A carbon-supported PtCo-Pt3Sn heterostructure catalyst and its preparation method
By preparing carbon-supported PtCo-Pt3Sn heterostructure catalysts, the problems of low activity and poor stability of Pt-based catalysts under high current density were solved, achieving high efficiency in hydrogen evolution reaction, especially exhibiting excellent catalytic activity and stability in acidic and alkaline water electrolysis.
Patent Information
- Application Number
- CN202510635339.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-16
- Publication Date
- 2026-11-17
AI Technical Summary
Existing Pt-based catalysts exhibit low catalytic activity and poor stability at high current densities, making it difficult to meet industrial demands.
A carbon-supported PtCo-Pt3Sn heterostructure catalyst was prepared. By constructing the PtCo-Pt3Sn heterostructure, the electronic synergistic effect of the two phases of the heterostructure was regulated, the hydrogen adsorption/desorption process was optimized, H* transport was promoted, and the activity and stability of the catalyst were improved.
It significantly improves catalytic efficiency under high current density and exhibits excellent hydrogen evolution reaction performance, especially maintaining good activity and stability in acidic and alkaline water electrolysis.
Smart Images

Figure CN123108622A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of precious metal catalyst technology, specifically to a method for preparing carbon-supported PtCo-Pt3Sn heterostructure catalysts and their application in the hydrogen evolution reaction at the cathode of water electrolysis. Background Technology
[0002] Promoting the transformation of the energy system towards a low-carbon, green, and renewable structure is of great significance for building a new energy system for the carbon-neutral era. H2, as a clean energy source, is considered one of the most promising alternative energy sources for alleviating the energy crisis and reducing environmental pollution. Water electrolysis is a simple and efficient method for producing high-purity hydrogen. However, the hydrogen evolution reaction (HER), as the cathode half-reaction in water electrolysis, suffers from slow reaction kinetics and poor catalyst stability, severely hindering the development of this technology. Developing efficient and stable HER catalysts is currently the core challenge.
[0003] Currently, many Pt-based catalysts exhibit good HER activity at low current densities. However, at high current densities in industrial applications, especially powdered catalysts, they still face challenges such as low overall catalytic activity and poor electrochemical stability. Therefore, further research is needed to develop efficient and stable hydrogen evolution reaction catalysts for high current densities.
[0004] Constructing heterostructures is an effective strategy for developing highly efficient hydrogen evolution reaction (HER) catalysts. Due to differences in chemical composition and lattice spacing, defects and changes in electron cloud occur at the interface between the two heterostructures. Simultaneously, electronic interactions exist between the two phases, promoting electron redistribution within the catalyst. These factors affect the adsorption strength of each phase on intermediate active species in the heterostructure catalyst. Optimizing charge transport pathways and the adsorption free energy of reaction intermediates can significantly improve catalytic efficiency and enhance HER performance. Currently, there are few reports on carbon-supported platinum-based heterostructure catalysts suitable for high-current water electrolysis and hydrogen evolution reaction. Summary of the Invention
[0005] The technical problem solved by this invention is to provide a carbon-supported PtCo-Pt3Sn heterostructure catalyst and its preparation method. Addressing the issues of sluggish reaction kinetics and poor stability of the catalyst under high-current testing environments, a synergistic regulation strategy of the alloy-heterostructure interface is provided. A PtCo-Pt3Sn heterostructure catalyst is constructed using carbon materials as a support. By regulating the electronic synergistic effect of the two phases of the heterostructure in the hydrogen adsorption / desorption process, the H* transport efficiency is accelerated, the hydrogen evolution reaction kinetic pathway is optimized, and the rapid release of hydrogen bubbles is promoted, maintaining excellent activity and stability in both acidic and alkaline water electrolysis hydrogen evolution reactions.
[0006] To achieve the above objectives, the present invention provides a carbon-supported PtCo-Pt3Sn heterostructure catalyst, comprising PtCo-Pt3Sn heterostructure metal particles on a carbon surface, characterized in that:
[0007] The PtCo-Pt3Sn heterostructure metal particles on the surface of the carbon support are composed of three elements: Pt, Co, and Sn. They are elliptical in shape and contain two phases: an intermetallic compound of PtCo and an alloy of Pt3Sn. The two phases expose the (111) crystal plane of the PtCo phase and the (200) and (111) crystal planes of the Pt3Sn phase, respectively. The content of the PtCo-Pt3Sn heterostructure metal particles on the surface of the carbon support accounts for 23-30 wt% of the catalyst, and the average particle size is 3.6-3.9 nm.
