A fibrous manganese-doped praseodymium ferrite perovskite electrocatalyst, its preparation method, and a method for electrocatalytic reduction of nitrate to produce ammonia.
By preparing fibrous manganese-doped praseodymium ferrite perovskite electrocatalysts, the problems of insufficient active site utilization and interfacial charge transfer performance of perovskite ferrite electrocatalysts in the electrocatalytic reduction of nitrate to ammonia were solved, achieving high ammonia selectivity and long-term stability.
Patent Information
- Application Number
- CN202611418272.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-14
- Publication Date
- 2026-11-17
AI Technical Summary
Existing perovskite ferrite electrocatalysts have insufficient utilization of active sites and interfacial charge transfer performance in the electrocatalytic reduction of nitrate to ammonia, making it difficult to synergistically improve ammonia selectivity and production rate, and resulting in insufficient long-term operational stability.
A fibrous manganese-doped praseodymium ferrite perovskite electrocatalyst was used to prepare a multi-interwoven fiber network by electrospinning technology, forming an orthorhombic perovskite crystal structure with the Pnma space group, thereby optimizing the local coordination environment and electronic structure.
It improved ammonia selectivity and mass-normalized ammonia generation rate, reduced interfacial impedance, ensured long-term operational stability, and achieved efficient electrocatalytic reduction of nitrate to ammonia.
Smart Images

Figure CN123108616A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of electrocatalytic ammonia production materials technology, specifically to a fibrous manganese-doped praseodymium ferrite perovskite electrocatalyst and its preparation method, and a method for producing ammonia by electrocatalytic reduction of nitrates. Background Technology
[0002] Ammonia is a crucial basic chemical in fertilizer, chemical synthesis, and energy storage and transportation. Traditional ammonia synthesis processes typically require high temperatures and pressures, and their upstream hydrogen production processes are highly dependent on fossil fuels. Utilizing renewable electricity to achieve electrochemical ammonia synthesis under ambient temperature and pressure conditions can help reduce energy consumption and carbon emissions in the ammonia synthesis process.
[0003] Nitrates are widely found in industrial wastewater and agricultural runoff. Electrocatalytic reduction of nitrates to ammonia can remove nitrogenous pollutants while simultaneously yielding usable ammonia. However, the reduction of nitrate to ammonia involves multi-electron and multi-proton coupling transfers and various nitrogen-containing intermediates, competing with the hydrogen evolution reaction. Therefore, challenges remain, including high reaction driving force, difficulty in synergistically improving ammonia selectivity and formation rate, and insufficient long-term operational stability.
[0004] ABO3-type perovskite oxides possess the characteristics of tunable composition, well-defined crystal structure, and good chemical stability. Perovskite ferrites can be used for the electrocatalytic reduction of nitrates, but there is still room for improvement in the utilization rate of active sites and interfacial charge transfer performance. Introducing Mn at the B site can regulate the local coordination environment and electronic structure; simultaneously, constructing the material as an interwoven one-dimensional fiber network is beneficial for increasing the active surface accessible to the electrolyte and forming continuous electron transport channels.
[0005] Therefore, it is still necessary to develop fibrous Mn-doped praseodymium ferrite perovskite electrocatalysts with well-defined composition and controllable morphology, and to systematically investigate the effects of Mn doping on ammonia production selectivity, mass-normalized ammonia generation rate, interfacial impedance, and long-term operational stability. Summary of the Invention
[0006] To improve the utilization of active sites and interfacial charge transfer performance of praseodymium ferrite perovskite electrocatalysts in the nitrate reduction process, and to enhance ammonia selectivity, mass-normalized ammonia generation rate, and long-term operational stability, this invention proposes a fibrous manganese-doped praseodymium ferrite perovskite electrocatalyst, its preparation method, and a method for ammonia production by electrocatalytic reduction of nitrate.
[0007] The specific technical solution of the present invention is as follows: A fibrous manganese-doped praseodymium ferrite perovskite electrocatalyst, the nominal chemical composition of which is PrFe 0.8 Mn 0.2 O3, and is composed of multiple interwoven fibers forming a fiber network.
[0008] Preferably, the electrocatalyst has an orthorhombic perovskite crystal structure as determined by X-ray diffraction, with space group Pnma (No. 62) and its equivalent axis set to Pbnm.
