A method for thermal insulation and corrosion protection of molten salt based on the addition of nano-rare earth oxides

By adding nano-rare earth oxides CeO2 and Y2O3 to sodium nitrate-potassium nitrate molten salt, a dense oxide film and refined grains are formed, solving the problem of metal corrosion in nitrate molten salt systems and achieving efficient and long-lasting anti-corrosion effect, which is suitable for solar thermal power generation and high-temperature thermal storage systems.

CN123108568APending Publication Date: 2026-11-17INNER MONGOLIA UNIV OF SCI & TECH
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202610870093.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-06-16
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies for inhibiting metal corrosion in nitrate molten salt systems suffer from limitations such as targeting a single target, restricting the form of additives, and not exploring the anti-corrosion mechanism in depth. As a result, it is difficult to achieve efficient and long-lasting anti-corrosion effects in solar thermal power generation and high-temperature thermal storage systems.

Method used

A stable suspension system is formed in sodium nitrate-potassium nitrate molten salt using nano-rare earth oxides CeO2 and Y2O3. This system forms a dense network oxide film on the surface of the metal material in situ, refines the grains, hinders the propagation of corrosion cracks, and reduces the corrosion rate.

Benefits of technology

It significantly reduces the corrosion rate of metallic materials in nitrate molten salt, extends equipment service life, is applicable to a wide range of nitrate molten salt systems, avoids the side effects of soluble ionic additives, and has a dual protection mechanism and good economic efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108568A_ABST
    Figure CN123108568A_ABST
Patent Text Reader

Abstract

This invention discloses a molten salt thermal storage corrosion prevention method based on the addition of nano-rare earth oxides. Sodium nitrate and potassium nitrate are mixed in a 6:4 ratio, melted and dehydrated, and 0.05-0.2wt% of 10-30nm CeO2 or Y2O3 nano-rare earth oxides are added. The mixture is kept at 565℃ to form a stable suspension system. The nanoparticles form a dense network oxide film on the metal surface in situ and refine the grains, reducing the corrosion rate by 24%. This method is suitable for solar thermal power generation and high-temperature thermal storage systems.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of inhibiting corrosion in molten salt systems, specifically, it relates to a method for molten salt thermal storage corrosion protection based on the addition of nano-rare earth oxides. Background Technology

[0002] Molten salts (especially nitrate molten salts) are widely used as heat transfer and storage media in solar thermal power generation, high-temperature thermal energy storage, and advanced nuclear energy systems due to their excellent thermal stability and high specific heat capacity. Among them, binary solar salts (NaNO3-KNO3, mass ratio 6:4) are the most commonly used molten salt system in current commercial solar thermal power plants. However, molten salts can corrode the metal materials they contact (such as stainless steel and nickel-based alloys) under high-temperature operating conditions, leading to thinner equipment walls, reduced structural strength, and in severe cases, leaks or even system shutdowns, significantly increasing operation and maintenance costs and threatening system safety. Therefore, mitigating the corrosion of metal materials by molten salts has always been a research hotspot in this field.

[0003] To suppress molten salt corrosion, existing technologies mainly focus on the following two directions:

[0004] (1) Surface protection and alloy modification of metallic materials

[0005] For example, high-temperature protective coatings (such as thermal barrier coatings and rare-earth-doped ceramic coatings) can be prepared on metal surfaces, or oxide dispersion-strengthened (ODS) alloys can be developed by adding rare-earth elements (Y, Ce, etc.). However, coating technology is subject to the risk of spalling failure under long-term thermal cycling, and the preparation process is complex and costly; alloy modification is limited by the difficulty of material processing and its versatility, making it difficult to apply to existing systems.

[0006] (2) Molten salt side additive regulation

[0007] Another technical approach involves directly adding corrosion inhibitors or redox modifiers to the molten salt. For example, Chinese invention patent CN109680282A discloses a method for inhibiting galvanic corrosion in molten salt systems by adding soluble redox ion pairs (such as Eu) to fluoride or chloride molten salts. 3+ / Eu 2+ Ce 4+ / Ce 3+ Cr 3+ / Cr 2+This method, including methods such as adding trace amounts of Y₂O₃ nanoparticles to nitrate molten salts, reduces or eliminates the potential difference between different metallic materials, thereby inhibiting galvanic corrosion caused by the contact of dissimilar materials. This method is mainly applicable to fluoride / chloride salt systems, and its mechanism relies on the redox reaction of ion pairs in molten salt, requiring a high level of chemical environment control from the molten salt itself. Furthermore, existing technologies have reported that adding trace amounts of Y₂O₃ nanoparticles to nitrate molten salts can reduce the corrosion current density of stainless steel (see "Study on Corrosion Behavior of 316 Stainless Steel in Nitrate Molten Salts with Added Trace Amounts of Rare Earth Elements", Chinese Journal of Corrosion and Protection, 2017). However, this study only involved a single rare earth oxide (Y₂O₃) and did not systematically investigate the effects of different rare earth types, particle sizes, and concentrations, nor did it reveal the regulatory effect of nanoparticles on the grain structure of the metal matrix.

