium stores a computer program that, when executed by a processor, performs the steps of the magnetron sputtering method for preparing a Ti / Cu seed layer as described in any one of claims 1 to 7.