A method for upgrading and reprocessing cathode materials from spent batteries into electrochemical catalysts
By doping waste lithium-ion battery cathode materials with Ni, Fe, and Pd and then subjecting them to plasma treatment, a LiCoNiFePd catalyst was prepared. This solved the problems of high energy consumption in waste lithium-ion battery recycling and poor performance of water electrolysis catalysts, and enabled a high-efficiency, low-cost green hydrogen production technology.
Patent Information
- Application Number
- CN202610647308.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2025-05-14
- Filing Date
- 2026-05-12
- Publication Date
- 2026-11-17
AI Technical Summary
Existing methods for recycling spent lithium-ion batteries are energy-intensive and environmentally unfriendly, and the recycled electrode materials cannot meet commercial-grade standards. Furthermore, the electrocatalysts in water electrolysis technology have poor performance, which limits the efficiency and cost of green hydrogen production.
LiCoO2, the cathode material of spent lithium-ion batteries, was doped with Ni, Fe, and Pd, and then subjected to plasma treatment and grinding to prepare a LiCoNiFePd catalyst. This catalyst was then used as the anode gas diffusion layer in anion exchange membrane water electrolysis, simplifying the process and improving the surface activity and stability of the catalyst.
A high-performance, low-cost electrocatalyst has been developed, which can efficiently generate green hydrogen in the AEMWE electrolyzer, exhibiting excellent stability and economic benefits, and is suitable for industrial applications.
Smart Images

Figure CN123108623A_ABST
Abstract
Description
Cross-referencing of patent applications
[0001] This application claims priority to U.S. Provisional Patent Application No. 63 / 805,295, filed May 14, 2025, the entire disclosure of which is incorporated herein by reference. Technical Field
[0002] This invention generally relates to battery recycling technology. More specifically, this invention relates to a method for upgrading and remanufacturing spent battery cathode materials into a water splitting electrocatalyst for green hydrogen production. Background Technology
[0003] The widespread adoption of portable electronic devices and electric vehicles has led to a significant increase in demand for the recycling of spent lithium-ion batteries. At the same time, global initiatives to achieve carbon neutrality highlight the urgent need for cost-effective and efficient green hydrogen production technologies, which still require further development.
[0004] Lithium-ion batteries (LIBs) are a crucial component of the global energy transition, driving rapid growth in demand for electric vehicles and renewable energy storage. The primary cathode materials for LIBs are layered oxides, including LiCoO2 (LCO) and LiNi. x Mn y Co z O2 (NMC), LiNiCoAlO2 (NCA), etc. The recycling of waste LIB is crucial for recovering valuable metals (such as cobalt and lithium) and mitigating environmental pollution. The most common recycling methods include direct recycling, pyrometallurgy, hydrometallurgy, biohydrometallurgy (bioleaching), and electrometallurgy.
[0005] The main strategy for direct recycling lies in reactivating the active electrode materials in spent batteries to restore their capacity and mitigate performance losses during recycling. This process typically involves multiple stages, such as discharge, disassembly, electrolyte recovery, electrode material or metal separation, and electrode material regeneration. Major regeneration technologies for cathode materials include solid-state reaction, hydrothermal treatment, co-precipitation, sol-gel method, and carbothermal reduction. However, challenges remain, including difficulties in impurity removal, high energy consumption, and complex reaction processes. Furthermore, due to the complexity of pretreatment procedures and the involvement of toxic reagents, its application is currently primarily limited to laboratory environments.
[0006] In the recycling of waste liquid metallurgy (LIB), pyrometallurgy, as a widely adopted extraction metallurgical technology, has made significant progress. Traditional pyrometallurgical techniques, such as direct roasting, typically convert different components in LIB (including cathode, anode, binder, diaphragm, and electrolyte) into cobalt-containing alloys, slag, and gases at high temperatures exceeding 1000°C. Hydrometallurgy has been widely used to recover valuable components from LIB using aqueous solutions (including acidic solutions). However, the use of strong acids and the treatment of liquid waste present significant sustainability challenges. Bioleaching refers to the process of promoting metal extraction using acidophilic microorganisms (which can be bacteria or fungi) under controlled conditions. The efficiency of bioleaching is affected by various factors, including pH, temperature, type and source of nutrients, and pulp concentration. Although bioleaching has many environmentally friendly advantages, its slow kinetics and selective metal dissolution process still present significant challenges that require further research and optimization. Electrometallurgy includes processes such as electrodeposition, electrowinning, electrolytic refining, and electroplating. Due to its low dependence on external reagents, electrometallurgy is gaining attention as a method for LIB recovery.
