A method for preparing an iridium oxide / cobalt hydroxyoxide heterojunction catalyst and its application
By preparing an iridium oxide/cobalt hydroxyoxide heterojunction catalyst, the problems of scarcity and high cost of iridium-based catalysts in water electrolysis for hydrogen production were solved, achieving high-efficiency and low-cost OER catalytic performance suitable for both acidic and alkaline environments.
Patent Information
- Application Number
- CN202610858321.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-06-15
- Publication Date
- 2026-11-17
AI Technical Summary
In existing water electrolysis hydrogen production technologies, the scarcity and high cost of iridium-based catalysts result in slow kinetics and high overpotentials in the oxygen evolution reaction at the anode, making it difficult to achieve efficient and low-cost OER catalysis.
A two-step hydrothermal method was used to prepare an iridium oxide/cobalt hydroxyoxide heterojunction catalyst. The heterostructure formed by IrO2 and CoOOH was utilized to promote electronic effects and charge transfer by leveraging their strong interaction, thereby optimizing the electronic structure of the electrochemical reaction intermediate, exposing more active sites, and improving catalytic performance.
This study achieved low overpotential and good stability of the OER reaction under acidic and alkaline conditions, reduced catalyst costs, and improved the efficiency and stability of hydrogen production through water electrolysis.
Smart Images

Figure CN123108624A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of catalysts for hydrogen production through water electrolysis; more specifically, it relates to a method for preparing an iridium oxide / cobalt hydroxyoxide heterojunction catalyst and its application as an OER catalyst. Background Technology
[0002] Electrolysis of water to produce hydrogen is a core technology in the green hydrogen industry. Among them, proton exchange membrane (PEM) electrolysis is the preferred technology for large-scale production. Its performance bottleneck lies in the slow kinetics and high overpotential of the oxygen evolution reaction (OER). Iridium-based catalysts are OER catalysts that can adapt to the harsh conditions of strong acidity and high oxidation in this technology. However, iridium is scarce in the earth's crust and expensive, resulting in high costs for PEM electrolysis of water to produce hydrogen.
[0003] To reduce iridium usage and improve its utilization, iridium oxide can be loaded onto transition metal oxides with high specific surface areas, leveraging the synergistic effect of iridium and transition metal oxides to enhance OER catalytic performance. In particular, constructing heterostructures of iridium oxide and transition metal oxides can further enhance the synergistic effect, enabling atomic-scale tuning of electronic structure, optimizing mass transfer efficiency, and improving catalyst stability and lifetime. Cobalt hydroxyoxide, with its unique crystal structure, good conductivity, and potential for synergistic effects with iridium, has become a preferred transition metal oxide material. Therefore, the preparation of OER catalysts with iridium oxide / cobalt hydroxyoxide heterostructures has become an important research direction in this field. Summary of the Invention
[0004] This invention aims to further develop existing technologies and discloses a method for preparing an iridium oxide / cobalt hydroxyoxide heterojunction catalyst, comprising the following steps: S1, first dissolve ammonium persulfate and cobalt salt in water, then react the mixed solution hydrothermally at 80~100℃ for 20~30h, and after washing and drying the reaction product, cobalt hydroxyl oxide is obtained; S2 involves first dispersing cobalt hydroxyoxide in water, then adding ammonium persulfate and iridium salt, and finally reacting the mixed solution hydrothermally at 150-200℃ for 8-15 hours to form a catalyst with an IrO2 / CoOOH heterostructure.
[0005] Preferably, the concentrations of cobalt salt and ammonium persulfate in the mixed solution of step S1 are both 0.01~0.1M.
[0006] Preferably, the hydrothermal reaction temperature in step S1 is 85~95℃ and the time is 20~25h.
[0007] Preferably, the concentration of ammonium persulfate in the mixed solution of step S2 is 5~50mM, and the concentration of iridium salt is 1~10mM.
[0008] Preferably, the hydrothermal reaction temperature in step S2 is 175~185℃ and the time is 8~12h.
[0009] Preferably, the cobalt salt is cobalt sulfate.
[0010] Preferably, the iridium salt is iridium chloride.
