Application of amorphous palladium-copper nanoparticles in electrocatalytic nitrate reduction to ammonia
By adjusting the amount of ascorbic acid, amorphous palladium-copper nanoparticles were synthesized, solving the problem of component control in amorphous palladium-copper nanoparticles. This enabled highly efficient electrocatalytic reduction of nitrates to ammonia, demonstrating excellent catalytic performance and component-performance relationship.
Patent Information
- Application Number
- CN202611411417.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-11
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies make it difficult to achieve continuous and precise control of the composition of amorphous palladium-copper nanoparticles by adjusting synthesis parameters, resulting in the failure to effectively optimize their catalytic performance in the electrocatalytic reduction of nitrate to ammonia.
Amorphous palladium-copper nanoparticles were synthesized in an oleylamine-potassium iodide reaction system by adjusting the amount of ascorbic acid, achieving a palladium atomic ratio of 35%–55% and a copper atomic ratio of 65%–45%, and were then loaded onto a carbon support as an electrocatalyst. The preparation method is simple and efficient.
Excellent catalytic activity and selectivity were obtained, with an ammonia Faraday efficiency of no less than 85% and an ammonia yield of no less than 400 mg h⁻¹ mgcat⁻¹. The "volcano-like" relationship between components and performance was clarified, providing theoretical guidance for the design of high-performance amorphous electrocatalysts.
Smart Images

Figure REF-OBJ-1789097433302-000002 
Figure REF-OBJ-1789097433302-000003 
Figure REF-OBJ-1789097433302-000004
Abstract
Description
Technical Field
[0001] This invention belongs to the field of nanocatalysis technology, specifically relating to the application of amorphous palladium-copper nanoparticles in the electrocatalytic reduction of nitrate to ammonia, and more particularly to the application of amorphous palladium-copper nanoparticles with tunable composition as an electrocatalyst in the reduction of nitrate to ammonia. Background Technology
[0002] Ammonia (NH3) is an indispensable basic chemical raw material in modern society, widely used in fertilizer production, chemical synthesis, and emerging energy fields. The traditional Haber-Bosch ammonia synthesis process requires high temperature (400–500℃) and high pressure (10–30 MPa), resulting in enormous energy consumption and significant carbon dioxide emissions. Therefore, developing milder and more sustainable alternatives to ammonia synthesis is of great importance.
[0003] Electrocatalytic nitrate reduction to ammonia (NO3RR) is a green technology that converts nitrate pollutants in wastewater into high-value-added ammonia under ambient temperature and pressure, and has attracted widespread attention in recent years. This process not only enables the resource utilization of nitrate-containing wastewater but also serves as a complementary alternative to the Haber-Bosch process. Developing efficient and highly selective electrocatalysts is crucial for the industrial application of this technology.
[0004] Noble metal nanomaterials (such as Pt, Pd, and Au) exhibit outstanding performance in electrocatalysis due to their excellent electron transport capabilities and abundant catalytic active sites. Among them, palladium-based alloy nanomaterials have been extensively studied due to their good catalytic activity and stability. Studies have shown that introducing transition metals such as copper into palladium to form alloys can significantly improve catalytic performance by modulating the electronic structure of active sites and the adsorption-desorption behavior of intermediates through electronic and geometric effects.
[0005] Amorphous alloys, due to their long-range disordered atomic arrangement, lack crystal defects such as grain boundaries and dislocations, exhibit high surface atomic coordination unsaturation and isotropic homogeneous surfaces, demonstrating superior performance compared to their crystalline counterparts in catalysis. Recent studies have shown that amorphous palladium-based nanomaterials exhibit excellent catalytic activity and durability in reactions such as formic acid oxidation and ethanol oxidation. Although the synthesis of amorphous PdCu nanoparticles has been reported, existing methods mainly control the size and morphology (nanospheres or nanowires) of nanoparticles by changing the amount of potassium iodide, without addressing the systematic and continuous control of the composition of amorphous PdCu nanoparticles through adjusting synthesis parameters. Because the composition control of amorphous alloys is inherently technically challenging, the controllable synthesis of amorphous palladium-copper nanoparticles with different compositions and their systematic evaluation of catalytic performance have not yet been reported.