[0007] U.S. Patent No. 6,511,639 discloses a method for recovering negative electrode materials from spent lithium-ion batteries, particularly for lithium / transition metal mixed oxides. The method includes the following steps: (i) opening the electrode pack; (ii) organic solvent extraction; (iii) drying; (iv) mechanical separation of the positive electrode; (v) grinding and grading; and (vi) high-temperature treatment at 300 to 700°C to remove non-electrode residues. U.S. Patent Publication No. 20220376312A1 describes an advanced method for recycling and regenerating cathode materials from lithium-ion batteries, particularly for LCO and NCM chemistry systems. The proposed technology combines hydrothermal treatment and thermal annealing to restore cathode material performance and emphasizes the environmental and economic benefits compared to conventional recycling methods. Unfortunately, these methods for recovering precious metals from spent LIBs often have high energy consumption and a large environmental footprint. Furthermore, the regenerated electrode materials typically do not meet the commercial-grade standards required for battery applications. This is because, firstly, the particle size of these materials is too large to provide sufficient surface area to support highly active reactions; secondly, layered lithium transition metal oxides do not exhibit high activity in water splitting reactions. Therefore, there is an urgent need to develop environmentally friendly and efficient LIB recovery processes.
[0008] Anion exchange membrane water electrolysis (AEMWE) is emerging as a promising technology for hydrogen production. Given its cleanliness and environmental friendliness, AEMWE is considered a promising solution in the context of global efforts to move away from traditional fossil fuels and address climate change. The basic configuration of an AEMWE electrolyzer includes an anion exchange membrane (AEM) and two catalytic electrodes. Typically, AEMWE uses a dilute alkaline solution or pure water as the electrolyte and employs a low-cost, non-precious metal catalyst and a carbon-based membrane. During operation, water undergoes electrolysis to produce hydrogen and oxygen. However, the development of current water electrolysis technology is still limited by the poor performance of electrocatalysts. The efficiency of these catalysts has a significant impact on power consumption, which accounts for approximately 70% to 90% of the total cost of hydrogen production. Furthermore, their durability determines the lifespan of the water electrolysis unit. Therefore, to achieve the economical and efficient production of green hydrogen through water electrolysis, there is an urgent need to develop high-performance and low-cost electrocatalysts.
[0009] Transition metal oxides, hydroxides, and phosphates are considered common water splitting catalysts. Among them, Fe, Co, and Ni-based materials exhibit favorable electronic structures and stability in alkaline environments, thus becoming promising candidates for this process. Furthermore, lithium-containing transition metal oxides (LTMOs), including LiCoO2, NMC, and NCA, have attracted considerable attention as electrocatalysts for water splitting, particularly for the oxygen evolution reaction (OER).
[0010] Among various cobalt oxides, layered lithium-ion oxides (LCOs) have attracted particular attention due to the ease of tuning the redox state of cobalt and the associated lithium composition. Furthermore, the abundant availability of LCOs from spent lithium-ion batteries makes them an attractive material for recycling in other energy applications. However, LCOs exhibit limited intrinsic oxygen evolution reaction (OER) activity due to the need to overcome a significant potential barrier to trigger their favorable surface reconstruction. Various strategies have been employed to improve their activity, including elemental doping, exfoliation, cation insertion, and electrochemical modulation. However, none of these strategies have yielded high-performance and durable OER electrocatalysts suitable for practical electrolyzer applications. Therefore, further improvements are needed to reduce overpotential, enhance stability at high current densities, and develop scalable synthetic routes that maintain catalytic performance. Summary of the Invention
[0011] According to one aspect of the present invention, a method is provided for upgrading and reprocessing cathode material from spent batteries into an electrochemical catalyst. The method includes: separating the cathode material from the spent battery; purifying the cathode material; doping the cathode material with one or more additives to obtain the electrochemical catalyst; grinding the electrochemical catalyst to reduce its particle size; and subjecting the electrochemical catalyst to plasma treatment to improve its surface activity.