[0011] The present invention also discloses the application of the iridium oxide / cobalt hydroxyoxide heterojunction catalyst obtained by the aforementioned preparation method as an OER catalyst in water electrolysis for hydrogen production.
[0012] Furthermore, the electrolysis of water to produce hydrogen is carried out in an acidic or alkaline environment.
[0013] The technical solution of the present invention has the following beneficial effects: 1. The preparation method of this invention combines iridium oxide (IrO2) with cobalt hydroxyoxide (CoOOH) to form an IrO2 / CoOOH heterostructure. IrO2 acts as a highly efficient active site, forming a heterostructure with CoOOH and exhibiting strong interactions. This strong interaction promotes electronic effects between Ir and Co, induces charge transfer between components, and modulates the electronic structure of electrochemical reaction intermediates. This, in turn, affects the adsorption and desorption between active sites and reactants and intermediates, promotes water dissociation, accelerates the reaction rate, and facilitates the oxygen evolution reaction (OER). Furthermore, this invention alters the microstructure of cobalt hydroxyoxide through a two-step hydrothermal reaction, which helps expose more active sites and synergistically enhances its OER catalytic performance.
[0014] 2. This invention employs a two-step hydrothermal method to prepare iridium oxide / cobalt hydroxyoxide heterojunction catalysts. The process is simple and can be industrialized at low cost.
[0015] 3. In the iridium oxide / cobalt hydroxyoxide heterojunction catalyst of the present invention, cobalt hydroxyoxide exhibits good chemical stability and corrosion resistance, which is beneficial for the catalyst to operate stably for a long time in acidic environments. Electrochemical test results show that the catalyst has a low overpotential in both acidic and alkaline OER reactions (247mV@10mAcm in acidic environments). -2 Alkaline 286mV@10mAcm -2 It exhibits good stability.
[0016] To more clearly illustrate the purpose, technical solution, and advantages of the present invention, the present invention will be further described in detail below with reference to the accompanying drawings and specific embodiments.
[0017] This invention aims to further develop existing technologies and discloses a method for preparing an iridium oxide / cobalt hydroxyoxide heterojunction catalyst, comprising the following steps: S1, first dissolve ammonium persulfate and cobalt salt in water, then react the mixed solution hydrothermally at 80~100℃ for 20~30h, and after washing and drying the reaction product, cobalt hydroxyl oxide is obtained; S2 involves first dispersing cobalt hydroxyoxide in water, then adding ammonium persulfate and iridium salt, and finally reacting the mixed solution hydrothermally at 150-200℃ for 8-15 hours to form a catalyst with an IrO2 / CoOOH heterostructure.
[0018] Preferably, the concentrations of cobalt salt and ammonium persulfate in the mixed solution of step S1 are both 0.01~0.1M.
[0019] Preferably, the hydrothermal reaction temperature in step S1 is 85~95℃ and the time is 20~25h.
[0020] Preferably, the concentration of ammonium persulfate in the mixed solution of step S2 is 5~50mM, and the concentration of iridium salt is 1~10mM.
[0021] Preferably, the hydrothermal reaction temperature in step S2 is 175~185℃ and the time is 8~12h.
[0022] Preferably, the cobalt salt is cobalt sulfate.
[0023] Preferably, the iridium salt is iridium chloride.
[0024] The present invention also discloses the application of the iridium oxide / cobalt hydroxyoxide heterojunction catalyst obtained by the aforementioned preparation method as an OER catalyst in water electrolysis for hydrogen production.
[0025] Furthermore, the electrolysis of water to produce hydrogen is carried out in an acidic or alkaline environment.
[0026] The technical solution of the present invention has the following beneficial effects: 1. The preparation method of this invention combines iridium oxide (IrO2) with cobalt hydroxyoxide (CoOOH) to form an IrO2 / CoOOH heterostructure. IrO2 acts as a highly efficient active site, forming a heterostructure with CoOOH and exhibiting strong interactions. This strong interaction promotes electronic effects between Ir and Co, induces charge transfer between components, and modulates the electronic structure of electrochemical reaction intermediates. This, in turn, affects the adsorption and desorption between active sites and reactants and intermediates, promotes water dissociation, accelerates the reaction rate, and facilitates the oxygen evolution reaction (OER). Furthermore, this invention alters the microstructure of cobalt hydroxyoxide through a two-step hydrothermal reaction, which helps expose more active sites and synergistically enhances its OER catalytic performance.