[0006] Therefore, developing a synthesis method that can continuously and precisely control the composition of amorphous palladium-copper nanoparticles over a wide range, and systematically studying their composition-performance structure-activity relationship, is of great significance for the rational design of high-performance amorphous electrocatalysts. Summary of the Invention
[0007] This invention provides an application of amorphous palladium-copper nanoparticles in the electrocatalytic reduction of nitrate to ammonia. By providing amorphous palladium-copper nanoparticles with a specific composition range as an electrocatalyst, this invention achieves excellent performance in the reduction of nitrate to ammonia. At the same time, it provides a method for preparing the amorphous palladium-copper nanoparticles, which can achieve precise control of the nanoparticle composition by simply adjusting the amount of ascorbic acid.
[0008] To achieve the above objectives, the present invention provides an application of amorphous palladium-copper nanoparticles in the electrocatalytic reduction of nitrate to ammonia, wherein the atomic ratio of palladium in the amorphous palladium-copper nanoparticles is 35% to 55%, and the atomic ratio of copper is 65% to 45%, and the ammonia Faradaic efficiency of the amorphous palladium-copper nanoparticles in the electrocatalytic reduction of nitrate is not less than 85%.
[0009] As a preferred technical solution, the atomic ratio of palladium in the amorphous palladium-copper nanoparticles is 45%, and the atomic ratio of copper is 55%.
[0010] As a preferred technical solution, the amorphous palladium-copper nanoparticles exhibit an ammonia Faradaic efficiency of 90%–100% in the electrocatalytic nitrate reduction reaction, with an ammonia yield of not less than 400 mg / h. -1 mg cat -1 .
[0011] As a preferred technical solution, the average particle size of the amorphous palladium-copper nanoparticles is 14–16 nm.
[0012] As a preferred technical solution, the amorphous palladium-copper nanoparticles are prepared by a method comprising the following steps: (1) Disperse sodium chloropalladium and copper chloride in oleylamine and stir until homogeneous to form a mixed solution; (2) Add ascorbic acid and potassium iodide solution to the mixed solution and stir to mix evenly; (3) Place the reaction solution obtained in step (2) in an oil bath at 80-120°C and heat for 2-4 hours; (4) After the reaction is complete, centrifuge and wash with ethanol to obtain the amorphous palladium-copper nanoparticles; In this process, by adjusting the amount of ascorbic acid added in step (2), the atomic ratio of palladium in the resulting amorphous palladium-copper nanoparticles can be varied within the range of 35% to 55%.
[0013] As a preferred technical solution, in step (2), every 6×10 -2 Add 20-200 mg of ascorbic acid to sodium chloropalladium.
[0014] As a preferred technical solution, in step (2), every 6×10 -2 Add 80 mg of ascorbic acid to sodium chloropalladium.
[0015] As a preferred technical solution, in step (1), the molar ratio of sodium chloropalladium to copper chloride is 1:1 to 3:1.
[0016] As a preferred technical solution, in step (2), the concentration of potassium iodide solution is 0.5 to 2.5 mg / mL, and the amount of potassium iodide solution added to each 5 mL of oleylamine is 20 to 150 μL.
[0017] As a preferred technical solution, amorphous palladium-copper nanoparticles are loaded onto a carbon support to serve as an electrocatalyst.
[0018] The present invention has the following beneficial effects: (1) Excellent catalytic performance. The amorphous palladium-copper nanoparticles provided by this invention exhibit excellent catalytic activity and selectivity in the electrocatalytic reduction of nitrate to ammonia. When the palladium atomic ratio is 45% (corresponding to a copper atomic ratio of 55%), the ammonia Faraday efficiency reaches nearly 100%, and the ammonia yield reaches 573 mg h⁻¹. -1 mg cat -1 It is significantly superior to existing technologies.
[0019] (2) Clear component-performance structure-activity relationship. This invention is the first to systematically reveal the “volcano-like” relationship between the electrocatalytic nitrate reduction performance and the composition in an amorphous palladium-copper alloy system, providing theoretical guidance for the rational design of high-performance amorphous electrocatalysts.
[0020] (3) The component control method is simple and efficient. This invention allows for continuous variation of the palladium atomic ratio in amorphous palladium-copper nanoparticles within the range of 35%–55% (corresponding to a copper atomic ratio of 65%–45%) by simply adjusting the amount of ascorbic acid added (20–200 mg) in the oleylamine-ascorbic acid-potassium iodide reaction system, while all components maintain their amorphous structure. This control method is simple to operate and has good repeatability, overcoming the shortcomings of existing technologies that can only control the size and morphology by adjusting the amount of potassium iodide, but cannot systematically control the components.