[0008] This invention also provides a method for preparing a carbon-supported PtCo-Pt3Sn heterostructure catalyst, comprising the following steps:
[0009] (1) Disperse the carbon support, chloroplatinic acid aqueous solution, cobalt chloride hexahydrate and stannous chloride pentahydrate in deionized water and ultrasonically mix for 40-70 min. Then, dry the mixture by rotary evaporation at 60-80 °C to obtain the initial mixture.
[0010] (2) The initial mixture was placed in an atmosphere of 5% hydrogen / 95% argon, and the temperature was increased at a rate of 5-10℃ / min. The mixture was reduced at 150-300℃ for 1-3h, and then heated to 650-850℃ and held for 1-2h to obtain a PtCo-Pt3Sn heterostructure catalyst. The obtained PtCo-Pt3Sn heterostructure catalyst was placed in sulfuric acid with a concentration of 0.3-1.0mol / L and the transition metal on the surface was etched away for 3-5h.
[0011] In step (1), the total metal content is 23-30 wt%, the molar ratio of chloroplatinic acid to other metal salts is 9:1, and the molar ratio of cobalt chloride hexahydrate to stannous chloride pentahydrate is 7:3-9:1.
[0012] The carbon support mentioned in step (1) is one of carbon black, graphene, carbon nanotubes, petroleum-derived carbon, and biomass-derived carbon. More preferably, the carbon support is petroleum-derived carbon.
[0013] The PtCo-Pt3Sn heterostructure catalyst provided in this application can be prepared by impregnation and heat treatment, a simple process. The catalyst exhibits excellent HER performance in both acidic and alkaline solutions, particularly at 500 mA cm⁻¹. -2At high current densities, the overpotentials in 0.5 M H₂SO₄ and 1 M KOH are only 96 and 297 mV, respectively, far superior to commercial Pt / C (238 and 478 mV) and other similar powdered catalysts. This is attributed to the synergistic effect between the PtCo intermetallic compound phase and the Pt₃Sn alloy phase, which promotes H* adsorption / desorption, accelerates H* transport, and significantly improves hydrogen production efficiency, thereby significantly enhancing the hydrogen evolution reaction efficiency under high current. Furthermore, the strong electronic interactions between the PtCo and Pt₃Sn phases effectively improve stability. Attached Figure Description
[0014] Figure 1 The X-ray diffraction (XRD) pattern of the carbon-supported PtCo-Pt3Sn heterostructure catalyst provided in Example 1 of this invention.
[0015] Figure 2 Transmission electron microscopy (TEM) image and particle size distribution diagram of the carbon-supported PtCo-Pt3Sn heterostructure catalyst provided in Example 1 of this invention.
[0016] Figure 3 This is a high-resolution transmission electron microscope (HRTEM) image of the carbon-supported PtCo-Pt3Sn heterostructure catalyst provided in Example 1 of the present invention.
[0017] Figure 4 The image shows the XRD pattern of the carbon-supported PtCo intermetallic compound catalyst provided in Comparative Example 1 of this invention.
[0018] Figure 5 TEM image and particle size distribution diagram of the carbon-supported PtCo intermetallic compound catalyst provided in Comparative Example 1 of this invention.
[0019] Figure 6 The image shows the XRD pattern of the carbon-supported Pt3Sn alloy catalyst provided in Comparative Example 2 of this invention.
[0020] Figure 7 TEM image and particle size distribution diagram of the carbon-supported Pt3Sn alloy catalyst provided in Comparative Example 2 of this invention.
[0021] Figure 8 The image shows a comparison of the X-ray photoelectron spectroscopy (XPS) of cobalt catalysts provided in Example 1 and Comparative Example 1 of this invention.
[0022] Figure 9 XPS comparison images of tin element in catalysts provided in Example 1 and Comparative Example 2 of this invention.
[0023] Figure 10 XPS comparison images of platinum elements in the catalysts provided in Example 1, Comparative Example 1, and Comparative Example 2 of this invention.
[0024] Figure 11 The linear voltammetric scans of the catalysts provided in Examples 1, 1, and 2 of this invention with 20% Pt / C in 0.5 M H2SO4 are shown.