[0027] 2. This invention employs a two-step hydrothermal method to prepare iridium oxide / cobalt hydroxyoxide heterojunction catalysts. The process is simple and can be industrialized at low cost.
[0028] 3. In the iridium oxide / cobalt hydroxyoxide heterojunction catalyst of the present invention, cobalt hydroxyoxide exhibits good chemical stability and corrosion resistance, which is beneficial for the catalyst to operate stably for a long time in acidic environments. Electrochemical test results show that the catalyst has a low overpotential in both acidic and alkaline OER reactions (247mV@10mAcm in acidic environments). -2 Alkaline 286mV@10mAcm -2 It exhibits good stability.
[0029] To more clearly illustrate the purpose, technical solution, and advantages of the present invention, the present invention will be further described in detail below with reference to the accompanying drawings and specific embodiments. Attached Figure Description
[0030] Figure 1 In the image: a is the XRD pattern of CoOOH and IrO2 / CoOOH catalysts, and b is the XRD pattern of Co3O4 and IrO2 / Co3O4 catalysts.
[0031] Figure 2 This is a SEM image of CoOOH.
[0032] Figure 3 This is a SEM image of the IrO2 / CoOOH catalyst.
[0033] Figure 4 This is a TEM image of the IrO2 / CoOOH catalyst.
[0034] Figure 5 This is a SEM image of Co3O4.
[0035] Figure 6 This is a SEM image of the IrO2 / Co3O4 catalyst.
[0036] Figure 7 In the image: a is the XPS total spectrum of CoOOH and IrO2 / CoOOH catalysts, and b is the XPS total spectrum of Co3O4 and IrO2 / Co3O4 catalysts.
[0037] Figure 8 In the image: a is the Co 2p XPS spectrum of CoOOH and IrO2 / CoOOH catalysts, b is the Co 2p XPS spectrum of Co3O4 and IrO2 / Co3O4 catalysts, c is the Ir 4f XPS spectrum of IrO2 / CoOOH catalyst, and c is the Ir 4f XPS spectrum of IrO2 / Co3O4 catalyst.
[0038] Figure 9The results are electrochemical tests of IrO2 / CoOOH, IrO2 / Co3O4 and commercial IrO2 catalysts in 0.5M H2SO4, where: a is the LSV curve, b is the overpotential comparison at different current densities, c is the Tafel slope, and d is the EIS impedance.
[0039] Figure 10 In the middle: a, b, and c are the CV curves of commercial IrO2, IrO2 / CoOOH, and IrO2 / Co3O4 catalysts at different scan rates, respectively. d is a comparison of the double-layer capacitance (Cdl) of the three catalysts.
[0040] Figure 11 The IrO2 / CoOOH catalyst in 0.5M H2SO4 at 50 mA cm⁻¹ -2 Stability test results at current density.
[0041] Figure 12 This is a SEM image of the IrO2 / CoOOH catalyst after 500 cycles of CV testing.
[0042] Figure 13 The results show the electrochemical test results of IrO2 / CoOOH, IrO2 / Co3O4 and commercial IrO2 catalysts in 1M KOH, where: a is the LSV curve, b is the overpotential comparison at different current densities, c is the Tafel slope, and d is the EIS impedance. Detailed Implementation
[0043] Numerous specific details are set forth in the following description to provide a thorough understanding of the invention; however, the invention may also be implemented using other variations or substitutions. Therefore, other possible implementations that can be discerned by those skilled in the art based on the embodiments described herein are all within the scope of protection of this invention.
[0044] The iridium oxide / cobalt hydroxyoxide heterojunction catalyst of the present invention is prepared by a two-step hydrothermal method, including step S1 of synthesizing cobalt hydroxyoxide and step S2 of reacting with Ir salt to synthesize the iridium oxide / cobalt hydroxyoxide heterojunction catalyst.