[0021] (4) The amorphous structure is well preserved. The palladium-copper nanoparticles obtained under all composition conditions are amorphous structures. In the X-ray diffraction patterns, they all show only a broad diffuse scattering packet, without any sharp characteristic diffraction peaks belonging to the crystalline structure of palladium or copper. Moreover, the elemental distribution is uniform, and there is no phase separation or segregation.
[0022] (5) Uniform particle size and regular morphology. The amorphous palladium-copper nanoparticles prepared by this invention have an average particle size of 14-16 nm, a narrow particle size distribution, and a regular spherical morphology, which is beneficial for subsequent loading and catalytic applications. Attached Figure Description
[0023] To make the objectives, technical solutions, and beneficial effects of this invention clearer, the following figures are provided for illustration: Figure 1 Transmission electron microscope (TEM) images of amorphous palladium-copper nanoparticles with different compositions prepared in Examples 1-5 of this invention.
[0024] Figure 2 The X-ray diffraction (XRD) patterns of amorphous palladium-copper nanoparticles with different compositions prepared in Examples 1-5 of this invention are shown.
[0025] Figure 3 The results of energy scattering X-ray spectroscopy (EDS) analysis of amorphous palladium-copper nanoparticles with different compositions prepared in Examples 1-5 of this invention are shown.
[0026] Figure 4 These are aberration-corrected high-resolution transmission electron microscope (AC-HRTEM) images of amorphous palladium-copper nanoparticles with different compositions prepared in Examples 1-5 of this invention.
[0027] Figure 5 The results of high-resolution elemental mapping distribution analysis of amorphous palladium-copper nanoparticles with different compositions prepared in Examples 1-5 of this invention are shown.
[0028] Figure 6 Linear sweep voltammetry (LSV) curves of amorphous palladium-copper nanoparticle catalysts with different compositions prepared in Examples 1-5 of this invention during the nitrate reduction reaction.
[0029] Figure 7 The performance of amorphous palladium-copper nanoparticle catalysts with different compositions prepared in Examples 1-5 of this invention in the nitrate reduction reaction is compared. Figure a shows the ammonia yield, Figure b shows the ammonia faradaic efficiency, Figure c shows the nitrite faradaic efficiency, and Figure d shows the hydrogen faradaic efficiency. Detailed Implementation
[0030] The present invention will be further illustrated below with specific embodiments and comparative examples. These embodiments are for illustrative purposes only and should not be construed as limiting the scope of the invention.
[0031] I. Preparation of Amorphous Palladium-Copper Nanoparticles Example 1 (Pd atomic ratio 35%) (1) 6×10 -2 mmol sodium chloropalladium and 6×10 -2 mmol of copper chloride was dispersed in 5 mL of oleylamine and stirred until well mixed; (2) Add 100 μL of potassium iodide solution (prepared by dissolving 16.6 mg of potassium iodide in 10 mL of water, with a concentration of 1.66 mg / mL) and 20 mg of ascorbic acid to the homogeneous solution in step (1), and continue stirring until homogeneous; (3) Place the homogeneous solution from step (2) in an oil bath at 100°C and react for 3 hours to obtain a black product. After the reaction is complete, cool to room temperature, centrifuge to collect the product, and wash with ethanol and cyclohexane to obtain the product.
[0032] Example 2 (Pd atomic ratio 40%) (1) 6×10 -2 mmol sodium chloropalladium and 6×10 -2 mmol of copper chloride was dispersed in 5 mL of oleylamine and stirred until well mixed; (2) Add 100 μL of potassium iodide solution (prepared by dissolving 16.6 mg of potassium iodide in 10 mL of water) and 40 mg of ascorbic acid to the homogeneous solution in step (1), and continue to stir until homogeneous; (3) Place the homogeneous solution from step (2) in an oil bath at 100°C and react for 3 hours to obtain a black product. After the reaction is complete, cool to room temperature, centrifuge to collect the product, and wash with ethanol and cyclohexane to obtain the product.