[0008] Although the aforementioned existing technologies have alleviated the problem of molten salt corrosion to some extent, they still have the following shortcomings:

[0009] 1. Limited target: Existing additive technologies are mostly designed for fluoride / chloride salt systems or specific corrosion types (such as galvanic corrosion). For nitrate molten salts widely used in solar thermal power generation, there is a lack of efficient and universal anti-corrosion methods.

[0010] 2. Limitations in additive morphology: Although known soluble ionic additives (such as ion pairs in CN109680282A) can adjust the molten salt potential, their effect is greatly affected by the composition and impurities of the molten salt, and may introduce new side reactions; while conventional micron-sized particles or simple rare earth salts are difficult to disperse stably in molten salt and cannot form long-term protection.

[0011] 3. Insufficient depth in corrosion prevention mechanism: Most existing studies focus on the apparent phenomenon of reduced corrosion rate, without revealing how nanoparticles simultaneously change oxide film properties and metal matrix grain size from the perspective of the evolution of microstructure at the metal / molten salt interface, thus making it difficult to guide the systematic optimization of materials.

[0012] Therefore, there is an urgent need in the art for an anti-corrosion technology suitable for nitrate molten salt systems, with stable additive dispersion and a dual protection mechanism, capable of significantly reducing the corrosion rate of metallic materials in high-temperature molten salts, extending equipment service life, and meeting the requirements of economic efficiency, safety, and long-term effectiveness for solar thermal power generation and high-temperature thermal storage systems. The information disclosed in this background section is intended only to enhance understanding of the overall background of the invention and should not be construed as an admission or in any way implying that such information constitutes prior art known to those skilled in the art. Summary of the Invention

[0013] In view of the shortcomings of the existing technology, the main purpose of this invention is to explore the protection mechanism of nano-rare earth oxides against molten salt corrosion and obtain the optimal parameters of their corrosion protection performance on metal materials. This method can effectively reduce the corrosion rate of metals in molten salt, extend the service life of metal materials in molten salt, thereby reducing operating costs and providing scientific and technological support for green and low-carbon development.

[0014] To achieve the above objectives, the present invention adopts the following technical solution:

[0015] A molten salt thermal storage and corrosion protection method based on the addition of nano-rare earth oxides, characterized by comprising the following steps:

[0016] 1) Preparation of molten salt: Sodium nitrate and potassium nitrate are mixed, placed in a crucible, and then placed in a tube furnace. The mixture is heated to 350°C at a rate of 10°C / min and held at 350°C for 3 hours to remove intercrystalline water. The mixture is then cooled to room temperature to allow the two salts to eutecticly crystallize and obtain molten salt.

[0017] 2) Establishing an anti-corrosion system: The molten salt prepared in step 1) is pulverized into powder, and nano-rare earth oxides are added to the molten salt in a certain mass ratio and mixed thoroughly and evenly. Then, the mixed molten salt is placed in a muffle furnace, heated to 565℃, and maintained at 565℃ for 1.5h. After cooling, a eutectic system is formed.

[0018] The rare earth oxide is at least one of CeO2 and Y2O3.

[0019] Preferably, the particle size of the nano-rare earth oxide is 10-30 nm.

[0020] Preferably, the amount of rare earth oxide added is 0.05-0.2 wt% by mass.

[0021] Preferably, the mass ratio of sodium nitrate to potassium nitrate in step 1) is 6:4.

[0022] Preferably, after adding rare earth oxides, the corrosion rate, measured by weight loss, decreased from the original 0.1042 mm / y of the molten salt base salt to 0.0792 mm / y to 0.0896 mm / y.

[0023] Preferably, the corrosion rate is reduced by 24% compared to a single molten salt system.

[0024] Preferably, the nano-rare earth oxide forms a stable suspension system in the molten salt and forms a dense network oxide film in situ on the surface of the metal material, preventing direct contact between the molten salt and the metal substrate.

[0025] Preferably, the metallic material is an iron-based alloy.

[0026] By adopting the above technical solution, the nano-rare earth oxide refines the grains of the metal material and hinders the propagation of corrosion cracks.

[0027] Preferably, the salt comprises a molten nitrate salt and nano-rare earth oxides dispersed therein; the nano-rare earth oxides include at least one of CeO2 and Y2O3; the particle size of the nano-rare earth oxides is 10~30nm, and the amount added is 0.05%-0.2% of the mass of the molten salt.