[0012] In one embodiment, the waste battery is a lithium-ion battery; and the cathode material is LiCoO2.
[0013] In one embodiment, the LiCoO2 material is doped with Ni, Fe, and Pd to make the electrochemical catalyst a LiCoNiFePd catalyst.
[0014] In one embodiment, doping the LiCoO2 material with Ni, Fe, and Pd includes: mixing the LiCoO2 material with Fe2O3, NiO, and Pd(NO3)2 to form a mixture; and sintering the mixture in ambient air to form the LiCoNiFePd catalyst.
[0015] In one embodiment, the mixture is sintered by sintering at 5 to 10 °C for 1 minute. −1 The heating process is performed by heating the mixture from ambient temperature to a sintering temperature within a range of 700 to 850 °C, such that the LiCoNiFePd catalyst exhibits LiCo... 0.79 Ni 0.1 Fe 0.1 Pd 0.01 The composition and layered structure of O2.
[0016] In one embodiment, the method further includes immersing the waste battery in a saturated NaCl solution to fully discharge the battery before separating the cathode material.
[0017] In one embodiment, separating the cathode material from the waste battery includes: cutting open the edge of the waste battery casing with a knife to expose the battery cell; and separating the cathode material from the anode material in the battery cell.
[0018] In one embodiment, the purification of the cathode material is performed by placing the cathode material in a muffle furnace at 600°C for 2 hours.
[0019] In one embodiment, grinding the electrochemical catalyst includes grinding the electrochemical catalyst for 2 hours using a ball mill equipped with ZrO2 balls at a speed of 450 rpm.
[0020] In one embodiment, the plasma treatment is performed using sulfur hexafluoride (SF6) plasma.
[0021] According to another aspect of the present invention, a method is provided for upgrading and reprocessing LiCoO2 material from spent lithium-ion batteries into a LiCoNiFePd catalyst and using the LiCoNiFePd catalyst to construct an anode gas diffusion layer for anion exchange membrane water electrolysis. The method includes: separating the LiCoO2 material from the spent lithium-ion battery; purifying the LiCoO2 material; doping the LiCoO2 material with Ni, Fe, and Pd to obtain the LiCoNiFePd catalyst; milling the LiCoNiFePd catalyst to reduce its particle size; and plasma treating the LiCoNiFePd catalyst to improve its surface activity; preparing an anode catalyst ink; and applying the anode catalyst ink to a plasma of 10 mg / cm³. 2 The loading was sprayed onto nickel foam on a hot plate at 80°C to form the anode-gas diffusion layer. The anode catalyst ink was prepared by mixing the LiCoNiFePd catalyst, sulfonated tetrafluoroethylene vinyl fluorinated copolymer, anhydrous ethanol, and deionized water in a ratio of 1 mg:20 μL:0.5 mL:0.5 mL to form a mixture; and ultrasonically treating the mixture in an ice bath for 1 hour to obtain the anode catalyst ink.
[0022] This invention provides an innovative and environmentally friendly process for recycling spent battery cathode materials. This process converts spent battery cathode materials into high-performance, non-precious metal-based electrocatalysts for green hydrogen production while minimizing carbon emissions and chemical waste. The process is scalable, enabling the recycling of spent battery cathode materials and the output of electrocatalysts on a kilogram-scale basis, and offers significant economic benefits by reducing reliance on precious metals.
[0023] Furthermore, the upgraded and remanufactured electrocatalyst can drive a high-performance AEMWE electrolyzer (electrolysis potential 1.58V@2.5A cm⁻¹). -2 Its performance is comparable to that of proton exchange membrane water electrolysis, but at a significantly lower cost. This catalyst exhibits robust performance in supporting kilowatt-scale AEMWE systems, making it suitable for industrial applications.