[0009] The present invention also provides a method for preparing the above-mentioned fibrous manganese-doped praseodymium ferrite perovskite electrocatalyst, comprising the following steps: S1. Prepare a metal precursor solution with a molar ratio of Pr, Fe and Mn of 1:0.8:0.2; S2. Mix the metal precursor solution with the spinning polymer solution to obtain the precursor spinning solution; S3. Electrospin the precursor spinning solution to obtain precursor fibers. S4. The precursor fiber is dried and heat-treated to remove the spinning polymer and form PrFe. 0.8 Mn 0.2 O3 perovskite phase.
[0010] Preferably, the Pr precursor is Pr(NO3)3·6H2O, the Fe precursor is Fe(NO3)3·9H2O, the Mn precursor is Mn(NO3)2·4H2O, the spinning polymer is polyvinylpyrrolidone, and the solvent is N,N-dimethylformamide.
[0011] Preferably, in step S1, 435 mg Pr(NO3)3·6H2O, 323 mg Fe(NO3)3·9H2O and 50 mg Mn(NO3)2·4H2O are added to 2 mL of N,N-dimethylformamide; in step S2, 1 g of polyvinylpyrrolidone is dissolved in 8 mL of N,N-dimethylformamide, and the metal precursor solution and the spinning polymer solution are mixed at a volume ratio of 1:4.
[0012] Preferably, in step S3, the electrospinning potential difference is 18 kV and the liquid supply rate is 1.0 mL / h. -1 The distance from the needle to the receiver was 20 cm, the ambient temperature was 25 ℃, the relative humidity was 76%, and the rotation speed of the roller receiver was 800 r / min. -1 The spinning time is 10 hours.
[0013] Preferably, step S4 includes: vacuum drying the precursor fiber at 80 °C for 6 h; and drying at 2 °C for 1 minute. -1 The temperature was increased to 200 °C at a heating rate and held for 5 h; then heated to 200 °C at a rate of 1 °C / min in air atmosphere. -1 The heating rate was increased to 600℃ and held for 0.5 h.
[0014] The present invention also provides an electrode for the electrocatalytic reduction of nitrate to ammonia, comprising a conductive substrate and the fibrous manganese-doped praseodymium ferrite perovskite electrocatalyst supported on the conductive substrate.
[0015] The present invention also provides a method for producing ammonia by electrocatalytic reduction of nitrate, wherein the aforementioned electrocatalytic reduction ammonia production electrode is used as the working electrode, and a reduction potential or reduction current is applied in an alkaline electrolyte containing nitrate to reduce nitrate to produce ammonia.
[0016] Preferably, the alkaline electrolyte contains 1.0 mol L. -1 KOH and 0.1 mol L -1 Or 1.0 mol L - 1 KNO3; the reduction potential is -0.3 V to -0.9 V relative to the reversible hydrogen electrode; the reduction current is 600 mA cm⁻¹. -2 .
[0017] Compared with the prior art, the specific beneficial effects of the present invention are as follows: (1) Fibrous PrFe 0.8 Mn 0.2 O3 is composed of interwoven one-dimensional fibers and has an orthorhombic perovskite crystal structure with the Pnma space group (No. 62; Pbnm is the equivalence axis). In XRD Rietveld refinement, PrFeO3 and PrFe... 0.8 Mn 0.2 R of O3 and PrMnO3 wp The percentages were 3.08%, 3.17%, and 3.58%, respectively, indicating that the refined calculated spectrum and the measured spectrum have good consistency.
[0018] (2) Estimate the specific capacitance of fibrous PrFeO3 and PrFe under the same empirical specific capacitance assumption. 0.8 Mn 0.2 The apparent electrochemical active surface areas of O3 and PrMnO3 are 9.01 cm², respectively. 2 14.91 cm 2 and 12.66 cm 2 ; at 1.0 mol·L - 1 KOH and 1.0 mol·L -1 Under the conditions of KNO3, -0.6 V relative to RHE, PrFe 0.8 Mn 0.2 The Nyquist semicircle of O3 is smaller than that of the other two control materials, indicating that it has a lower apparent interfacial impedance.
