An amorphous phase FeS x Modified Ni3S2 self-supporting oxygen evolution precatalyst, its preparation method and application; an alkaline water electrolyzer.
By introducing amorphous FeSx into Ni3S2 to form a heterostructure, the conductivity and stability problems of nickel-iron-based catalysts were solved, achieving efficient oxygen evolution reaction and long-term catalyst stability, and reducing the oxygen evolution reaction energy barrier.
Patent Information
- Application Number
- CN202611383999.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-08
- Publication Date
- 2026-11-17
AI Technical Summary
Existing nickel-iron-based oxide or hydroxide catalysts have insufficient conductivity, resulting in slow charge transport, excessive consumption of lattice oxygen leading to decreased structural stability, high oxygen evolution overpotential, and insufficient catalytic effect.
Amorphous phase FeSx is introduced into crystalline phase Ni3S2 to form a crystalline-amorphous heterostructure. The amorphous phase provides abundant dangling bonds and coordination unsaturated sites, which promotes rapid interfacial charge transfer through the porous NiFe alloy substrate and generates the Ni(Fe)OOH active phase under alkaline conditions.
It significantly reduces the oxygen evolution reaction energy barrier, improves the activity and stability of the catalyst, reduces overpotential, maintains stable operation at high current density, and avoids the contact resistance and active site coverage problems of traditional catalysts.
Smart Images

Figure CN123108601A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the technical field of electrocatalytic water splitting and alkaline oxygen evolution reaction catalysts, and relates to an amorphous FeS phase catalyst. x A modified Ni3S2 self-supporting oxygen evolution precatalyst, its preparation method and application, and an alkaline water electrolyzer. Background Technology
[0002] Electrolysis of water to produce hydrogen is an important pathway for achieving green hydrogen energy production. The oxygen evolution reaction (OER) at the anolyte involves multiple electron transfer steps and is kineticly slow, requiring a highly efficient OER catalyst to reduce the reaction overpotential. Nickel-iron based catalysts are considered important alternatives to noble metal-based Ir and Ru OER catalysts due to their low cost, abundant reserves, and high catalytic activity under alkaline conditions.
[0003] Traditional nickel-iron-based oxides or hydroxides suffer from insufficient conductivity, limiting the rapid charge transport between the catalyst bulk phase and surface active sites. Simultaneously, in the oxygen evolution process involving the lattice oxygen mechanism, excessive consumption of lattice oxygen can lead to a large accumulation of oxygen vacancies, resulting in catalyst structural collapse and decreased long-term stability. Therefore, maintaining catalyst structural stability while enhancing lattice oxygen activity is a key issue in the design of alkaline oxygen evolution catalysts.
[0004] Transition metal sulfides typically exhibit good electrical conductivity and can undergo surface reconstruction during the oxygen evolution reaction (OER), generating the active phase of metal hydroxyl oxides that truly exert catalytic activity. For example, Chinese patent application CN112023946A discloses a method for preparing a self-supporting nickel-iron layered double hydroxide sulfide electrocatalyst. Using nickel foam as a substrate, a NiFe LDH-Sx / NF catalyst is grown on its surface, thereby improving the catalyst's catalytic activity. However, this material does not form a special crystalline phase modification structure, resulting in a still high OER overpotential and insufficient catalytic effect.
[0005] Therefore, if an appropriate amount of amorphous FeS phase can be introduced into the crystalline Ni3S2 phase... x Constructing a crystalline-amorphous heterostructure is expected to utilize the crystalline phase component to provide a conductive framework and the amorphous phase component to provide abundant defects, dangling bonds, and coordination unsaturated sites, thereby promoting the rapid generation of the active phase and improving OER performance. Summary of the Invention
[0006] To address the problems of insufficient conductivity, slow active phase formation, and decreased structural stability due to excessive lattice oxygen participation in existing nickel-iron-based oxygen evolution catalysts, the first objective of this invention is to provide an amorphous FeS phase catalyst. x A self-supported oxygen evolution precatalyst modified with crystalline Ni3S2. This is achieved by introducing transition metal sulfur compounds to improve catalyst conductivity, while utilizing the amorphous FeS2 phase.x The porous NiFe alloy substrate, which forms a crystalline-amorphous heterogeneous interface with the crystalline Ni3S2, provides abundant active sites and promotes rapid interfacial charge transfer.