[0024] This invention also provides a composite doping method to improve the actual OER performance of LCO recovery and elucidates the key roles of each doping element. By controlling the degree of catalyst remodeling at increased electrolysis temperatures, a high-performance LiCo catalyst is developed. 0.79 Ni 0.1 Fe 0.1 Pd 0.01 The O2 (LCNFPdO) electrocatalyst exhibits excellent stability (over 2,000 hours) and superior activity compared to the benchmark catalyst.
[0025] Furthermore, this invention involves surface modification, endowing the cobalt-based electrocatalyst with novel surface properties that are more favorable for water splitting. Therefore, this invention will exhibit higher activity than commercial electrocatalysts. Recycling spent LIB cathode materials for use in water splitting catalysts represents a significant opportunity for scientific and technological advancement. This innovative approach addresses two pressing issues: the sustainable management of electronic waste and the development of low-cost electrocatalysts for water splitting. Recycling spent LIB cathodes rich in transition metals such as Co, Ni, and Mn can potentially yield active materials suitable for the oxygen evolution reaction (OER) or hydrogen evolution reaction (HER). By employing techniques such as chemical leaching, heteroatom doping, and structural reconstruction, these materials can be reused to enhance their catalytic performance, thereby promoting a circular economy and driving the development of renewable energy technologies. By combining battery recycling with advanced hydrogen production technologies, this invention advances the concept of a circular economy while improving the affordability and scalability of green hydrogen, thus addressing key environmental and economic challenges. Attached Figure Description
[0026] The embodiments of the present invention will be described in more detail below with reference to the accompanying drawings, wherein:
[0027] Figure 1 A flowchart of a method for recycling spent lithium-ion battery cathode materials and upgrading them into electrocatalysts according to an embodiment of the present invention is shown.
[0028] Figure 2 A schematic diagram of an AEMWE electrolyzer is shown.
[0029] Figure 3 A flowchart illustrating the preparation process of an anode-gas diffusion layer according to an embodiment of the present invention is shown.
[0030] Figure 4 This shows the effect at 80 ºC with a working electrode area of 1 cm². −2 The anode is the AEMWE polarization curve under the conditions of the studied catalyst and the cathode is Pt / C. Solid dots represent the test results of this work, while hollow dots represent comparative results from published literature.
[0031] Figure 5The electrochemical impedance spectroscopy (EIS) plot at a potential of 1.8 V is shown.
[0032] Figure 6 The results showed that at 60 ºC and 500 mA cm⁻¹ −2 Stability test under current density. Detailed Implementation
[0033] In the following description, the details of the invention are set forth in conjunction with preferred embodiments and are not intended to be limiting. It will be understood by those skilled in the art that various modifications, including additions and / or substitutions, can be made to the invention without departing from its scope and spirit. To avoid making the description of the invention overly complex, certain specific details may be omitted; however, the content of this disclosure is sufficiently described to enable those skilled in the art to implement the technical solutions disclosed herein without excessive experimentation.
[0034] Unless otherwise defined, all technical and scientific terms used in this specification shall have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains.
[0035] Figure 1 A flowchart of a method S100 for recycling spent lithium-ion battery cathode materials and upgrading them into electrocatalysts is shown. The method S100 includes the following steps:
[0036] S101: Separate the cathode material from the waste battery;
[0037] S102: Purify the cathode material;
[0038] S103: The cathode material is doped with one or more additives to obtain an electrochemical catalyst, such as a durable cobalt oxide-based OER electrocatalyst with improved electrochemical stability (e.g., mitigating surface reconstruction by suppressing cobalt redox during OER).
[0039] S104: The electrochemical catalyst is ground to reduce its particle size; and
[0040] S105: The electrochemical catalyst is subjected to plasma treatment to improve its surface activity.
[0041] Prior to step S101, method S100 may include discharging the waste lithium-ion battery by immersing it in a saturated NaCl solution for 12 hours or until no more bubbles are observed in the solution.