[0028] Furthermore, it is preferred to add 0.1% of nano-rare earth oxides with a particle size of 20 nm.

[0029] By adopting the above technical solutions, the corrosion resistance of the metal itself can be improved, thereby reducing the corrosion rate and extending the service life of the pipeline.

[0030] The beneficial effects of this invention are:

[0031] 1) Significantly reduces the corrosion rate of metallic materials in nitrate molten salts.

[0032] This invention involves adding nano-rare earth oxides (CeO2, Y2O3) to sodium nitrate-potassium nitrate solar salt and conducting corrosion tests on 316L stainless steel in a high-temperature static molten salt at 565℃. The results show that adding 0.1 wt% of rare earth oxides with a particle size of 20 nm reduces the corrosion rate (based on weight loss) from the original 0.1042 mm / y in the molten salt base salt to 0.0792 mm / y to 0.0896 mm / y, a reduction of approximately 24%. This data confirms the significant effect of the method of this invention on mitigating molten salt corrosion, which can directly extend the service life of metal components in solar thermal power generation and high-temperature thermal storage systems, and reduce operation and maintenance costs.

[0033] 2) Overcoming the limitations of existing technologies on molten salt systems, it is applicable to the nitrate system commonly used in concentrated solar power generation.

[0034] Existing additive technologies for inhibiting molten salt corrosion are mostly aimed at fluoride or chloride salt systems (such as CN109680282A), or only applicable to galvanic corrosion scenarios. This invention, however, specifically targets the binary nitrate (solar salt) system widely used in commercial solar thermal power plants, filling the gap in efficient and long-lasting corrosion protection technology for this system. Furthermore, this invention does not rely on adjusting the potential difference between dissimilar metals, but directly inhibits the uniform corrosion of a single metal material by molten salt, thus having a wider range of applications.

[0035] 3) Insoluble nanoparticles are used to avoid the side effects of soluble ionic additives.

[0036] Compared to existing technologies that add soluble redox ion pairs (such as Eu) to molten salts 3+ / Eu 2+ Ce 4+ / Ce 3+ The present invention uses insoluble nano-rare earth oxide solid particles, as described in the methods of (etc.). These nanoparticles form a stable suspension system in molten salt without introducing additional soluble impurities or altering the basic properties of the molten salt (such as melting point and viscosity), thereby avoiding side reactions or adverse effects on the thermal properties of the molten salt that may be caused by ionic additives.

[0037] 4) Establishing a dual protection mechanism ensures longer-lasting and more reliable corrosion prevention.

[0038] This invention reveals for the first time the dual-action mechanism of nano-rare earth oxides in molten salt corrosion protection: on the one hand, nanoparticles form a dense and continuous network oxide film in situ on the surface of the metal material, physically blocking direct contact between the molten salt and the metal substrate; on the other hand, nanoparticles can refine the surface grains of the metal material, hindering the initiation and propagation of corrosion cracks. This synergistic protection mechanism of "external barrier and internal reinforcement" has better anti-scraping ability and long-term stability compared to technologies that rely solely on surface coatings or corrosion inhibitors.

[0039] 5) The system optimized the types, particle sizes, and amounts of nano-rare earth oxides to achieve "micro-volume, high-efficiency" results.

[0040] This invention systematically studied the effects of two rare earth oxides, CeO2 and Y2O3, three particle sizes (10-30 nm), and three addition concentrations (0.05-0.2 wt%) on corrosion protection performance, and established a quantitative structure-activity relationship between the physical properties of nano-additives and their corrosion protection effect. Experiments show that only 0.1 wt% of 20 nm-sized nanoparticles are needed to achieve significant effects; the addition amount is small, the cost is low, and it is convenient for industrial application.

[0041] 6) Easy to operate and compatible with existing molten salt thermal energy storage systems

[0042] This invention only requires adding a mixing and dispersion step of nano-rare earth oxides to the existing molten salt preparation process. It does not require modification of existing equipment or replacement of metal materials and can be directly applied to existing solar thermal power generation and high-temperature thermal storage systems, with good economic efficiency and feasibility.

[0043] In summary, this invention provides a nano-rare earth oxide corrosion protection technology applicable to nitrate molten salt systems, with significant anti-corrosion effect, clear mechanism, low cost, and easy implementation. It overcomes the shortcomings of existing technologies such as the limitations of molten salt systems, large side effects of additives, and single protection mechanism. It is of great significance for promoting the safe, efficient, and low-cost development of solar thermal power generation and high-temperature thermal storage technologies. Attached Figure Description

[0044] Figure 1 The results of the molecular dynamics simulation in Example 8 consist of 4 small figures: ( Figure 1-a is a snapshot of the equilibrium structure of the three-phase interface of molten salt-nano rare earth oxide-Fe2O3; Figure 1 -b represents the mean square displacement (MSD) curve of corrosive ions at the interface; Figure 1 -c is the radial distribution function (RDF) between rare earth ions and interfacial oxygen atoms. Figure 1 -d represents the calculated result of the interfacial interaction energy between nanoparticles and oxide film).