[0007] The second objective of this invention is to provide an amorphous FeS phase. x A method for preparing a modified Ni3S2 self-supporting oxygen evolution precatalyst is disclosed. This invention allows the catalyst layer to be grown directly in situ on a porous NiFe alloy substrate, resulting in tight bonding between the materials. Then, A-FeS is simultaneously generated through a hydrothermal sulfidation reaction. x The / Ni3S2 composite catalyst layer has advantages such as simple process and readily available raw materials.
[0008] The third objective of this invention is to provide an amorphous FeS phase. x The application of modified Ni3S2 self-supporting oxygen evolution precatalyst as a catalyst in alkaline water electrolysis oxygen evolution reaction shows that surface reconstruction can occur during the alkaline oxygen evolution reaction to generate the Ni(Fe)OOH active phase, which significantly reduces the oxygen evolution reaction energy barrier.
[0009] The fourth objective of this invention is to provide an alkaline water electrolyzer that can maintain stable and long-term operation.
[0010] To achieve the above technical objectives, the present invention provides an amorphous FeS phase. x Modified Ni3S2 self-supporting oxygen evolution precatalyst, comprising a porous NiFe alloy substrate and A-FeS grown in situ on the surface of the porous NiFe alloy substrate. x / Ni3S2 composite catalyst layer; the A-FeS x Ni3S2 and A-FeS in the Ni3S2 composite catalyst layer x There is a crystalline-amorphous heterogeneous interface between them, where x is any number from 1 to 2.
[0011] The catalyst of this invention possesses abundant active sites, high structural stability, and the ability to rapidly generate an active phase. The key lies in the porous NiFe alloy substrate and the A-FeS... x Synergistic effect with the Ni3S2 composite catalyst layer. Specifically, the porous NiFe alloy substrate not only serves as a three-dimensional self-supporting conductive framework, significantly reducing interfacial contact resistance, but its pore structure also provides efficient mass transfer channels for electrolyte wetting and rapid desorption of oxygen bubbles, thereby ensuring stable operation under high current densities. Furthermore, the alloy substrate of this invention has a significant advantage in overpotential compared to powder-synthesized nickel-iron or foamed nickel-iron substrates, at 100 mA·cm⁻¹. -2 The overpotential decreased by approximately 150 mV. Simultaneously, the in-situ grown A-FeS... xThe Ni3S2 composite catalyst layer forms a tight bond with the substrate, with the crystalline Ni3S2 providing high-speed electron transport, while the amorphous FeS... x The porous NiFe alloy substrate is rich in dangling bonds and coordinately unsaturated Fe sites, serving as active centers for preferential adsorption of hydroxyl groups and triggering surface reconstruction. At the crystalline-amorphous heterogeneous interface, strong electronic interactions induce electron delocalization at Ni sites and electron enrichment at Fe sites, effectively enhancing metal-oxygen covalentity, promoting lattice oxygen activation and O / O bond coupling, thereby lowering the oxygen evolution reaction energy barrier. More importantly, the porous NiFe alloy substrate can gradually dissolve Ni and Fe ions under alkaline oxidation potential, continuously replenishing the active components and interacting with the amorphous FeS... x Rapid pre-oxidation synergistically accelerates A-FeS x The reconstruction of / Ni3S2 into the highly active Ni(Fe)OOH phase achieved a synergistic improvement in catalyst activity and stability.
[0012] The amorphous FeS prepared by this invention x The modified Ni3S2 self-supporting oxygen evolution precatalyst exhibits a nanoflower morphology composed of nanosheets. This morphology not only significantly increases the specific surface area of the material, exposing more active sites, but also the open pores promote rapid electrolyte wetting, ion transport, and timely desorption of oxygen bubbles during oxygen evolution, avoiding dead zones caused by bubbles covering active sites. In this invention, A-FeS... x In the middle, A represents the amorphous phase.