[0033] Example 3 (Pd atomic ratio 45%) (1) 6×10 -2 mmol sodium chloropalladium and 6×10 -2 mmol of copper chloride was dispersed in 5 mL of oleylamine and stirred until well mixed; (2) Add 100 μL of potassium iodide solution (prepared by dissolving 16.6 mg of potassium iodide in 10 mL of water) and 80 mg of ascorbic acid to the homogeneous solution in step (1), and continue to stir until homogeneous; (3) Place the homogeneous solution from step (2) in an oil bath at 100°C and react for 3 hours to obtain a black product. After the reaction is complete, cool to room temperature, centrifuge to collect the product, and wash with ethanol and cyclohexane to obtain the product.
[0034] Example 4 (Pd atomic ratio 50%) (1) 6×10 -2 mmol sodium chloropalladium and 6×10-2 mmol of copper chloride was dispersed in 5 mL of oleylamine and stirred until well mixed; (2) Add 100 μL of potassium iodide solution (prepared by dissolving 16.6 mg of potassium iodide in 10 mL of water) and 120 mg of ascorbic acid to the homogeneous solution in step (1), and continue to stir until homogeneous; (3) Place the homogeneous solution from step (2) in an oil bath at 100°C and react for 3 hours to obtain a black product. After the reaction is complete, cool to room temperature, centrifuge to collect the product, and wash with ethanol and cyclohexane to obtain the product.
[0035] Example 5 (Pd atomic ratio 55%) (1) 6×10 -2 mmol sodium chloropalladium and 6×10 -2 mmol of copper chloride was dispersed in 5 mL of oleylamine and stirred until well mixed; (2) Add 100 μL of potassium iodide solution (prepared by dissolving 16.6 mg of potassium iodide in 10 mL of water) and 150 mg of ascorbic acid to the homogeneous solution in step (1), and continue to stir until homogeneous; (3) Place the homogeneous solution from step (2) in an oil bath at 100°C and react for 3 hours to obtain a black product. After the reaction is complete, cool to room temperature, centrifuge to collect the product, and wash with ethanol and cyclohexane to obtain the product.
[0036] II. Characterization of Amorphous Palladium-Copper Nanoparticles The amorphous palladium-copper nanoparticles with different compositions prepared in Examples 1-5 were characterized by transmission electron microscopy (TEM), and the results are as follows: Figure 1 As shown, the nanoparticles obtained with different amounts of ascorbic acid exhibit a uniform spherical morphology and a relatively concentrated particle size distribution, with an average particle size of approximately 14–16 nm. This indicates that the preparation method of the present invention has good morphology and size controllability under different component conditions.
[0037] The powder X-ray diffraction (PXRD) analysis results of amorphous palladium-copper nanoparticles with different compositions prepared in Examples 1-5 are as follows: Figure 2 As shown, the PXRD patterns of all samples exhibit only a broad diffuse scattering pattern around approximately 40°, with no sharp characteristic diffraction peaks attributed to crystalline palladium or copper, indicating that the prepared nanoparticles are all amorphous. Furthermore, samples obtained with different amounts of ascorbic acid maintained their amorphous structural characteristics, confirming that the component control of this invention is achieved within an amorphous structural framework.
[0038] Energy-scattering X-ray spectroscopy (EDS) analysis was performed on amorphous palladium-copper nanoparticles with different compositions prepared in Examples 1-5. Figure 3As shown, the relative contents of palladium and copper in the nanoparticles changed systematically as the amount of ascorbic acid added increased from 20 mg to 150 mg. In the samples obtained in Examples 1-5, the atomic percentages of palladium were 35%, 40%, 45%, 50%, and 55%, respectively, and the atomic percentages of copper were 65%, 60%, 55%, 50%, and 45%, respectively, with the sum of the atomic percentages of palladium and copper being 100%. This result indicates that the composition of amorphous palladium-copper nanoparticles can be precisely controlled over a wide range by simply adjusting the amount of ascorbic acid added.
[0039] The amorphous palladium-copper nanoparticles with different compositions prepared in Examples 1-5 were characterized by aberration-corrected high-resolution electron microscopy (AC-HRTEM), such as... Figure 4 As shown. All samples were spherical with a diameter of 14–15 nm, and... Figure 1 The TEM observations were consistent; the disordered atomic arrangement proved that the obtained palladium-copper nanoparticles were all amorphous. Elemental mapping analysis was performed as follows: Figure 5 As shown, palladium and copper elements are uniformly distributed in all samples, and no obvious elemental segregation or phase separation was observed, indicating that the amorphous palladium-copper nanoparticles with different compositions prepared in this invention have a homogeneous alloy structure.