[0042] In step 101, separating the cathode material from the waste battery includes: using a knife to cut open the edge of the waste battery casing to expose the battery cell; and separating the cathode material from the anode material in the battery cell.
[0043] In step 102, purifying the cathode material includes placing the cathode material in a muffle furnace and heating it to 600°C and holding it for 2 hours to purify the waste cathode material by removing the binder and conductive carbon mixed in the cathode material.
[0044] In step 104, the doped cathode material is transferred to a ball mill and then ground in a ZrO2 grinding jar containing ZrO2 balls at 450 rpm for 2 hours. This significantly reduces the size of the cathode material and alters its surface structure.
[0045] In step 105, the surface of the electrochemical catalyst is subjected to plasma treatment using sulfur hexafluoride (SF6) plasma to improve its surface activity.
[0046] In one embodiment, the spent battery is a lithium-ion battery; and the cathode material is LiCoO2. The LiCoO2 material is doped with Ni, Fe, and Pd to make the electrochemical catalyst a LiCoNiFePd catalyst.
[0047] The obtained LiCoNiFePd catalyst possesses LiCo 0.79 Ni 0.1 Fe 0.1 Pd 0.01 The composition and layered structure of O2 (LCNFPdO) achieved a record-breaking OER stability of over 2,000 hours. It should be understood that other upgraded reconstituted LiCoNiFePd catalysts with different Ni, Fe, and Pd compositions also exhibit good OER stability. Through the synergistic effect of Ni, Fe, and Pd, the composite doping enhances the initial cobalt valence state, thereby limiting lithium loss and raising the energy barrier for the formation of a thick, unstable reconstructed layer. Furthermore, the introduction of Fe and Pd increases electronic conductivity and accelerates bubble desorption, thereby enhancing mechanical robustness and preventing metal leaching. Crucially, this composition produces the highest catalytic activity while requiring the lowest overpotential during operation; this lower energy barrier further mitigates the electrochemical degradation of the catalyst structure, resulting in long-term stability.
[0048] Furthermore, membrane electrolyzer tests showed that its anodic performance was superior to that of the reference RuO2, achieving 2.5 A cm⁻¹ at only 1.58 V. −2 And at 0.5 A cm −2 It maintains long-term stability for more than 1,420 hours.
[0049] Different elemental doping of LiCoO2 was achieved by mixing it with stoichiometric oxides / salts, including Fe2O3 (≥99%), NiO (99%), and Pd(NO3)2 (0.216 M). The uniformly mixed powder was then incubated in ambient air at 10 °C for [time missing]. −1 The sintering time was 12 hours at a heating rate of 12 hours. The heat treatment temperature for catalyst preparation has been optimized. For LCO, 700-850 ºC is suitable. In this invention, 800 ºC was selected as the sintering temperature to balance appropriate kinetics and high-purity phase.
[0050] The composite multi-element doping is beneficial for regulating the cation extraction rate, thereby controlling the surface dynamic reconstruction. Firstly, multi-doping increases the initial Co valence state, thereby enhancing the OER activity of layered LCO. Secondly, the strain induced by multi-element doping leads to Li… + Migration is inhibited, thus preventing excessive delithiation and Co peroxidation on the surface. This leads to the formation of a stable bulk structure and an amorphous layer with high OER activity adjacent to the surface, especially at industrial temperatures. The strategy described in this paper can also be potentially applied to the redox kinetics of a large class of intercalated cation layered materials, such as layered oxides (AMO2: A is an alkali metal; M is a transition metal), spinel-type oxides (AM2O4: A is an alkali metal; M is a transition metal), perovskites (ABO3: A is Li or K; B is Nb or Ti), and other layered (hydrogen) oxides (e.g., montmorillonite).
[0051] In one practical implementation, the LCNFPdO catalyst obtained by method S100 can be used in an AEMWE electrolyzer ( Figure 2 An anode-gas diffusion layer (GDL) is constructed in the process.