[0019] (3) At 1.0 mol·L -1 KOH and 1.0 mol·L -1 In KNO3, fibrous PrFe 0.8 Mn 0.2 O3 achieved an ammonia faradaic efficiency of 96.81% and a yield of 257.03 mg at -0.9 V relative to RHE. NH3 ·h -1 ·mg cat -1 The mass-normalized ammonia formation rate.
[0020] (4) Mn doping exhibits a significant promoting effect under relatively small reduction driving forces. At 1.0 mol·L⁻¹ -1 KOH and 1.0 mol·L -1 At KNO3 and -0.3 V relative to RHE, the ammonia Faraday efficiency increased from 61.94% for fibrous PrFeO3 to that for fibrous PrFeO3. 0.8 Mn 0.2 The concentration of O3 was 82.10%, an absolute increase of 20.16 percentage points and a relative increase of 32.55%; the mass-normalized ammonia formation rate increased from 8.44 mg NH3 ·h -1 ·mg cat -1 Increased to 14.43 mg NH3 ·h -1 ·mg cat -1 This represents a relative increase of 70.97%.
[0021] (5) At 1.0 mol·L -1 KOH and 0.1 mol·L -1 In KNO3, fibrous PrFe 0.8 Mn 0.2 The highest ammonia Faraday efficiency of O3 was 96.26%, and the highest mass-normalized ammonia formation rate was 168.27 mg. NH3 ·h -1 ·mg cat -1 At -0.4 V relative to RHE, its ammonia Faraday efficiency and mass-normalized ammonia formation rate were increased by 20.78 percentage points and 20.06 mg, respectively, in absolute terms compared to fibrous PrFeO3. NH3 ·h -1 ·mg cat -1 .
[0022] (6) At 600 mA·cm -2In long-term constant current testing, the ammonia Faraday efficiency remained between 89.53% and 91.83% over 104 h, and was 89.66% after 104 h; the working electrode geometric area was 0.5 cm². 2 With a catalyst mass of 0.20 mg and a corresponding total current of 300 mA, the cumulative ammonia production reached 11.09 g NH3·mg after 104 h. cat -1 This indicates that the electrocatalyst has good long-term operational stability under high current density. Attached Figure Description
[0023] Figure 1 Scanning electron microscope image of fibrous PrFeO3; Figure 2 Fiber-like PrFe 0.8 Mn 0.2 Scanning electron microscope image of O3; Figure 3 Scanning electron microscope image of fibrous PrMnO3; Figure 4 The Rietveld refined XRD pattern of fibrous PrFeO3; Figure 5 Fiber-like PrFe 0.8 Mn 0.2 Retouched XRD Rietveld image of O3; Figure 6 The Rieteld refinement image of fibrous PrMnO3; Figure 7 Three fibrous perovskite materials were tested at 1.0 mol·L⁻¹. -1 KOH blank electrolyte and 1.0 mol·L - 1 KOH and 1.0 mol·L -1 Linear sweep voltammetry curves in KNO3 mixed electrolyte; Figure 8 Three fibrous perovskite materials were tested at 1.0 mol·L⁻¹. -1 KOH and 1.0 mol·L -1 Ammonia Faraday efficiency and mass-normalized ammonia formation rate under KNO3 conditions; Figure 9 Fiber-like PrFe 0.8 Mn 0.2 O3 at 600 mA·cm -2 Ammonia Faraday efficiency and cumulative ammonia production during a 104-hour operation under constant current conditions; Figure 10Three fibrous perovskite materials were tested at 1.0 mol·L⁻¹. -1 KOH and 1.0 mol·L -1 Nyquist plot of KNO3, -0.6 V relative to RHE condition; Figure 11 The results of fitting the capacitance current density to the scan rate and the apparent ECSA estimation for three fibrous perovskite materials are presented. Figure 12 Three fibrous perovskite materials were tested at 1.0 mol·L⁻¹. -1 KOH blank electrolyte and 1.0 mol·L - 1 KOH and 0.1 mol·L -1 Linear sweep voltammetry curves in KNO3 mixed electrolyte; Figure 13 Three fibrous perovskite materials were tested at 1.0 mol·L⁻¹. -1 KOH and 0.1 mol·L -1 Ammonia Faraday efficiency and mass-normalized ammonia formation rate under KNO3 conditions. Detailed Implementation
[0024] To make the technical solutions of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. It should be noted that the following embodiments are only used to better understand the technical solutions of the present invention and should not be construed as limiting the present invention.