[0013] As a preferred embodiment, the molar percentage of Fe in the porous NiFe alloy substrate is 10-30%. By controlling the molar percentage of Fe in the porous NiFe alloy substrate, the in-situ formation of the amorphous FeS phase on its surface can be indirectly controlled. x The ratio of the crystalline phase Ni3S2 to the α-FeS2 phase further affects the α-FeS2 phase. x The degree of amorphousness of Ni3S2 is controlled to achieve a better balance between conductivity, number of active sites, and structural stability in the overall catalytic material. A further preferred value is 20-25%.
[0014] As a preferred embodiment, the porosity of the porous NiFe alloy substrate is 30-70%. Within the porosity range selected in this invention, both electrolyte wetting and rapid desorption of oxygen bubbles can be ensured, while also avoiding instability of the catalyst structure.
[0015] As a preferred embodiment, the A-FeS x The thickness of the Ni3S2 composite catalyst layer is 10 nm to 5 μm. In this invention, the thickness of the catalyst layer is mainly controlled based on the hydrothermal synthesis time and the amount of complexing agent and sulfur source added.
[0016] As a preferred embodiment, the A-FeS x / Ni3S2 composite catalyst layer A-FeS x The molar ratio of Ni3S2 is (1-3): (9-7). Within the further preferred molar ratio range of this invention, catalysts with superior catalytic performance can be obtained. This invention also provides an amorphous FeS2 phase... x A method for preparing a modified Ni3S2 self-supported oxygen evolution precatalyst, comprising the following steps:
[0017] S1 mixes nickel powder, iron powder and organic pore-forming agent, and the resulting slurry is coated and cured, and then vacuum sintered to obtain a porous NiFe alloy substrate;
[0018] The porous NiFe alloy substrate described in S2 undergoes a hydrothermal reaction under the action of an alkaline solution and a complexing agent to obtain a porous NiFe alloy substrate@NiFe-LDH precursor;
[0019] The porous NiFe alloy substrate @NiFe-LDH precursor described in S3 undergoes a hydrothermal sulfidation reaction with a sulfur source in solution to obtain the porous NiFe alloy substrate @A-FeS. x / Ni3S2 composite catalyst layer.
[0020] The method of this invention can obtain porous NiFe alloy substrates @A-FeS x The principle behind the Ni3S2 composite catalyst layer is as follows: First, nickel powder and iron powder are uniformly mixed and sintered at high temperature under vacuum conditions, allowing Ni and Fe to diffuse into each other and form a metallic alloy. Simultaneously, an organic pore-forming agent decomposes and is removed to form a porous structure, resulting in a porous NiFe alloy substrate that can provide a self-supporting conductive network and serve as a base for subsequent reactions. Subsequently, under alkaline hydrothermal conditions, in-situ oxidation and corrosion occur on the substrate surface, precipitating Ni and Fe ions, which then react with OH-. - Coordination, with the assistance of a complexing agent, allows for the controllable growth of a NiFe-LDH precursor layer with better morphology on the surface of a porous NiFe alloy substrate, achieving a tight bond between the catalyst layer and the substrate; finally, during the hydrothermal sulfidation process containing a sulfur source, Ni and Fe ions are utilized in conjunction with S... 2- The difference in reactivity causes Ni to preferentially sulfide and form a crystalline Ni3S2 conductive framework, while some Fe exists as an amorphous FeS2 structure. x The form is deposited on the surface of the crystalline phase, forming A-FeS with a crystalline-amorphous heterogeneous interface. x / Ni3S2 composite catalyst layer.
[0021] As a preferred embodiment, in S1, the molar ratio of nickel powder to iron powder is (9~7):(1~3). In this invention, controlling the molar ratio of nickel powder to iron powder indirectly controls the amorphous FeS phase in the composite catalyst layer.x The ratio of the crystalline phase Ni3S2 to the overall catalytic material achieves a good balance between conductivity, number of active sites, and structural stability.