[0052] See Figure 3 The preparation process of the anode-gas diffusion layer S300 may include the following steps:
[0053] S301: Preparation of anode catalyst ink, comprising: mixing the LiCoNiFePd catalyst, sulfonated tetrafluoroethylene vinyl fluorinated copolymer, anhydrous ethanol and deionized water in a ratio of 1 mg:20 μL:0.5 mL:0.5 mL to form a mixture; and subjecting the mixture to ultrasonic treatment in an ice bath for 1 hour to obtain the anode catalyst ink; and
[0054] S302: Dissolve the anode catalyst ink at 10 mg cm⁻¹ -2 The loading is sprayed onto nickel foam on a hot plate at 80°C to form the anode-gas diffusion layer.
[0055] The prepared anode gas diffusion layer (i.e., LCNFPdO loaded on nickel foam) can then be used in conjunction with a cathode gas diffusion layer (e.g., 10% Pt / C on carbon paper) to sandwich an anion exchange membrane (AEM) between the anode and cathode current collectors at a pressure of about 3 MPa.
[0056] The preparation process of the cathode gas diffusion layer is similar to that of the anode gas diffusion layer, except that 10% Pt / C is used to replace LCNFPdO and carbon paper is used to replace nickel foam.
[0057] In AEMWE testing, LCNFPdO achieved 2 A cm⁻¹ at the same 2 V tank voltage. −2 current density ( Figure 4 The polarization impedance was significantly higher than that of comparable samples, including RuO2, α-Co(OH)2, and β-Co(OH)2. This superior performance was also accompanied by a lower polarization impedance. Figure 5 After iR correction, LCNFPdO can achieve 2.5 A cm⁻¹ at only 1.58 V. −2 ( Figure 4 This indicates its significant application potential. Furthermore, the AEMWE electrolyzer using LCNFPdO as the anode at 500 mA cm⁻¹... −2 It can operate continuously at current density for more than 1,420 hours without any degradation. Figure 6 ).
[0058] In this invention, the upgrading and remanufacturing process is simplified, eliminating the need for complex procedures or lengthy paths. Furthermore, this method is not limited to waste lithium cobalt oxides but has broad applications, suitable for a wider range of lithium-ion batteries using transition metal oxides as cathode materials.
[0059] In this invention, this embodiment provides a feasible process for recovering cathode materials from spent lithium-ion batteries without high energy consumption and chemical waste, and provides an easy-to-implement process to directly upgrade and remanufacture the recovered materials into electrocatalysts for the production of green hydrogen without excessively long paths or high costs.
[0060] Although described and illustrated with reference to specific embodiments of the present disclosure, such descriptions and illustrations are not limiting. The drawings are not necessarily drawn to scale. Due to manufacturing processes and tolerances, there may be differences between the drawings in this disclosure and actual apparatus. Other embodiments of the present disclosure may also exist that are not specifically shown. Modifications may be made to specific circumstances, materials, composition, methods, or processes to suit the purpose and scope of this disclosure. All such modifications are intended to fall within the scope of the appended claims. While the methods disclosed herein have been described with reference to specific operations performed in a particular order, it should be understood that these operations may be combined, subdivided, or reordered to form equivalent methods without departing from the teachings of this disclosure. Therefore, unless specifically stated otherwise herein, the order and grouping of operations do not constitute a limitation.
Claims
1. A method for upgrading and reprocessing cathode materials from spent batteries into electrochemical catalysts, comprising: Separate the cathode material from the waste battery; The cathode material is purified; The cathode material is doped with one or more additives to obtain the electrochemical catalyst; The electrochemical catalyst is ground to reduce its particle size; as well as The electrochemical catalyst is subjected to plasma treatment to improve its surface activity.
2. The method according to claim 1, wherein, The waste battery is a lithium-ion battery; and the cathode material is LiCoO2.
3. The method according to claim 2 further includes doping the LiCoO2 material with Ni, Fe and Pd, so that the electrochemical catalyst is a LiCoNiFePd catalyst.
4. The method according to claim 3, wherein, The doping of the LiCoO2 material with Ni, Fe and Pd includes: mixing the LiCoO2 material with Fe2O3, NiO and Pd(NO3)2 to form a mixture; and sintering the mixture in ambient air to form the LiCoNiFePd catalyst.