[0025] Example 1. This embodiment prepares fibrous PrFe 0.8 Mn 0.2 The specific steps for using O3 perovskite electrocatalyst are as follows: (1) Preparation of metal precursor solution: Weigh 435 mg of praseodymium nitrate hexahydrate Pr(NO3)3·6H2O, 323 mg of ferric nitrate nonahydrate Fe(NO3)3·9H2O, and 50 mg of manganese nitrate tetrahydrate Mn(NO3)2·4H2O, so that the molar ratio of Pr, Fe, and Mn is 1∶0.8∶0.2; add 2 mL of N,N-dimethylformamide and stir for 1 h. The total amount of metal ions is about 2 mmol, and the corresponding total metal ion concentration in the metal precursor solution is about 1.0 mol·L. -1 .
[0026] (2) Preparation of spinning polymer solution: Add 1 g of polyvinylpyrrolidone with an average molecular weight of about 200,000 to 8 mL of N,N-dimethylformamide and stir at 60 °C for 5 h until completely dissolved.
[0027] (3) Preparation of precursor spinning solution: Mix the metal precursor solution and the spinning polymer solution at a volume ratio of 1:4, continue stirring for 5 h, and then let stand for 2 h to remove bubbles.
[0028] (4) Electrospinning: The precursor spinning solution was loaded into a 10 mL syringe and connected to an 18 G needle, so that the needle was at a potential of -18 kV relative to the receiver, and the liquid supply rate was 1.0 mL·h. -1 The distance from the needle tip to the roller receiver was 20 cm; the ambient temperature was 25 ℃, the relative humidity was 76%, the spinning time was 10 h, and the roller speed was 800 r·min. -1 , to obtain precursor fibers.
[0029] (5) Drying and heat treatment: The precursor fibers were dried under vacuum at 80 °C for 6 h; and then dried at 2 °C·min. -1 The temperature was increased to 200 °C at a heating rate and held for 5 h, then heated in air at a rate of 1 °C·min. -1 The heating rate was continued to increase to 600℃ and held for 0.5 h. After natural cooling, fibrous PrFe was obtained. 0.8 Mn 0.2 O3.
[0030] Example 2. To provide a univariate control, fibrous PrFeO3 and fibrous PrMnO3 were prepared using the same polymer amounts, solvent volumes, electrospinning conditions, and heat treatment procedures as in Example 1, except for the composition of the B-site metal precursor. No Mn precursor was added during the preparation of fibrous PrFeO3, and the molar ratio of Pr to Fe was 1:1; no Fe precursor was added during the preparation of fibrous PrMnO3, and the molar ratio of Pr to Mn was 1:1.
[0031] Example 3. This embodiment involves the preparation of a catalytic electrode and the testing of its nitrate electroreduction performance, as detailed below: (1) Preparation of catalytic electrode: Weigh 10 mg of catalyst, add 9.8 mL of isopropanol and 200 μL of 5% Nafion dispersion, and sonicate for 10 min to obtain a concentration of 1.0 mg·mL -1 Catalyst ink. 100 μL of catalyst ink was loaded onto an effective area of 0.5 cm². 2 On TGP-H-060 hydrophilic carbon paper, the corresponding catalyst mass was 0.10 mg; after drying at 120 ℃ for 2 h, a catalyst loading of 0.2 mg·cm³ was obtained. -2 The working electrode. All three catalyst electrodes were prepared using the same geometric area, catalyst mass, and binder ratio.