[0022] As a preferred embodiment, the organic pore-forming agent comprises at least one of polyvinyl butyral, polyvinyl alcohol, and polymethacrylate. Polyvinyl butyral is more preferably preferred.
[0023] As a preferred embodiment, the amount of the organic pore-forming agent is 1-5% relative to the total amount of nickel powder and iron powder. This invention controls the porosity of the porous NiFe alloy substrate by controlling the amount of the organic pore-forming agent.
[0024] As a preferred embodiment, the vacuum sintering temperature is 700~900℃, and the time is 1~4h. Within the vacuum sintering temperature range of the present invention, Ni and Fe can achieve sufficient solid-phase diffusion to form a homogeneous NiFe alloy solid solution single phase, while simultaneously achieving the decomposition and removal of the organic pore-forming agent.
[0025] As a preferred embodiment, in S2, the alkaline solution includes urea. When urea is further preferred, a uniform alkaline environment can be provided through slow hydrolysis, enabling controllable crystal growth.
[0026] As a preferred option, the amount of urea added is 150~500 mmol / L.
[0027] As a preferred embodiment, the complexing agent comprises ammonium fluoride. This invention utilizes a complexing agent to further slow down the reaction rate through complexation, and when used in conjunction with urea, it can better achieve morphology control of NiFe-LDH.
[0028] As a preferred option, the amount of ammonium fluoride added is 50~250 mmol / L.
[0029] As a preferred embodiment, the hydrothermal reaction temperature is 90~130℃, and the time is 3~8h. The hydrothermal reaction temperature affects the nucleation rate and growth morphology of the NiFe-LDH precursor on the porous NiFe alloy substrate. Within the preferred temperature and time range of this invention, a NiFe-LDH precursor layer with a more uniform morphology and a tighter bond to the substrate can be obtained.
[0030] As a preferred embodiment, in step S3, the sulfur source includes at least one of sodium sulfide, elemental sulfur, and thiourea. Sodium sulfide is more preferably preferred.
[0031] As a preferred embodiment, the amount of sulfur source added is 150~400 mmol / L. The amount of sulfur source added in this invention affects the thickness of the catalyst layer and the crystallinity of the synthesized crystals.
[0032] As a preferred embodiment, the hydrothermal sulfidation reaction is carried out at a temperature of 120-180°C for 2-6 hours. Too low a hydrothermal temperature or too short a time will result in incomplete synthesis and residual LDH; while too high a temperature or too long a time will cause the catalyst morphology and structure to collapse, severely affecting catalyst performance.
[0033] The present invention also provides an amorphous phase FeS x The application of the modified Ni3S2 self-supporting oxygen evolution precatalyst as a catalyst in the alkaline water electrolysis oxygen evolution reaction (OER). The precatalyst of this invention undergoes surface reconstruction during the alkaline OER, generating a Ni(Fe)OOH active phase, significantly reducing the OER reaction energy barrier.
[0034] As a preferred option, it serves as the anode catalytic electrode in an alkaline water electrolyzer.
[0035] Finally, the present invention also provides an alkaline water electrolyzer, comprising an anode, a cathode, and an alkaline electrolyte; the anode comprises the aforementioned amorphous phase FeS. x A self-supporting oxygen evolution precatalyst modified with Ni3S2 crystalline phase.
[0036] Compared with the prior art, the present invention has the following beneficial effects:
[0037] (1) The amorphous FeS provided by the present invention x A modified crystalline Ni3S2 self-supporting oxygen evolution precatalyst, by introducing transition metal sulfur-containing compounds to improve catalyst conductivity while utilizing the amorphous FeS phase... x The porous NiFe alloy substrate, which forms a crystalline-amorphous heterogeneous interface with the crystalline Ni3S2, provides abundant active sites and promotes rapid interfacial charge transfer.