[0025] Figure 12 The linear voltammetric scan curves of hydrogen evolution electrochemically performed by the catalysts provided in Examples 1, 1, and 2 of this invention with 20% Pt / C in 1M KOH are shown.
[0026] Figure 13 The initial and 10,000th LSV curves of the carbon-supported PtCo-Pt3Sn heterostructure catalyst provided in Example 1 of the present invention in 0.5 M H2SO4.
[0027] Figure 14 The LSV curves of the carbon-supported PtCo-Pt3Sn heterostructure catalyst provided in Example 1 of the present invention are the initial and 10,000th cycles of cyclic voltammetry in 1 MKOH.
[0028] Test procedure: 5 mg of catalyst was dispersed in 500 μL of deionized water, 490 μL of ethanol, and 10 μL of Nafion solution (5 wt%), and sonicated for 60 min to obtain catalyst ink. A certain volume of ink was dropped onto a surface with an area of 1 cm². 2 On carbon paper, the LSV test scan range was -0.06V to 0.05V (vs RHE), and the scan speed was 5mV / s. The stability test CV range was 0.1V to 0.9V (vs RHE), the scan speed was 50mV / s, and the number of scans was 10,000. Detailed Implementation
[0029] To further understand the present invention, preferred embodiments are described below with reference to examples. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of them. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention.
[0030] Example 1
[0031] 50 mg of carbon support, 36.5 mg of H₂PtCl₆·6H₂O, 13.4 mg of CoCl₂·6H₂O, and 3.2 mg of SnCl₂·2H₂O were dispersed in 40 mL of deionized water and ultrasonically mixed for 60 min. After rotary evaporation at 70 °C, a homogeneous precursor was obtained. The precursor was placed in a tube furnace, and argon-hydrogen (95% Ar + 5% H₂ by volume) was introduced into the tube furnace as a protective gas. The temperature of the tube furnace was increased to 200 °C at a rate of 5 °C / min for 2 h, and then increased to 700 °C at a rate of 5 °C / min and held for 1.5 h. Finally, the temperature was allowed to drop naturally to room temperature while maintaining atmospheric pressure in the tube furnace to obtain a carbon-supported PtCo-Pt₃Sn heterostructure catalyst. The obtained carbon-supported PtCo-Pt₃Sn heterostructure catalyst was placed in 0.5 mol / L sulfuric acid and etched for 4 h.
[0032] Figure 1 The image shows the XRD pattern of the carbon-supported PtCo-Pt3Sn heterostructure catalyst provided in Example 1 of this invention. Figure 1 As shown, the peak positions in the XRD pattern indicate that PtCo and Pt3Sn phases coexist in the PtCo-Pt3Sn / C catalyst. Figure 2 The images show TEM images and particle size distribution diagrams of the carbon-supported PtCo-Pt3Sn heterostructure catalyst provided in Example 1 of this invention. It can be observed that the PtCo-Pt3Sn / C catalyst metal particles are uniformly distributed on the carbon support, and the average particle size of approximately 140 metal particles is calculated to be 3.91 nm. Figure 3 The image shows an HRTEM image of the carbon-supported PtCo-Pt3Sn heterostructure catalyst provided in Example 1 of this invention. Clear lattice stripes and heterostructure interfaces between PtCo and Pt3Sn can be clearly seen, with lattice spacings corresponding to the (111) crystal plane of the PtCo phase and the (200) and (111) crystal planes of the Pt3Sn phase, respectively.
[0033] Example 2
[0034] 25 mg of carbon support, 18.3 mg of H₂PtCl₆·6H₂O, 6.7 mg of CoCl₂·6H₂O, and 1.6 mg of SnCl₂·2H₂O were dispersed in 20 mL of deionized water and ultrasonically mixed for 60 min. After rotary evaporation at 70 °C, a homogeneous precursor was obtained. The precursor was placed in a tube furnace, and argon-hydrogen (95% Ar + 5% H₂ by volume) was introduced into the tube furnace as a protective gas. The temperature of the tube furnace was increased to 200 °C at a rate of 5 °C / min for 2 h, and then increased to 700 °C at a rate of 5 °C / min and held for 2 h. Finally, the temperature was allowed to drop naturally to room temperature while maintaining atmospheric pressure in the tube furnace to obtain a carbon-supported PtCo-Pt₃Sn heterostructure catalyst. The obtained carbon-supported PtCo-Pt₃Sn heterostructure catalyst was placed in 0.5 mol / L sulfuric acid and etched for 4 h.