[0032] (2) Electrochemical testing: An H-type electrolytic cell was used, with the cathode and anode chambers separated by a Nafion 211 membrane that had been soaked in deionized water for 1 h before use; the catalytic electrode was used as the working electrode, the Hg / HgO electrode as the reference electrode, and a 2 cm × 2 cm Pt mesh as the counter electrode. Unless otherwise specified in the long-term cycling test of Example 7, the volumes of the cathode and anode electrolytes were both 25 mL. The cathode electrolyte was 1.0 mol·L⁻¹. -1 KOH and 0.1 mol·L -1 Or 1.0 mol·L -1 A mixed solution of KNO3; the blank electrolyte is 1.0 mol·L⁻¹. -1 KOH; the anolyte is 1.0 mol·L⁻¹. -1 The packing solution for the KOH-Hg / HgO reference electrode was 1.0 mol·L⁻¹. -1 KOH. The test temperature was 25 ℃, and the cathode electrolyte was injected at a rate of 1000 r·min during the test. -1 Stir. Before testing, bubble with Ar for 15 min; during testing, do not continuously introduce Ar. At 25 °C, all potentials are determined according to E. RHE =E Hg / HgO +0.098 V + 0.0591 × pH converted to the reversible hydrogen electrode (RHE) scale. All electrochemical data were not iR compensated. Linear sweep voltammetry was performed from +0.2 V to -1.0 V at a scan rate of 10 mV·s. -1 The constant potential ammonia production test potentials were -0.3V, -0.4V, -0.5V, -0.6V, -0.7V, -0.8V, and -0.9V, with each potential lasting for 40 minutes.
[0033] (3) Ammonia quantification: The ammonia produced was determined using the indophenol blue method. Take 2 mL of cathode electrolyte and dilute as needed, then add 2 mL of colorimetric reagent A and 1 mL of 0.05 mol·L⁻¹ solution sequentially. -1 NaClO solution and 0.2 mL of 1% sodium nitrosoferricyanide solution; colorimetric reagent A is 1 mol·L⁻¹. -1 A NaOH solution containing 5% salicylic acid and 5% sodium citrate by mass was prepared. After thorough mixing, the mixture was incubated at 25 °C for 60 min for color development, and the absorbance was measured at 655 nm. The ammonia production was calculated based on the ammonia standard curve. The ammonia Faradaic efficiency was calculated according to FE. NH3 =8Fn NH3 Calculated as / Q×100%; mass-normalized ammonia formation rate is calculated as r NH3 =m NH3 / (t·m cat ) Calculate. Where F is the Faraday constant, nNH3 The amount of ammonia produced is given by m, where Q is the absolute value of the total charge passing through the working electrode, and m is the amount of ammonia produced by the working electrode. NH3 The mass of ammonia produced is given by t, where t is the constant potential test time, and m is the mass of ammonia produced by t. cat This represents the mass of the catalyst on the working electrode.
[0034] Example 4. This embodiment characterizes the morphology, crystal structure, and interfacial electrochemical properties of three fibrous materials.
[0035] Scanning electron microscopy results as follows Figures 1 to 3 As shown, fibrous PrFeO3 and PrFe 0.8 Mn 0.2 Both O3 and PrMnO3 exhibit an interwoven one-dimensional fiber morphology; based on the 500 nm scale bar in the figure, the fiber diameter is estimated to be mainly approximately 0.1–0.3 μm. The XRD Rietveld refinement results are as follows: Figures 4 to 6 As shown, all three materials form orthorhombic perovskite phases in the Pnma space group (No. 62; Pbnm is the equivalence axis setting); PrFeO3, PrFe 0.8 Mn 0.2 R of O3 and PrMnO3 p The percentages were 2.39%, 2.57%, and 2.60%, respectively. wp They were 3.08%, 3.17%, and 3.58%, respectively.
[0036] At the selected non-Radida potentials, at values of 20, 40, 60, 80, 100, and 120 mV·s -1 Cyclic voltammetry tests were performed at a scan rate. Half the difference between the anode and cathode current densities (Δj / 2) was taken as the capacitance current density, and the slope obtained by fitting it to the scan rate was the double-layer capacitance C per unit geometric area. dl,geo Apparent electrochemically active surface area is calculated according to ECSA=C dl,geo ×A geo / C s Calculate, where A geo 0.5 cm 2 C s Take 40 μF·cm -2 This value is an empirical specific capacitance commonly used in the estimation of apparent ECSA for oxide electrodes. It is only used for relative comparison of three samples under the same test and calculation conditions, and the resulting ECSA does not represent the absolute true surface area. Figure 11 As shown, fibrous PrFeO3 and PrFe 0.8 Mn 0.2 The apparent ECSA of O3 and PrMnO3 were 9.01 cm⁻¹. 2 14.91 cm 2and 12.66 cm 2 .