[0038] (2) The preparation method provided by the present invention allows the catalyst layer to be grown directly in situ on a porous NiFe alloy substrate, resulting in a tight bond between the materials. Then, A-FeS is generated simultaneously through a hydrothermal sulfidation reaction. x The / Ni3S2 composite catalyst layer has advantages such as simple process and readily available raw materials.
[0039] (3) The amorphous FeS provided by the present invention x A modified Ni3S2 self-supporting oxygen evolution precatalyst was applied to the alkaline water electrolysis oxygen evolution reaction (OER). During the alkaline OER process, it rapidly reconstructs into the Ni(Fe)OOH active phase, improving reaction kinetics and significantly lowering the OER energy barrier. When the current density reaches 100 mA·cm⁻¹, [the reaction proceeds smoothly].2 At that time, the oxygen evolution overpotential was only 217mV.
[0040] (4) The catalyst of the present invention is grown directly in situ on a porous NiFe alloy substrate without the need for additional binders and conductive additives, thus avoiding the problems of binders covering active sites and increasing contact resistance in traditional powder electrodes.
[0041] (5) The catalyst of the present invention can be used as the anode of an alkaline water electrolyzer and maintains stable operation under high temperature, high concentration of KOH and industrial-grade current density, and has good application prospects. Attached Figure Description
[0042] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will now be described in detail with reference to the accompanying drawings.
[0043] Figure 1 The amorphous FeS of the present invention x A schematic diagram of the preparation process of the modified Ni3S2 self-supporting oxygen evolution precatalyst.
[0044] Figure 2 The porous NiFe alloy substrate, NiFe-LDH precursor, and A-FeS prepared in Example 1 x SEM images of Ni3S2, where a is the porous NiFe alloy substrate, b is the NiFe-LDH precursor, and c is the Al-FeS2 substrate. x / Ni3S2.
[0045] Figure 3 It consists of crystalline Ni3S2 and amorphous FeS x HRTEM diagram of heterogeneous interface structure.
[0046] Figure 4 A-FeS prepared in Example 1 x Raman spectrum of the reconstructed Ni(Fe)OOH active phase by Ni3S2 during alkaline OER process.
[0047] Figure 5 A-FeS prepared in Example 1 x A schematic diagram of an apparatus using Ni3S2 as the anode in an alkaline water electrolysis cell. Where a represents A-FeS... x A schematic diagram of the oxygen evolution system in an alkaline water electrolyzer using Ni3S2 as the anode, and b is the OER process route diagram of the alkaline water electrolyzer.
[0048] Figure 6 A-FeS x / Ni3S2、C-FeS x / Ni3S2、FeS xA comparison of the catalytic performance of Ni3S2 and Ruhr (commercial ruthenium-iridium electrode), where a is the overpotential comparison, b is the Tafel slope, c is the EIS, d is the double-layer capacitance, and C-FeS x The x value of / Ni3S2 is 2. Detailed Implementation
[0049] The following specific examples illustrate the implementation of the present invention. Those skilled in the art can easily understand other advantages and effects of the present invention from the content disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention.
[0050] The present invention will be further described below with reference to the accompanying drawings and specific embodiments, so that those skilled in the art can better understand and implement the present invention. However, the embodiments described are not intended to limit the present invention.
[0051] Example 1
[0052] An amorphous phase FeS x The modified Ni3S2 self-supporting oxygen evolution precatalyst is obtained by the following preparation steps:
[0053] S1 mixes nickel-iron powder (molar ratio of nickel powder to iron powder is 4:1) with PVB solution to form a metal slurry, which is then used to make a metal foil precursor. The metal foil precursor is dried and then placed in a vacuum sintering furnace for vacuum sintering to form a porous nickel-iron substrate.
[0054] S2 cuts the porous nickel-iron substrate to a size of 1×1.5cm. 2 The porous nickel-iron substrate was then cleaned three times with deionized water and ethanol to remove oil and impurities from its surface.