[0035] Example 3
[0036] 50 mg of carbon support, 36.2 mg of H₂PtCl₆·6H₂O, 15 mg of CoCl₂·6H₂O, and 1.6 mg of SnCl₂·2H₂O were dispersed in 40 mL of deionized water and ultrasonically dispersed for 1 h. After rotary evaporation and drying, a homogeneous precursor was obtained. The precursor was placed in a tube furnace, and argon-hydrogen (95% Ar + 5% H₂ by volume) was introduced into the tube furnace as a protective gas. The tube furnace was heated to 200 °C at a rate of 5 °C / min for 2 h, and then heated to 700 °C at a rate of 5 °C / min and held for 1.5 h. Finally, it was allowed to cool naturally to room temperature while maintaining atmospheric pressure in the tube furnace to obtain a carbon-supported PtCo-Pt₃Sn heterostructure catalyst. The obtained carbon-supported PtCo-Pt₃Sn heterostructure catalyst was placed in 0.5 mol / L sulfuric acid and etched for 4 h.
[0037] Comparative Example 1
[0038] The only difference from Example 1 is that SnCl2·2H2O is not added, while the other steps remain the same, resulting in a carbon-supported PtCo intermetallic compound catalyst.
[0039] Figure 4 The image shows the XRD pattern of the carbon-supported PtCo intermetallic compound catalyst provided in Comparative Example 1 of this invention. The formation of PtCo intermetallic compounds is determined based on the peak positions of the XRD pattern. Figure 5 The images show TEM images and particle size distribution diagrams of the carbon-supported PtCo intermetallic compound catalyst provided in Comparative Example 1 of this invention. The metal particles are uniformly distributed on the carbon support, without agglomeration, and have an average particle size of 2.57 nm. Figure 8 XPS comparison images of cobalt element in the catalysts provided in Example 1 and Comparative Example 1 of this invention. Figure 8In the PtCo / C heterostructure, compared to PtCo / C, the Co 2p orbital binding energy exhibits a positive shift (0.3 eV). This indicates that the presence of the PtCo-Pt3Sn heterostructure causes Co to lose more electrons.
[0040] Comparative Example 2
[0041] The only difference from Example 1 is that CoCl2·6H2O is not added, while the other steps remain the same, resulting in a carbon-supported Pt3Sn alloy catalyst.
[0042] Figure 6 The image shows the XRD pattern of the carbon-supported Pt3Sn alloy catalyst provided in Comparative Example 2 of this invention. The formation of Pt3Sn alloy is determined based on the peak positions of the XRD pattern. Figure 7 The images show TEM images and particle size distribution diagrams of the carbon-supported Pt3Sn alloy catalyst provided in Comparative Example 2 of this invention. The Pt3Sn metal particles are uniformly supported on carbon, with an average particle size of 2.22 nm. Figure 9 XPS comparison images of tin elements in the catalysts provided in Example 1 and Comparative Example 2 of this invention. Compared with PtCo-Pt3Sn / C, the Sn 3d peak of Pt3Sn / C shows a negative shift (0.3 eV), indicating that the Sn element in the PtCo-Pt3Sn / C catalyst gains electrons. Figure 10 These are XPS comparison images of the platinum element in the catalysts provided in Example 1, Comparative Example 1, and Comparative Example 2 of the present invention. Figure 10 As shown, compared to PtCo / C, PtCo-Pt3Sn / C has higher Pt content. 0 and Pt 2+ Both peaks show a slight negative shift, indicating that the introduction of Sn optimizes the electron density distribution of Pt sites. However, compared with Pt3Sn / C, the Pt 4f binding energy of PtCo-Pt3Sn / C undergoes a positive shift (0.3 eV), confirming the presence of Co-Sn-Pt multimetallic orbital hybridization at the heterojunction, leading to enhanced electron cloud rearrangement and charge transfer at Pt sites. Electron redistribution on the catalyst surface creates electron-poor / electron-rich regions. The PtCo phase gains electrons and exhibits strong H* adsorption, belonging to the hydrogen-rich component, which is conducive to H2 adsorption. Conversely, Pt3Sn loses electrons and exhibits weak H* adsorption, belonging to the hydrogen-poor component, which is conducive to H2 desorption. The heterojunction acts as a hydrogen overflow channel, enabling ultra-fast transfer of hydrogen atoms from PtCo to