[0037] At 1.0 mol·L -1 KOH and 1.0 mol·L -1 Nyquist curves were acquired under the same conditions as RHE, using KNO3 and -0.6 V. (Example: ...) Figure 10 As shown, PrFe 0.8 Mn 0.2 The high and mid-frequency semicircular diameters of O3 are smaller than those of PrFeO3 and PrMnO3, indicating that its apparent interfacial impedance is lower under the test conditions.
[0038] Example 5. This embodiment evaluates three fibrous materials at 1.0 mol·L⁻¹ -1 KOH and 1.0 mol·L -1 The electroreduction performance of nitrates in KNO3. After the addition of KNO3, the absolute values of the cathode current densities of all three electrodes were higher than 1.0 mol·L⁻¹. -1 The KOH blank electrolyte showed a significant increase, see Figure 7 The potential-wise ammonia Faraday efficiency and mass-normalized ammonia formation rate are shown in [reference needed]. Figure 8 .
[0039] Depend on Figure 8 It can be seen that fibrous PrFe 0.8 Mn 0.2 The ammonia Faraday efficiency of O3 increased from 82.10% to 96.81% with a negative potential shift, and reached 257.03 mg at -0.9 V relative to RHE. NH3 ·h -1 ·mg cat -1 The mass-normalized ammonia formation rates were calculated. At the same potential, the ammonia Faradaic efficiencies of PrFeO3 and PrMnO3 were 80.18% and 82.18%, respectively, with mass-normalized ammonia formation rates of 221.39 and 194.00 mg, respectively. NH3 ·h -1 ·mg cat -1 At -0.3 V relative to RHE, PrFe 0.8 Mn 0.2 The ammonia Faraday efficiency of O3 is 20.16 percentage points higher than that of PrFeO3, indicating that Mn doping can still significantly improve ammonia production selectivity even with a small reduction driving force.
[0040] Example 6. This embodiment evaluates three fibrous materials at 1.0 mol·L⁻¹ -1 KOH and 0.1 mol·L-1 Electroreduction performance of nitrates in KNO3. Linear sweep voltammetry curves are shown below. Figure 12 The potential-wise ammonia Faraday efficiency and mass-normalized ammonia formation rate are shown in [reference needed]. Figure 13 .
[0041] Depend on Figure 13 It can be seen that fibrous PrFe 0.8 Mn 0.2 O3 achieved the highest ammonia faradaic efficiency of 96.26% at -0.6 V relative to RHE, and the highest mass-normalized ammonia formation rate of 168.27 mg at -0.9 V relative to RHE. NH3 ·h -1 ·mg cat -1 At -0.4 V relative to RHE, its ammonia Faraday efficiency increased from 68.22% for PrFeO3 to 89.00%, an absolute increase of 20.78 percentage points; the mass-normalized ammonia formation rate increased from 12.42 mg / L to 32.48 mg / L. NH3 ·h -1 ·mg cat -1 An absolute increase of 20.06 mg. NH3 ·h -1 ·mg cat -1 .
[0042] Example 7. This embodiment uses 1.0 mol·L⁻¹ -1 KOH and 1.0 mol·L -1 In KNO3, an effective geometric area of 0.5 cm² is used. 2 The catalyst mass is 0.20 mg (corresponding to a loading of 0.40 mg·cm³). -2 fibrous PrFe 0.8 Mn 0.2 The O3 electrode was used as the working electrode at 600 mA·cm⁻¹. -2 Long-term testing was conducted under a constant current condition (total current 300 mA). The total volume of the cathode electrolyte was 6.0 L, and it was circulated between the storage container and the cathode chamber of the H-type electrolytic cell by a peristaltic pump. Every 8 hours, 2 mL samples were taken to determine the ammonia Faraday efficiency and record the cumulative ammonia production. No electrolyte was added after each sampling. A total of 26 mL samples were taken over 104 hours, approximately 0.43% of the total cathode electrolyte volume; therefore, the volume change due to sampling was ignored in the calculations. The cumulative test was conducted for 104 hours, and the results are shown below. Figure 9 .