5. The method according to claim 4, wherein, The mixture is sintered by sintering at 5 to 10 °C for 1 minute. −1 The heating process is performed by heating the mixture from ambient temperature to a sintering temperature within a range of 700 to 850 °C, such that the LiCoNiFePd catalyst exhibits LiCo... 0.79 Ni 0.1 Fe 0.1 Pd 0.01 The composition and layered structure of O2.
6. The method according to claim 1 further includes immersing the waste battery in a saturated NaCl solution before separating the cathode material to allow the battery to be fully discharged.
7. The method according to claim 1, wherein, Separating the cathode material from the waste battery includes: using a knife to cut open the edge of the waste battery casing to expose the battery cell; and separating the cathode material from the anode material in the battery cell.
8. The method according to claim 1, wherein, The purification of the cathode material was performed by placing the cathode material in a muffle furnace at 600 °C for 2 hours.
9. The method according to claim 1, wherein, The grinding of the electrochemical catalyst includes grinding the electrochemical catalyst for 2 hours using a ball mill equipped with ZrO2 balls at a speed of 450 rpm.
10. The method according to claim 1, wherein, The plasma treatment is performed using sulfur hexafluoride (SF6) plasma.
11. A method for upgrading and reprocessing LiCoO2 material from spent lithium-ion batteries into a LiCoNiFePd catalyst and using the LiCoNiFePd catalyst to construct an anode-gas diffusion layer for anion exchange membrane water electrolysis, comprising: Separate the LiCoO2 material from the waste lithium-ion battery; The LiCoO2 material was purified; The LiCoO2 material was doped with Ni, Fe and Pd to obtain the LiCoNiFePd catalyst; The LiCoNiFePd catalyst is ground to reduce its particle size; as well as The LiCoNiFePd catalyst was subjected to plasma treatment to improve its surface activity. Preparation of anode catalyst ink includes: The LiCoNiFePd catalyst, sulfonated tetrafluoroethylene vinyl fluorinated copolymer, anhydrous ethanol, and deionized water were mixed in a ratio of 1 mg:20 μL:0.5 mL:0.5 mL to form a mixture; and The mixture was ultrasonically treated in an ice bath for 1 hour to obtain the anode catalyst ink; as well as The anode catalyst ink was prepared at 10 mg / cm³ 2 The load is sprayed onto nickel foam on a hot plate at 80°C to form the anode gas diffusion layer.
12. The method according to claim 11, wherein, Doping the LiCoO2 material with Ni, Fe and Pd includes: mixing the LiCoO2 material with Fe2O3, NiO and Pd(NO3)2 to form a mixture; and sintering the mixture in ambient air to form the LiCoNiFePd catalyst.
13. The method according to claim 12, wherein, The mixture is sintered by sintering at 5 to 10 °C for 1 minute. −1 The heating process is performed by heating the mixture from ambient temperature to a sintering temperature within a range of 700 to 850 °C, such that the LiCoNiFePd catalyst exhibits LiCo... 0.79 Ni 0.1 Fe 0.1 Pd 0.01 The composition and layered structure of O2.
14. The method according to claim 11, wherein, Separating the cathode material from the waste battery includes: using a knife to cut open the edge of the waste battery casing to expose the battery cell; and separating the cathode material from the anode material in the battery cell.
15. The method according to claim 11, wherein, The purification of the cathode material was performed by placing the cathode material in a muffle furnace at 600°C for 2 hours.
16. The method according to claim 11, wherein, The grinding of the electrochemical catalyst includes grinding the electrochemical catalyst for 2 hours using a ball mill equipped with ZrO2 balls at a speed of 450 rpm.
17. The method according to claim 11, wherein, The plasma treatment is performed using sulfur hexafluoride (SF6) plasma.
Citation Information
Patent Citations
Regeneration of lithium cathode materials
US20220376312A1
Process for recycling negative-electrode materials from spent lithium batteries
US6511639B1