[0055] S3 prepared a hydrothermal solution of Na2S·9H2O aqueous solution, and placed it with a porous nickel-iron substrate in a polytetrafluoroethylene reactor. The reaction was carried out at 150°C for 6 hours. After the reactor cooled down, the electrode was removed and washed three times with deionized water and ethanol. Then it was placed in a vacuum drying oven at 60°C for drying and ready for use, resulting in a porous NiFe alloy substrate (porosity of 50%).
[0056] S4 cut the above-mentioned porous NiFe alloy substrate into 1cm×1cm pieces and ultrasonically cleaned them until neutral. The substrate was then placed in 20mL of deionized water containing 6mmol urea and 3mmol ammonium fluoride, and subsequently transferred to a polytetrafluoroethylene high-pressure reactor liner.
[0057] S5 The reactor was placed in an oven at 110℃ for hydrothermal reaction for 5 hours. After the reaction was completed, it was naturally cooled to room temperature, the sample was taken out and ultrasonically cleaned, and then vacuum dried at 50℃ for 12 hours to obtain the NiFe-LDH precursor grown in situ on the surface of the porous NiFe alloy substrate (i.e., porous NiFe alloy substrate@NiFe-LDH precursor), denoted as NiFe-LDH precursor.
[0058] S6 placed the NiFe-LDH precursor in 20 mL of deionized water containing 5 mmol Na2S·9H2O and transferred it to the liner of a polytetrafluoroethylene high-pressure reactor. The reactor was then placed in a 150℃ oven for hydrothermal reaction for 4 h to allow the NiFe-LDH precursor to undergo in-situ sulfidation.
[0059] After the S7 reaction was completed and the mixture was allowed to cool naturally to room temperature, the resulting product was washed three times with deionized water and ethanol to remove surface residues. It was then vacuum dried at 50°C for 12 hours to obtain amorphous FeS. x Self-supporting composite precatalyst for modified crystalline Ni3S2 (i.e., porous NiFe alloy substrate @A-FeS) x / Ni3S2 composite catalyst layer, A-FeS x The thickness of the / Ni3S2 composite catalyst layer is 1μm, and the A-FeS x The molar ratio of Ni3S2 is 1:4, denoted as A-FeS. x / Ni3S2, where x is 1~2.
[0060] S8 will A-FeS x Ni3S2 was used directly as the working electrode for testing the alkaline oxygen evolution reaction in 1.0M KOH electrolyte. Because the catalyst has a self-supporting structure, no binder such as Nafion was required before testing.
[0061] The result is Figure 4 As shown, Figure 4 This indicates that during the electrochemical activation process, A-FeS x The Ni3S2 surface undergoes remodeling, and the sulfide precatalyst gradually transforms into the Ni(Fe)OOH active phase. x The presence of [something] promotes the reconstruction process, enables the rapid generation of the active phase, and improves the charge transfer efficiency and active site utilization in the oxygen evolution reaction.
[0062] S9 will be A-FeS x Using Ni3S2 as the anode and Raney nickel as the cathode in an alkaline water electrolyzer, and a 30% KOH solution as the electrolyte, an overall water decomposition test was conducted at 80℃. A schematic diagram is shown below. Figure 5 As shown.
[0063] Under industrial-grade current density conditions, this anode catalyst exhibits low electrolyzer voltage and excellent long-term stability, indicating that it can be used as an anode material for industrial alkaline water electrolysis.
[0064] Depend on Figure 2 This confirms that the A-FeS prepared in this embodiment... x The / Ni3S2 catalyst exhibits a nanoflower-like morphology composed of nanosheets.
[0065] Depend on Figure 3 The successful formation of A-FeS in the composite catalyst layer was confirmed. x It and Ni3S2, and there is a crystalline-amorphous heterogeneous interface between the two.
[0066] Example 2
[0067] The only difference between this embodiment and Example 1 is that the molar ratio of nickel powder to iron powder is changed to 9:1; all other steps and conditions are the same, yielding A-FeS. x / Ni3S2-1.
[0068] When the current density reaches 100 mA·cm 2 At that time, the oxygen evolution overpotential was 290mV.