[0045] Figure 2 This is a diagram of the experimental setup for the weightlessness test;

[0046] Figure 3 A bar chart comparing the corrosion rates of 316L stainless steel under different molten salt systems is presented, showing the average corrosion rates and error bars for three groups: single solar salt, solar salt + cerium oxide, and solar salt + yttrium oxide.

[0047] Figure 4 The X-ray diffraction (XRD) analysis results of the corrosion products in Example 7 consist of three large images: ( Figure 4 -a is the XRD pattern of corrosion products of 316L stainless steel in a single solar salt system. Figure 4 -b is the XRD pattern of corrosion products of 316L stainless steel in the solar salt + cerium oxide system; Figure 4 -c represents the XRD pattern of corrosion products of 316L stainless steel in the solar salt + yttrium oxide system.

[0048] Figure 5 SEM images of surface corrosion of stainless steel in Example 7 at different times in a base salt (single solar salt);

[0049] Figure 6 EDS elemental distribution diagram of stainless steel after surface corrosion in basic salt (single solar salt);

[0050] Figure 7 EDS elemental distribution diagram of stainless steel after surface corrosion in the presence of nano-rare earth oxides (CeO2);

[0051] Figure 8 SEM images for corrosion morphology analysis, including Figure 8 -a represents the microstructure of the corrosion layer with added nano-rare earth oxides; Figure 8 -b represents the microstructure of the corrosion layer without the addition of nano-rare earth oxides. Detailed Implementation

[0052] The present invention will be further described below through specific embodiments. To make the inventive objectives, technical solutions, and beneficial technical effects of the present invention clearer, the present invention will be further described in detail below with reference to the embodiments. It should be understood that the embodiments described in this specification are merely for explaining the present invention and are not intended to limit the present invention.

[0053] Unless otherwise stated, all instruments and reagents used in the examples are commercially available or synthesized using conventional methods and can be used directly without further processing, and all instruments used in the examples are commercially available.

[0054] Example 1:

[0055] 1) Preparation of molten salt:

[0056] Sodium nitrate and potassium nitrate were weighed together in a 6:4 ratio, placed in a crucible, and then placed in a tube furnace for heating. The temperature was increased to 350°C at a rate of 10°C / min and maintained at 350°C for 3 hours to remove intercrystalline water. The mixture was then cooled to room temperature to allow the two salts to eutecticly crystallize, thus completing the preparation.

[0057] 2) Establish an anti-corrosion system:

[0058] The molten salt prepared in step 1) is pulverized into powder, and nano-rare earth oxides are added to the molten salt at a certain mass ratio (0.2%) and mixed thoroughly and evenly. Then, the mixed molten salt is placed in a muffle furnace, heated to 565°C, and maintained at 565°C for 1.5 hours. After cooling, a eutectic is formed to form a stable system.

[0059] The particle size of the nano-rare earth oxides (CeO2, Y2O3) is 30nm.

[0060] Example 2:

[0061] 1) Preparation of molten salt: Weigh sodium nitrate and potassium nitrate in a 6:4 ratio, place them in a crucible, and put them in a tube furnace for heating; raise the temperature to 350℃ at a rate of 10℃ / min, maintain the temperature at 350℃ for 3 hours to remove intercrystalline water, and cool to room temperature to allow the two salts to eutecticly crystallize, thus preparing the molten salt;

[0062] 2) Establishing an anti-corrosion system: The molten salt prepared in step 1) is pulverized into powder, and nano-rare earth oxides are added to the molten salt at a certain mass ratio (0.1%). The nanoparticles are evenly distributed in the molten salt system using a muffle furnace. The system is kept at 565℃ for 1.5 hours and then cooled to form a stable eutectic system.

[0063] The particle size of the nano-rare earth oxide (CeO2) is 20 nm.

[0064] Example 3:

[0065] 1) Preparation of molten salt: Weigh sodium nitrate and potassium nitrate in a 6:4 ratio, place them in a crucible, and put them in a tube furnace for heating; raise the temperature to 350℃ at a rate of 10℃ / min, maintain the temperature at 350℃ for 3 hours to remove intercrystalline water, and cool to room temperature to allow the two salts to eutecticly crystallize, thus preparing the molten salt;

[0066] 2) Establishing an anti-corrosion system: The molten salt prepared in step 1) is pulverized into powder, and nano-rare earth oxides are added to the molten salt at a certain mass ratio (0.1%). The nanoparticles are evenly distributed in the molten salt system using a muffle furnace. The system is kept at 565℃ for 1.5 hours and then cooled to form a stable eutectic system.