[0040] III. Application of Amorphous Palladium-Copper Nanoparticles in Electrocatalytic Nitrate Reduction to Ammonia (1) Preparation of catalyst powder: Catalyst powder was prepared by loading amorphous palladium-copper nanoparticles of different compositions prepared in Examples 1-5 onto a carbon support: amorphous palladium-copper nanoparticles were uniformly dispersed in 5 mL of cyclohexane and 5 mL of ethanol solution to obtain a sample solution; 5 mg of carbon black was uniformly dispersed in 10 mL of ethanol to obtain a support solution; the sample solution was slowly added dropwise to the support solution and sonicated until homogeneous; finally, the final product was collected by centrifugation, the product was washed 3 times with ethanol, the supernatant was removed by centrifugation, and the catalyst powder was obtained after drying.
[0041] (2) Preparation of catalyst ink: The above catalyst powder was dispersed in 1 mL of solution (isopropanol volume: 5 wt% Nafion solution volume = 980:20), and ultrasonicated for 30 min to prepare catalyst ink for electrochemical testing; the obtained homogeneous catalyst ink was then used to drop-coat a surface with an area of 0.5 cm². 2 On the carbon cloth working electrode.
[0042] (3) Alkaline nitrate reduction performance test: Electrochemical tests were performed in a standard three-electrode system using an H-type electrolytic cell, with the cathode and anode chambers separated by a Nafion 117 proton exchange membrane. A catalyst-coated carbon cloth served as the working electrode, a carbon rod as the counter electrode, and an Hg / HgO electrode as the reference electrode. The electrolyte was 50 mL of 1 M KOH solution, with 0.1 M KNO3 added to the cathode chamber as a reactant.
[0043] Before testing, the electrolyte in the cathode chamber was bubbled with high-purity Ar gas (99.999%) for 30 minutes to remove dissolved oxygen. During the test, Ar gas was continuously introduced to maintain the atmosphere. All potentials were converted to potentials relative to the reversible hydrogen electrode (RHE).
[0044] The following electrochemical tests were performed sequentially: ① Linear scan voltammetry (LSV): at a scan rate of 10 mV·s -1 Under these conditions, linear sweep voltammetry was performed in the potential range of 0 V to -1.2 V (vs. RHE) to record the polarization curves of nitrate reduction by different catalyst components.
[0045] ② Chronoamperometry: Constant potential electrolysis was performed for 2 h at different applied potentials (e.g., -0.4 V, -0.6 V, -0.8 V, -1.0 V vs. RHE), and the electrolyte in the cathode chamber was collected for product analysis.
[0046] (4) Product analysis and performance evaluation: The indophenol blue colorimetric method was used to determine the NH3 / NH4 generated in the electrolyte. + Quantitative analysis was performed. The absorbance was measured at 655 nm using a UV-Vis spectrophotometer, and the NH4+ was calculated based on the standard curve. + Concentration. The Griess reagent method was used to determine the concentration of NO2 that might be generated in the electrolyte. - Byproducts are tested.
[0047] The Faraday efficiency (FE) of the nitrate reduction reaction to produce ammonia is calculated using the following formula: FE (%) = (8 × F × C) NH3 × V) / Q × 100% Where F is the Faraday constant (96485 C·mol⁻¹) -1 ), C NH3 The concentration of NH3 in the electrolyte (mol·L) -1 V is the volume of electrolyte (L), and Q is the total charge passing through the reaction (C).
[0048] NH3 yield is calculated using the following formula: NH3 yield (mg h) -1 mgcat -1 )= C NH3 × V × 17 / (m) cat × t) Where 17 is the molar mass of NH3 (g·mol⁻¹) -1 ), m cat The catalyst loading on the working electrode (mg / cm²) -2 ), where t is the electrolysis time (h).
[0049] (5) Test results: Amorphous palladium-copper nanoparticles with different compositions prepared in Examples 1-5 (for ease of description, the products obtained in Examples 1-5 are respectively named a-Pd) 0.35 Cu 0.65 a-Pd 0.40 Cu 0.60 a-Pd 0.45 Cu 0.55 a-Pd 0.50 Cu 0.50 a-Pd 0.55 Cu 0.45 The electrocatalytic reduction of nitrate to ammonia production performance was tested.