[0043] During long-term testing, the average ammonia Faraday efficiency was 90.61%, with a maximum of 91.83% and a minimum of 89.53%. At 104 h, the ammonia Faraday efficiency was 89.66%, representing a 98.98% retention rate compared to 90.58% at 8 h. The cumulative ammonia production increased continuously over time, reaching 11.09 g at 104 h. NH3 ·mg cat -1 .
[0044] Obviously, the above embodiments are merely illustrative examples for clear explanation and are not intended to limit the implementation. Those skilled in the art will recognize that other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively list all possible implementations here. However, obvious variations or modifications derived therefrom are still within the scope of protection of this invention.
Claims
1. A fibrous manganese-doped praseodymium ferrite perovskite electrocatalyst, characterized in that, The nominal chemical composition of the electrocatalyst is PrFe 0.8 Mn 0.2 O3, and forms a fibrous network from a plurality of interwoven fibers.
2. The fibrous manganese-doped praseodymium ferrite perovskite electrocatalyst according to claim 1, characterized in that, The electrocatalyst, as determined by X-ray diffraction, has an orthorhombic perovskite crystal structure with space group Pnma (No. 62) and its equivalence axis set to Pbnm.
3. A method for preparing the fibrous manganese-doped praseodymium ferrite perovskite electrocatalyst according to claim 1 or 2, characterized in that, Includes the following steps: S1. Prepare a metal precursor solution with a molar ratio of Pr, Fe and Mn of 1:0.8:0.2; S2. Mix the metal precursor solution with the spinning polymer solution to obtain the precursor spinning solution; S3. Electrospin the precursor spinning solution to obtain precursor fibers. S4, drying and heat treating the precursor fibers to remove the spinning polymer and form PrFe 0.8 Mn 0.2 O3 perovskite phase.
4. The preparation method according to claim 3, characterized in that, The precursor for Pr is Pr(NO3)3·6H2O, the precursor for Fe is Fe(NO3)3·9H2O, the precursor for Mn is Mn(NO3)2·4H2O, the spinning polymer is polyvinylpyrrolidone, and the solvent is N,N-dimethylformamide.
5. The preparation method according to claim 4, characterized in that, In step S1, 435 mg Pr(NO3)3·6H2O, 323 mg Fe(NO3)3·9H2O and 50 mg Mn(NO3)2·4H2O are added to 2 mL of N,N-dimethylformamide; in step S2, 1 g of polyvinylpyrrolidone is dissolved in 8 mL of N,N-dimethylformamide, and the metal precursor solution and the spinning polymer solution are mixed at a volume ratio of 1:
4.
6. The preparation method according to claim 5, characterized in that, The potential difference of electrospinning in step S3 is 18 kV, the liquid supply rate is 1.0 mL h -1 , the distance from the needle to the receiver is 20 cm, the ambient temperature is 25 ℃, the relative humidity is 76%, the rotating speed of the drum receiver is 800 r min -1 , and the spinning time is 10 h.
7. The preparation method according to claim 6, characterized in that, Step S4 comprises: vacuum drying the precursor fibers at 80℃ for 6 h; heating at a heating rate of 2℃ min -1 to 200℃ and holding for 5 h; and then continuing to heat at a heating rate of 1℃ min -1 to 600℃ and holding for 0.5 h in an air atmosphere.
8. An electrode for the electrocatalytic reduction of nitrate to ammonia, characterized in that, The invention includes a conductive substrate and a fibrous manganese-doped praseodymium ferrite perovskite electrocatalyst of claim 1 or 2 supported on the conductive substrate.
9. A method for producing ammonia by electrocatalytic reduction of nitrate, characterized in that, Using the nitrate electrocatalytic reduction ammonia production electrode as described in claim 8 as the working electrode, a reduction potential or reduction current is applied in an alkaline electrolyte containing nitrate to reduce nitrate to ammonia.
10. The method for producing ammonia by electrocatalytic reduction of nitrate according to claim 9, characterized in that, The alkaline electrolyte comprises 1.0 mol L -1 KOH and 0.1 mol L -1 or 1.0 mol L -1 KNO3; a reduction potential is applied, the reduction potential being -0.3 V to -0.9 V vs. a reversible hydrogen electrode; a reduction current is applied, the current density being 600 mA cm -2 .