[0067] The particle size of the nano-rare earth oxide (Y2O3) is 20 nm.

[0068] Example 4:

[0069] 1) Preparation of molten salt: Weigh sodium nitrate and potassium nitrate in a 6:4 ratio, place them in a crucible, and put them in a tube furnace for heating; raise the temperature to 350℃ at a rate of 10℃ / min, maintain the temperature at 350℃ for 3 hours to remove intercrystalline water, and cool to room temperature to allow the two salts to eutecticly crystallize, thus preparing the molten salt;

[0070] 2) Establishing an anti-corrosion system: The molten salt prepared in step 1) is crushed into powder, and nano-rare earth oxides are added to the molten salt at a certain mass ratio (0.05%). The nanoparticles are evenly distributed in the molten salt system using a muffle furnace. The system is kept at 565℃ for 1.5 hours and then cooled to form a stable eutectic system.

[0071] The particle size of the nano-rare earth oxide (CeO2) is 10 nm.

[0072] Example 5:

[0073] 1) Preparation of molten salt: Weigh sodium nitrate and potassium nitrate in a 6:4 ratio, place them in a crucible, and put them in a tube furnace for heating; raise the temperature to 350℃ at a rate of 10℃ / min, maintain the temperature at 350℃ for 3 hours to remove intercrystalline water, and cool to room temperature to allow the two salts to eutecticly crystallize, thus preparing the molten salt;

[0074] 2) Establishing an anti-corrosion system: The molten salt prepared in step 1) is crushed into powder, and nano-rare earth oxides are added to the molten salt at a certain mass ratio (0.05%). The nanoparticles are evenly distributed in the molten salt system using a muffle furnace. The system is kept at 565℃ for 1.5 hours and then cooled to form a stable eutectic system.

[0075] The particle size of the nano-rare earth oxide (Y2O3) is 30 nm.

[0076] Example 6: Influence of nano-rare earth oxides on molten salt corrosion protection performance

[0077] This embodiment uses Solar Salt as the corrosive medium and Examples 2 and 3 as examples to systematically study the effects of the type, particle size, and concentration of nano-rare earth oxides on the corrosion behavior of 316L stainless steel in static molten salt at 565℃. The corrosion rate of the material under different parameter combinations was determined using the weight loss method.

[0078] 6.1 Corrosion Test by Weight Loss Method

[0079] Sample preparation:

[0080] 316L stainless steel was processed into standard sheet-shaped samples. The surface was successively polished to a smooth finish using 400#, 600#, 800#, 1000#, and 1500# sandpaper, and then polished to a mirror finish. The samples were then ultrasonically cleaned in acetone and deionized water, dried with cold air, and stored in a desiccator for later use. The initial mass of the samples was weighed using an analytical balance (accuracy 0.0001g).

[0081] 6.2 Corrosion Test:

[0082] Weigh 200g of the modified molten salt prepared in Examples 2-3 and the comparative molten salt prepared in Comparative Example 1, and place them in a clean corundum crucible. Place the sample vertically in the crucible, ensuring that the sample is completely immersed in the molten salt. Place the crucible in a muffle furnace and, under the protection of high-purity argon, heat to 565℃ at a rate of 10℃ / min, and maintain the temperature for 200h for corrosion.

[0083] 6.3 Procedure for the weightlessness method:

[0084] 6.3.1 Preparation of Basic Salt

[0085] Sodium nitrate and potassium nitrate, both with a purity of 99.9%, were uniformly mixed in a 6:4 ratio. The mixed salt was then heated in a muffle furnace at 350°C for 3 hours to fully melt the salt and evaporate the water of crystallization. After complete melting, the mixed salt was removed from the muffle furnace and cooled to obtain solar salt, also known as base salt. The base salt was then ground into powder using an ultrafine pulverizer, dried, and stored for later use.

[0086] 6.3.2 Preparation of Molten Salt Nanocomposites

[0087] First, weigh out a certain amount of nanoparticles and basic salt, and grind them thoroughly in a mortar to achieve a preliminary mixture. Then, place the crucible containing the basic salt and nanoparticle mixture in a muffle furnace and heat it to 565℃, holding it at that temperature for 1.5 hours. After a certain period of time, remove the mixture, cool it, and grind it into powder using an ultrafine pulverizer. Store the powder in an 80℃ forced-air drying oven to avoid the molten salt absorbing moisture and affecting the thermophysical property measurements.