[0050] ① Linear sweep voltammetric curve ( Figure 6 The results showed that all samples contained NO3. - All catalysts exhibited significant reduction current responses in their electrolytes, and the catalysts with different components showed significantly different electrocatalytic activities. With a negative potential shift, the reduction current density of each catalyst gradually increased, but there were significant differences in the onset potential and current density. Among them, a-Pd... 0.45 Cu 0.55 The catalyst exhibited the highest reduction current density and the highest activity among all catalyst components. The ranking of the LSV curves showed that the nitrate reduction activity was significantly dependent on the palladium-copper composition, and a suitable palladium-copper ratio was beneficial for obtaining optimal catalytic activity.
[0051] ② Constant potential electrolysis experiment ( Figure 7 The results showed that at a potential of -0.8 V (vs. RHE), all catalyst components could effectively reduce NO3-. - Selective reduction to NH3. Among them, the amorphous palladium-copper nanoparticle catalyst corresponding to Example 3 (Pd atomic ratio 45%, Cu atomic ratio 55%) exhibited the best performance in nitrate reduction to ammonia, with an ammonia Faradaic efficiency of nearly 100% and an ammonia yield of 573 mg / h. -1 mg cat -1Considering both the nitrite Faraday efficiency and the hydrogen Faraday efficiency, the catalytic performance of the amorphous palladium-copper alloy does not change monotonically with any one component. Instead, it reaches its optimum when Pd:Cu ≈ 45:55, exhibiting a typical "volcano-type" component-performance relationship.
[0052] The above results show that the composition of the amorphous palladium-copper nanoparticles provided by the present invention has a significant impact on their electrocatalytic performance in the reduction of nitrate to ammonia. By controlling the composition on the amorphous structure platform, the optimal state of catalytic performance can be obtained.
[0053] The above-described embodiments are merely preferred embodiments provided to fully illustrate the present invention, and the scope of protection of the present invention is not limited thereto. Equivalent substitutions or modifications made by those skilled in the art based on the present invention are all within the scope of protection of the present invention. The scope of protection of the present invention is defined by the claims.
Claims
1. The application of amorphous palladium-copper nanoparticles in the electrocatalytic reduction of nitrate to ammonia, characterized in that, The amorphous palladium-copper nanoparticles contain 35% to 55% palladium and 65% to 45% copper, and the amorphous palladium-copper nanoparticles exhibit an ammonia-farada efficiency of not less than 85% in the electrocatalytic nitrate reduction reaction.
2. The application according to claim 1, characterized in that, The amorphous palladium-copper nanoparticles contain 45% palladium and 55% copper.
3. The application according to claim 1, characterized in that, The amorphous palladium-copper nanoparticles exhibit an ammonia Faradaic efficiency of 90%–100% in the electrocatalytic nitrate reduction reaction, with an ammonia yield of not less than 400 mg / h. -1 mg cat -1 .
4. The application according to claim 1, characterized in that, The amorphous palladium-copper nanoparticles have an average particle size of 14–16 nm.
5. The application according to any one of claims 1 to 4, characterized in that, The amorphous palladium-copper nanoparticles are prepared by a method comprising the following steps: (1) Disperse sodium chloropalladium and copper chloride in oleylamine and stir until homogeneous to form a mixed solution; (2) Add ascorbic acid and potassium iodide solution to the mixed solution and stir to mix evenly; (3) Place the reaction solution obtained in step (2) in an oil bath at 80-120°C and heat for 2-4 hours; (4) After the reaction is complete, centrifuge and wash with ethanol to obtain the amorphous palladium-copper nanoparticles; In this process, by adjusting the amount of ascorbic acid added in step (2), the atomic ratio of palladium in the resulting amorphous palladium-copper nanoparticles can be varied within the range of 35% to 55%.
6. The application according to claim 5, characterized in that, In step (2), every 6 × 10 -2 Add 20–200 mg of ascorbic acid to sodium chloropalladium.
7. The application according to claim 6, characterized in that, In step (2), every 6 × 10 -2 Add 80 mg of ascorbic acid to sodium chloropalladium.
8. The application according to claim 5, characterized in that, In step (1), the molar ratio of sodium chloropalladium to copper chloride is 1:1 to 3:
1.
9. The application according to claim 5, characterized in that, In step (2), the concentration of potassium iodide solution is 0.5–2.5 mg / mL, and the amount of potassium iodide solution added to every 5 mL of oleylamine is 20–150 μL.
10. The application according to any one of claims 1 to 4, characterized in that, Amorphous palladium-copper nanoparticles were loaded onto a carbon support to serve as an electrocatalyst.