[0045] In step S1, appropriate amounts of ammonium persulfate and cobalt salt are dissolved in water, and the mixed solution is then hydrothermally reacted at 80-100℃ for 20-30 hours. The reaction product is washed and dried to obtain cobalt hydroxyl oxide. In step S2, cobalt hydroxyl oxide is dispersed in water, and appropriate amounts of ammonium persulfate and iridium salt are added. The mixed solution is then hydrothermally reacted at 150-200℃ for 8-15 hours to obtain a catalyst with an IrO2 / CoOOH heterostructure.
[0046] Specifically, in step S1, the concentrations of ammonium persulfate and cobalt salt in the mixed solution can be the same or different, preferably 0.01~0.1M (mol / L), more preferably 0.01~0.05M. In step S2, the concentration of ammonium persulfate in the mixed solution is preferably 5~50mM (mmol / L), more preferably 5~10mM; the concentration of iridium salt is preferably 1~10mM, more preferably 1~5mM.
[0047] The following is a detailed description with reference to the embodiments.
[0048] Example (IrO2 / CoOOH catalyst) 114 mg (≈0.5 mmol) of ammonium persulfate and 140.5 mg (≈0.5 mmol) of CoSO4·7H2O were dissolved in 30 mL of deionized water and stirred at room temperature for 10 min. The resulting mixture was then transferred to a Teflon high-pressure reactor, heated to 90 °C, and maintained at that temperature for 24 h. The reaction product was washed three times with deionized water and anhydrous ethanol, and then dried in a vacuum drying oven at 60 °C for 6 h to obtain CoOOH.
[0049] 30 mg (≈0.13 mmol) of ammonium persulfate and 30 mg of CoOOH were dispersed in 20 mL of deionized water and stirred at room temperature for 10 min. Then, 15 mg (≈0.043 mmol) of IrCl3·3H2O was added. The resulting mixed solution was then transferred to a Teflon high-pressure reactor, heated to 180 °C and kept at that temperature for 10 h. The resulting catalyst was labeled as IrO2 / CoOOH.
[0050] Comparative example (IrO2 / Co3O4 catalyst) 80 mg NaOH and 85 mg CoSO4·7H2O were dissolved in 30 mL of deionized water and stirred at room temperature for 10 min. The mixture was then transferred to a Teflon high-pressure reactor, heated to 90 °C, and maintained at that temperature for 24 h. The reaction product was washed three times with deionized water and anhydrous ethanol, and then dried in a vacuum drying oven at 60 °C for 6 h to obtain Co3O4.
[0051] 30 mg ammonium persulfate and 30 mg Co3O4 were dispersed in 20 mL of deionized water and stirred at room temperature for 10 min. Then, 15 mg IrCl3·3H2O was added. The resulting mixed solution was then transferred to a Teflon high-pressure reactor, heated to 180 °C and kept at that temperature for 10 h. The resulting catalyst was labeled as IrO2 / Co3O4.
[0052] Morphological and phase analysis
[0053] Figure 1a is the XRD pattern of IrO2 / CoOOH catalyst and CoOOH, where the diffraction peak of CoOOH corresponds to CoOOH (PDF#01-071-5039). The IrO2 / CoOOH catalyst shows a relatively broad diffraction peak near 28.1°, which can be attributed to the (110) crystal plane of IrO2. Figure 1 b is the XRD pattern of Co3O4 and IrO2 / Co3O4, with its diffraction peaks corresponding to Co3O4 (PDF#01-080-1536).
[0054] Figure 2 This is a SEM image of CoOOH. Figure 3 This is a SEM image of the IrO2 / CoOOH catalyst. (Comparison) Figure 2 and Figure 3 It is evident that after reacting with Ir salt to form a heterojunction catalyst, the microstructure of CoOOH undergoes a significant change, transforming from spherical to irregular particles. Figure 4 The image shows a TEM image of the IrO2 / CoOOH catalyst, which displays two different lattice stripe spacings. The lattice stripe spacing of approximately 0.452 nm corresponds to the (002) crystal plane of CoOOH, while the lattice stripe spacing of approximately 0.249 nm matches the (101) crystal plane of rutile IrO2. A heterostructure interface is formed between CoOOH and IrO2, confirming the successful synthesis of the IrO2 / CoOOH heterostructure catalyst. Figure 5 This is a SEM image of Co3O4. Figure 6 This is a SEM image of the IrO2 / Co3O4 catalyst. (Comparison) Figure 5 and Figure 6 It is evident that the initial structure of Co3O4 has been partially disrupted.