[0088] 6.3.3 Experimental Procedure

[0089] The corrosion behavior of 316L stainless steel samples in base salt and molten salt nanofluids was evaluated using the weight loss method. Three identical samples were vertically placed in corundum crucibles containing different molten salts and completely immersed. After 200 hours of corrosion, the samples were removed from the muffle furnace. After cooling to room temperature, the samples were placed in beakers containing deionized water, and residual molten salt was removed from the surface with a soft brush. The cleaned stainless steel samples were then placed in a drying oven to air dry and sealed for storage. Corrosion products on the stainless steel surface were removed according to ASTM G1-03 (2017) standard, with the following specific steps:

[0090] (1) Immerse the sample in a beaker containing deionized water to fully soak and clean it to remove residual salt from the sample surface.

[0091] (2) Place the sample in a beaker containing ethanol solution to clean it.

[0092] (3) Then the sample was placed in a 1.5 mol / L nitric acid solution and kept at 70°C for 300 min to ensure that the corrosion products on the surface of the sample were fully removed.

[0093] (4) Finally, after soaking the sample in ethanol solution, place it in a drying oven to dry. Weigh each sample three times and take the final mass (m). f The average value of ).

[0094] The mass loss of the etched sample is obtained using equation (1):

[0095]

[0096] In the formula, ∆m — mass loss, mg; m i —Initial mass of the sample after corrosion, mg; m f —The mass of the sample after time t, mg; A0 —Surface area, cm² 2 ;A0=(2.5*2+2.5*0.2+2*0.2)*2=11.8cm 2 .

[0097] The corrosion rate of the etched sample is obtained using equation (2):

[0098]

[0099] In the formula, t is the immersion time of the corroded sample (h); ρ is the density of the stainless steel sample (g / cm³). 3 .

[0100] The formula for calculating the standard deviation is shown in equation (3):

[0101]

[0102] In the formula, x i —Measured corrosion rate of stainless steel sample, mm / y;

[0103] x̅—Average corrosion rate of stainless steel samples, mm / y; n—Number of samples. Post-processing and calculations:

[0104] After corrosion, the samples were removed and immersed in deionized water to thoroughly remove residual salts from the surface. They were then rinsed with deionized water and ethanol, dried with cold air, and weighed. The corrosion rate was calculated using the weight loss method formula. Three parallel samples were used in each experiment, and the average value and standard deviation were calculated. The weight loss method test results are summarized in Table 1, and the corrosion rate comparison bar chart is attached. Figure 3 :

[0105] Table 1. Weight loss corrosion rate of 316L stainless steel in different molten salt systems (565℃, 200h)

[0106] serial number Molten salt system Initial mass (g) Mass after corrosion (g) Mass loss ΔM(g) Corrosion rate (mm / y) Average value (mm / y) Standard deviation 3 Basic salt (blank) 7.7441 7.7401 0.004 0.1034 — — 4 Basic salt (blank) 7.7455 7.7415 0.004 0.1034 0.1042 0.0015 5 Basic salt (blank) 7.7338 7.7297 0.0041 0.1059 — — 6 <![CDATA[Base salt + nano Y₂O₃ (Example 3)]]> 7.7273 7.7244 0.0029 0.0749 — — 9 <![CDATA[Base salt + nano Y2O3 (Example 3)]]> 7.7222 7.7185 0.0037 0.0956 0.0896 0.0127 10 <![CDATA[Base salt + nano Y2O3 (Example 3)]]> 7.7238 7.72 0.0038 0.0982 — — 16 <![CDATA[Base salt + nano CeO2 (Example 2)]]> 7.7292 7.7263 0.0029 0.0749 — — 19 <![CDATA[Base salt + nano CeO2 (Example 2)]]> 7.7338 7.7303 0.0035 0.0904 0.0792 0.0098 20 <![CDATA[Base salt + nano CeO₂ (Example 2)]]> 7.7288 7.726 0.0028 0.0724 — —

[0107] Note that the base salt is solar salt (also known as molten salt: including sodium nitrate and potassium nitrate).

[0108] Analysis of the results of the weightlessness method:

[0109] From Table 1 and Appendix Figure 3 The corrosion rate histogram shows that after 200 hours of corrosion in static solar salt at 565℃, the average corrosion rate of the blank control group was 0.1042 mm / y. After adding 0.1 wt% and 20 nm Y₂O₃ (Example 3), the average corrosion rate decreased to 0.0896 mm / y. After adding 0.1 wt% and 20 nm CeO₂ (Example 2), the average corrosion rate decreased to 0.0792 mm / y, a reduction of approximately 24.0%.

[0110] Example 7: Mechanism of action of nano-rare earth oxides in improving the corrosion resistance of molten salt

[0111] Based on the corrosion test of the sample in Example 6, various characterization methods were used to reveal the effect of the addition of nano-rare earth oxides on the composition, structure, density and chemical state evolution of the oxide film, and to explain the mechanism of its effect on improving the corrosion resistance of the material at the microscopic level.