Pt3Sn. Figure 11 The linear voltammetric scans of the catalysts provided in Examples 1, 1, and 2 of this invention with 20% Pt / C in 0.5 M H₂SO₄ are shown. Figure 12Linear voltammetric scans of the hydrogen evolution electrochemical properties of the catalysts provided in Examples 1, 1, and 2 of this invention, along with 20% Pt / C, in 1 mH₂O. The PtCo-Pt₃Sn / C catalyst exhibited excellent hydrogen evolution catalytic performance in both acidic and alkaline media, with particularly superior performance at correspondingly higher current densities. The improved hydrogen evolution performance is mainly due to the electronegativity gradient formed by Pt / Co / Sn in the metal particles, which facilitates the synergistic regulation of the intermediate adsorption-desorption balance and enhances the intrinsic HER activity. Figure 13 The initial and 10,000th LSV curves of the carbon-supported PtCo-Pt3Sn heterostructure catalyst provided in Example 1 of the present invention in 0.5M H2SO4. Figure 14 The LSV curves of the carbon-supported PtCo-Pt3Sn heterostructure catalyst provided in Example 1 of this invention are shown in the initial and 10,000th cycles of cyclic voltammetry testing in 1M KOH. The LSV curves before and after cyclic voltammetry testing in both acidic and alkaline media show no significant changes, fully demonstrating the excellent stability of PtCo-Pt3Sn / C. This may be due to the strong electronic interactions between the PtCo and Pt3Sn interfaces, which reduce the shedding, aggregation, and migration of metal particles, thereby improving durability.
[0043] In summary, this invention provides a carbon-supported noble metal heterostructure catalyst. The method is simple to operate and can be scalable. It utilizes the synergistic effect of the two phases in the heterostructure to accelerate the catalytic reaction efficiency. Simultaneously, the electronic interaction between the PtCo and Pt3Sn phases effectively prevents particle shedding, dissolution, or migration, thus improving stability. It exhibits good catalytic activity and application prospects in both acidic and basic hydrogen evolution reactions.
[0044] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A carbon-supported PtCo-Pt3Sn heterostructure catalyst, comprising PtCo-Pt3Sn heterostructure metal particles on the surface of a carbon support, characterized in that: The PtCo-Pt3Sn heterostructure metal particles on the surface of the carbon support are composed of three elements: Pt, Co, and Sn. They are elliptical in shape and contain two phases: an intermetallic compound of PtCo and an alloy of Pt3Sn. The two phases expose the (111) crystal plane of the PtCo phase and the (200) and (111) crystal planes of the Pt3Sn phase, respectively. The content of the PtCo-Pt3Sn heterostructure metal particles on the surface of the carbon support accounts for 23-30 wt% of the catalyst, and the average particle size is 3.6-3.9 nm.
2. The method for preparing the carbon-supported PtCo-Pt3Sn heterostructure catalyst according to claim 1, characterized in that: (1) The carbon support, aqueous solution of chloroplatinic acid, cobalt chloride hexahydrate, stannous chloride pentahydrate and deionized water are ultrasonically mixed for 40-70 min to obtain a reaction precursor solution. The molar ratio of chloroplatinic acid to other metal salts is 9:1, and the molar ratio of cobalt chloride hexahydrate and stannous chloride pentahydrate is 7:3-9:
1. (2) The reaction precursor solution obtained in step (1) is dried by rotary evaporation at 60-80°C to obtain an initial mixture. The mixture is then heat-treated in a reducing atmosphere of 5% hydrogen / 95% argon at a reduction temperature of 150-300°C for 1-3 hours. The temperature for the second heating is 700-800°C and the holding time is 1-2 hours. (3) Place the powder obtained in step (2) in sulfuric acid and etch away the transition metal on the surface; the concentration of the sulfuric acid is 0.3 to 1.0 mol / L; the etching time is 3 to 5 h.
3. The application of the carbon-supported PtCo-Pt3Sn heterostructure catalyst according to claim 1, characterized in that, It is used for hydrogen evolution reaction at the cathode of water electrolysis in acidic and alkaline environments.