[0069] Example 3
[0070] The only difference between this embodiment and Example 1 is that the molar ratio of nickel powder to iron powder is changed to 7:3; all other steps and conditions are the same, yielding A-FeS. x / Ni3S2-2.
[0071] When the current density reaches 100 mA·cm 2 At that time, the oxygen evolution overpotential was 250mV.
[0072] Comparative Example 1
[0073] 1.6 g of ferric chloride hexahydrate was added to 50 mL of ethylene glycol. 0.6 g of sodium citrate was added. The mixture was in a water bath at 80 °C with stirring and ultrasonic treatment for 1 hour until a thick, orange-yellow solution was formed. The mixture was transferred to a vacuum oven and dried for 12 hours. The product was collected and reacted in a muffle furnace at 150 °C for 2 hours to obtain Fe2O3 particles. C-FeS2 / Ni3S was synthesized by placing nickel foam and Fe2O3 particles downstream of sulfur powder upstream in a tubular furnace and sulfiding at 150 °C for 2 hours. 2。
[0074] Comparative Example 2
[0075] The preparation of this comparative example differs from that of Example 1 only in that the substrate is replaced with foamed iron; all other steps and conditions are the same, yielding FeS. x .
[0076] Comparative Example 3
[0077] The preparation of this comparative example differs from that of Example 1 only in that the substrate is replaced with nickel foam; all other steps and conditions are the same, yielding Ni3S2.
[0078] Comparative Example 4
[0079] This comparative example uses commercially available ruthenium-iridium electrodes (Rulr), purchased from Octagonal Metals.
[0080] Figure 6 A-FeS x / Ni3S2、C-FeS x / Ni3S2、FeS x Comparison of catalytic performance between Ni3S2 and Ruhr (commercial ruthenium-iridium electrode). Figure 6 As shown in a, Example 1's A-FeS x The Ni3S2 catalyst exhibits the best OER performance, reaching 100 mAcm. -2 At current density, only an overpotential of 217 mV is required, significantly lower than that of commercial RuIr catalysts (345 mV) and crystalline C-FeS. x / Ni3S2 (298mV), pure phase Ni3S2 (375mV) and pure phase FeS x (347mV). As the current density gradually increases, A-FeS x / Ni3S2 reaches 400mA cm -2 Even under high current density conditions, it can still maintain a low overpotential (η). 400 =315mV), far lower than that of commercial RuIr catalysts (469mV), which indicates that A-FeS x The Ni3S2 catalyst exhibits excellent catalytic activity and charge transport capability under various high current densities. This study aims to investigate single-phase FeS... x Ni3S2 and A-FeS x The OER kinetics of the Ni3S2 catalyst were analyzed. This study used the LSV test results to analyze the curves and obtain the Tafel slope, which can more accurately assess the reaction kinetics of the catalyst. Figure 6 As shown in b, A-FeS x The / Ni3S2 composite catalyst exhibits the smallest Tafel slope (22 mV·dec). -1 (), far lower than crystalline C-FeS x / Ni3S2 (66mV·dec) -1 ), single-phase Ni3S2 (70mV·dec) -1 ) and single-phase FeSx (100 mV·dec) -1 ).like Figure 6 As shown in c, the Nyquist curves of all samples exhibit a typical semi-circular characteristic, indicating that the electrolysis process is mainly controlled by the charge transfer process at the interface. Among them, A-FeS x The / Ni3S2 composite catalyst exhibits the smallest semi-circular diameter, indicating that it has the lowest charge transfer resistance (Rct), which is due to the FeS x Its amorphous phase characteristics result in a large number of dangling bonds and coordinate-unsaturated Fe sites on its surface, promoting the transition of electrons from the bulk catalyst phase to the surface active centers. For example... Figure 6 As shown in d, A-FeS x The / Ni3S2 composite catalyst exhibits the highest C dl The value reached 38.12 mF cm. -2 It is significantly higher than that of crystalline C-FeS2 / Ni3S2, single-phase Ni3S2, and FeS x .