[0112] 7.1 Corrosion Morphology Analysis (SEM)

[0113] After 200 hours of corrosion, the 316L stainless steel samples (Example 2 and Comparative Example 1) were cut, inlaid, ground, and polished, and then the sample surface was observed by scanning electron microscopy (SEM).

[0114] Addition of nano-rare earth oxides (Example 2): A dense, continuous network oxide film is formed on the metal surface, with uniform film thickness and no obvious through cracks (see Appendix). Figure 8 -a).

[0115] Without the addition of nano-rare earth oxides (Comparative Example 1): the oxide film is loose and porous, with uneven thickness, and obvious cracks and spalling pits are visible in some areas. The crack depth has penetrated the oxide film and points towards the substrate (see Appendix). Figure 8 -b).

[0116] 7.2 Phase Analysis of Corrosion Products (EDS)

[0117] X-ray diffraction analysis was performed on the surface of the corroded sample to identify the phase composition of the corrosion products. Figure 4 :

[0118] Figure 4 -a is a spectrum of corrosion products of 316L stainless steel in a single solar salt system.

[0119] Figure 4 -b is a spectrum of corrosion products of 316L stainless steel in the solar salt + cerium oxide system;

[0120] Figure 4 -c is a spectrum of corrosion products of 316L stainless steel in the solar salt + yttrium oxide system.

[0121] XRD analysis results showed that the blank group mainly detected diffraction peaks of Fe2O3, Fe3O4 and Cr2O3; after adding nano-rare earth oxides, in addition to the above oxides, weak rare earth composite oxide diffraction peaks also appeared. These composite oxides have high thermal stability and can fill the gaps in the oxide film grain boundaries, thereby improving the overall compactness of the oxide film.

[0122] Mechanism summary:

[0123] Nano-rare earth oxides form a stable suspension system in molten salt and form a dense network oxide film in situ on the surface of the metal material, physically blocking the direct contact between the molten salt and the metal matrix; at the same time, rare earth elements diffuse into the grain boundaries of the metal surface, refine the grains and hinder the propagation of corrosion cracks, forming a dual protection mechanism of "external barrier and internal reinforcement".

[0124] Furthermore, Figure 6 The results showed that the corrosion products were mainly composed of O, Fe, Cr and Ni elements, and each characteristic peak corresponded to the composition of the matrix metal oxide. No rare earth element signals were detected in the spectrum, indicating that the corrosion of the blank control group was a typical matrix selective oxidation corrosion without the participation of external corrosion inhibitors.

[0125] and Figure 6 compared to, Figure 7In addition to the matrix element peaks of O, Fe, Cr, and Ni, obvious rare earth element characteristic peaks (labeled as Y in the figure, corresponding to the characteristic X-ray energies of the L and K series of rare earth elements) also appeared at approximately 1.5 keV, 14 keV, and 16 keV, confirming that nano-rare earth oxides migrate and accumulate on the metal surface during corrosion, participating in the formation of surface corrosion products.

[0126] This result corroborates the dense oxide film observed by SEM and the rare earth composite oxide phase identified by XRD, supporting the dual protection mechanism of "in-situ film formation" of nano-rare earth oxides at the elemental composition level.

[0127] Example 8: Microscopic interaction mechanism at the molten salt-nanoparticle-oxide film interface

[0128] In this embodiment, a multiphase composite interface model of molten salt-nano rare earth oxide-metal oxide film (Fe2O3) was constructed, and molecular dynamics (MD) simulation studies were carried out to elucidate the microscopic mechanism by which nano rare earth oxides hinder the transport of corrosive ions and stabilize the interface structure at the atomic scale.

[0129] 8.1 Model Construction and Simulation Parameters

[0130] Construct containing Na + K + NO3 - A three-phase interface model was developed for the molten salt phase of ions, the oxide film phase of α-Fe2O3(0001) crystal planes, and the nano-rare earth oxide clusters. The simulation was performed using the NVT ensemble at 565℃ (838K) with a time step of 1 fs and a total simulation time of 500 ps.

[0131] 8.2 Calculation Content and Result Analysis

[0132] Interface structure snapshot (see appendix) Figure 1 -a): Visual analysis of the simulated trajectories shows that nano-rare earth oxides tend to adsorb at defect sites on the Fe2O3 surface, thereby improving the interfacial density by filling the defects.

[0133] Mean square displacement (MSD) analysis (see appendix) Figure 1 -b): Calculate the MSD curve of corrosive ions at the interface in the molten salt. The results show that the interfacial diffusion coefficient of corrosive ions is significantly reduced after the addition of nano-rare earth oxides, indicating that nanoparticles have a physical barrier effect on ion transport.

[0134] Radial distribution function (RDF) analysis (see appendix) Figure 1 -c): Calculate the RDF of rare earth ions and oxygen atoms. The results show strong peaks and secondary ordered peaks at specific distances, indicating that a stable oxygen coordination layer is formed on the surface of the nanoparticles, which can stabilize the interfacial oxygen partial pressure.

[0135] Interfacial interaction energy analysis (see appendix) Figure 1 -d): Calculate the interfacial binding energy between nanoparticles and the Fe2O3 oxide film. A negative binding energy indicates that the nano-rare earth oxides have thermodynamic adsorption stability on the oxide film surface and can reside at the interface for a long time to exert a protective effect.

[0136] Simulation conclusion:

[0137] Molecular dynamics simulations confirmed the stable adsorption behavior of nano-rare earth oxides at the molten salt / oxide film interface at the atomic scale, revealing the microscopic mechanism by which they achieve corrosion protection by reducing the diffusion dynamics of corrosive ions and stabilizing the local structure of the interface, which corroborates the macroscopic characterization results in Example 7.

[0138] Comparative Example 1: Pure Solar Salt Blank Control

[0139] To quantitatively evaluate the anti-corrosion effect of nano-rare earth oxides, a blank control experiment was set up. Except for the absence of any nano-rare earth oxides, the molten salt preparation process, corrosion test conditions (565℃, 200h, high-purity argon atmosphere), sample material and size were all consistent with those in Example 1.

[0140] The results of the weightlessness test are summarized in Table 1 and Appendix. Figure 4 The average corrosion rate of the blank group was 0.1042 mm / y, which served as the benchmark for evaluating the anti-corrosion effect after adding nano-rare earth oxides.

[0141] The above description of the disclosed embodiments enables those skilled in the art to make or use the invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the invention is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A molten salt heat storage and corrosion prevention method based on the addition of nanosized rare earth oxides, characterized by, Includes the following steps: 1) Preparation of molten salt: Sodium nitrate and potassium nitrate are mixed, placed in a crucible, and then placed in a tube furnace. The mixture is heated to 350°C at a rate of 10°C / min and held at 350°C for 3 hours to remove intercrystalline water. The mixture is then cooled to room temperature to allow the two salts to eutecticly crystallize and obtain molten salt. 2) Establishing an anti-corrosion system: The molten salt prepared in step 1) is pulverized into powder, and nano-rare earth oxides are added to the molten salt in a certain mass ratio and mixed thoroughly and evenly. Then, the mixed molten salt is placed in a muffle furnace, heated to 565℃, and maintained at 565℃ for 1.5h. After cooling, a eutectic system is formed. The rare earth oxide is at least one of CeO2 and Y2O3.

2. The method according to claim 1, wherein the nano-rare earth oxide is added to the molten salt. The particle size of the nano-rare earth oxide is 10-30 nm. ​ 3. The molten salt thermal storage and corrosion protection method based on the addition of nano-rare earth oxides according to claim 1, characterized in that, The amount of rare earth oxide added is 0.05-0.2 wt% by mass.

4. The molten salt thermal storage and corrosion protection method based on the addition of nano-rare earth oxides according to claim 1, characterized in that, In step 1), the mass ratio of sodium nitrate to potassium nitrate is 6:

4.

5. The molten salt thermal storage and corrosion protection method based on the addition of nano-rare earth oxides according to claim 1, characterized in that, After adding rare earth oxides, the corrosion rate, measured by weight loss, decreased from 0.1042 mm / y for the original molten salt base salt to 0.0792 mm / y to 0.0896 mm / y.

6. The molten salt thermal storage and corrosion protection method based on the addition of nano-rare earth oxides according to claim 5, characterized in that, Compared to a single molten salt system, the corrosion rate was reduced by 24%.

7. The molten salt thermal storage and corrosion protection method based on the addition of nano-rare earth oxides according to claim 1, characterized in that, The nano-rare earth oxides form a stable suspension system in the molten salt and form a dense network oxide film in situ on the surface of the metal material, preventing direct contact between the molten salt and the metal substrate.

8. The molten salt thermal storage and corrosion protection method based on the addition of nano-rare earth oxides according to claim 7, characterized in that, The metallic material is an iron-based alloy.

9. The molten salt thermal storage and corrosion protection method based on the addition of nano-rare earth oxides according to claim 8, characterized in that, The nano-rare earth oxides refine the grains of the metal material, hindering the propagation of corrosion cracks.

10. A modified molten salt for solar thermal power generation or high-temperature thermal storage, characterized in that, It comprises a molten salt containing nitrate and nano-rare earth oxides dispersed therein; the nano-rare earth oxides are at least one of CeO2 and Y2O3; the particle size of the nano-rare earth oxides is 10-30 nm, and the amount added is 0.05%-0.2% of the mass of the molten salt.

Citation Information

Patent Citations

  • Method for restraining galvanic corrosion of molten salt system

    CN109680282A