Claims
1. An amorphous phase FeS x Modified Ni3S2 self-supporting oxygen evolution precatalyst, characterized in that: Includes a porous NiFe alloy substrate and A-FeS grown in situ on the surface of the porous NiFe alloy substrate. x / Ni3S2 composite catalyst layer; the A-FeS x Ni3S2 and A-FeS in the Ni3S2 composite catalyst layer x There is a crystalline-amorphous heterogeneous interface between them, where x is any number from 1 to 2.
2. The amorphous FeS phase according to claim 1 x Modified Ni3S2 self-supporting oxygen evolution precatalyst, characterized in that: The molar percentage of Fe in the porous NiFe alloy substrate is 10-30%; The porosity of the porous NiFe alloy substrate is 30-70%.
3. An amorphous FeS phase according to claim 1 or 2 x Modified Ni3S2 self-supporting oxygen evolution precatalyst, characterized in that: The A-FeS x The thickness of the / Ni3S2 composite catalyst layer is 10nm~5μm; The A-FeS x / Ni3S2 composite catalyst layer A-FeS x The molar ratio of Ni3S2 is (1~3): (9~7).
4. An amorphous FeS phase as described in any one of claims 1 to 3 x A method for preparing a modified Ni3S2 self-supporting oxygen evolution precatalyst, characterized by: step include: S1 mixes nickel powder, iron powder and organic pore-forming agent, and the resulting slurry is coated and cured, and then vacuum sintered to obtain a porous NiFe alloy substrate; The porous NiFe alloy substrate described in S2 undergoes a hydrothermal reaction under the action of an alkaline solution and a complexing agent to obtain a porous NiFe alloy substrate@NiFe-LDH precursor; The porous NiFe alloy substrate @NiFe-LDH precursor described in S3 undergoes a hydrothermal sulfidation reaction with a sulfur source in solution to obtain the porous NiFe alloy substrate @A-FeS. x / Ni3S2 composite catalyst layer.
5. The amorphous FeS phase according to claim 4 x A method for preparing a modified Ni3S2 self-supporting oxygen evolution precatalyst, characterized in that: In S1, The molar ratio of nickel powder to iron powder is (9~7):(1~3); The organic pore-forming agent includes at least one of polyvinyl butyral, polyvinyl alcohol, and polymethyl methacrylate; The amount of the organic pore-forming agent used is 1-5% relative to the total amount of nickel powder and iron powder. The vacuum sintering temperature is 700~900℃ and the time is 1~4h.
6. The amorphous FeS phase according to claim 4 or 5 x A method for preparing a modified Ni3S2 self-supporting oxygen evolution precatalyst, characterized in that: In S2, The alkaline solution includes urea, and the amount of urea added is 150~500 mmol / L; The complexing agent includes ammonium fluoride, and the amount of ammonium fluoride added is 50~250 mmol / L; The hydrothermal reaction is carried out at a temperature of 90~130℃ for 3~8 hours.
7. The amorphous FeS phase according to claim 4 or 5 x A method for preparing a modified Ni3S2 self-supporting oxygen evolution precatalyst, characterized in that: In S3 The sulfur source includes at least one of sodium sulfide, elemental sulfur, and thiourea. The amount of sulfur source added is 150~400 mmol / L; The hydrothermal sulfidation reaction is carried out at a temperature of 120~180℃ for 2~6 hours.
8. An amorphous FeS phase as described in any one of claims 1 to 3 x The application of modified Ni3S2 self-supporting oxygen evolution precatalyst is characterized by: It is used as a catalyst in the alkaline water electrolysis oxygen evolution reaction.
9. The application according to claim 8, characterized in that: It serves as the anodic catalytic electrode in an alkaline water electrolyzer.
10. An alkaline water electrolysis cell, characterized in that: It includes an anode, a cathode, and an alkaline electrolyte; the anode comprises the amorphous FeS as described in any one of claims 1 to 3. x A self-supporting oxygen evolution precatalyst modified with Ni3S2 crystalline phase.
Citation Information
Patent Citations
Preparation method of self-supporting ferronickel layered double hydroxide sulfide electrocatalyst
CN112023946A