[0055] Figure 7 a is the XPS total spectrum of CoOOH and IrO2 / CoOOH. Figure 7 b is the XPS total spectrum of Co3O4 and IrO2 / Co3O4. Figure 8 a shows the Co 2p XPS spectra of CoOOH and IrO2 / CoOOH. A significant difference from CoOOH is the presence of a prominent Co 2p chromatogram in the XPS spectrum of IrO2 / CoOOH. 2+ Signal, and Co 3+ 2p 3 / 2 The characteristic peak shifted from 781.07 eV to 780.85 eV. This change in the Co valence state proves that there is a strong electronic interaction between the Ir species and CoOOH. Figure 8 b is the Co 2p XPS spectrum of Co3O4 and IrO2 / Co3O4, neither of which shows Co. 2+The signal proves that the Ir species and Co3O4 do not have the aforementioned strong electronic interaction. Figure 8 c and 8d are the Ir 4f XPS spectra of IrO2 / CoOOH and IrO2 / Co3O4, respectively, further confirming the Ir... 4+ The existence of (IrO2) species.
[0056] Based on the above characterization results, it can be seen that CoOOH forms an IrO2 / CoOOH heterostructure during the second-step hydrothermal synthesis of IrO2. IrO2 and CoOOH interact sufficiently, leading to the transfer of electrons from Ir to Co. This electronic interaction between Ir and Co optimizes the intrinsic activity of Ir sites, thereby endowing the catalyst with better intrinsic activity and stability. At the same time, the IrO2 / CoOOH catalyst exhibits an irregular particle morphology, which is conducive to exposing more active sites and providing abundant surface defects, thus synergistically improving its OER catalytic performance.
[0057] OER electrocatalytic performance test The tests were conducted using a three-electrode system on an electrochemical workstation under the following conditions: 0.5 M H2SO4 and 1 M KOH solutions saturated with O2; the reference electrode was an Ag / AgCl electrode, and the counter electrode was a Pt sheet electrode.
[0058] Figure 9 This is a comparison of the OER electrochemical test results of IrO2 / CoOOH, IrO2 / Co3O4, and a commercial IrO2 catalyst in 0.5 M H2SO4. Among them, IrO2 / CoOOH showed the best OER at 10 mAcm⁻¹. -2 The OER overpotential at current density is 247 mV, and at 100 mAcm -2 The OER overpotential at current density is 295 mV, and the Tafel slope is only 43.94 mV dec. -1 The lowest EIS impedance indicates that its catalytic activity, catalytic efficiency, and catalytic impedance for acidic OER reactions are significantly better than IrO2 / Co3O4 and commercial IrO2.
[0059] Figure 10 This is a comparison chart of double-layer capacitance (Cdl) used to evaluate electrochemical surface area (ECSA), where the Cdl of the IrO2 / CoOOH catalyst is 113.83 mF cm⁻¹. -2 The concentration was significantly higher than that of IrO2 / Co3O4 and commercial IrO2 catalysts, indicating that IrO2 / CoOOH can provide more active sites in the OER process.
[0060] Figure 11This is the OER chronopotential curve of the IrO2 / CoOOH catalyst in 0.5M H2SO4. It can be seen that at 50 mAcm... -2 The catalytic activity of IrO2 / CoOOH hardly decayed even after operating at the specified current density for more than 50 hours. Figure 12 The image shows the SEM image of IrO2 / CoOOH after 500 cycles of CV testing. The catalyst morphology did not change significantly, proving its structural stability.
[0061] Figure 13 These are the OER electrochemical test results for IrO2 / CoOOH, IrO2 / Co3O4, and commercial RuO2 in 1M KOH, with IrO2 / CoOOH at 10 mA cm⁻¹. -2 The OER overpotential at a current density of 286 mV is at 100 mA cm⁻¹. -2 The OER overpotential at current density is 374 mV, and the Tafel slope is only 60.12 mV dec. -1 The lowest EIS impedance indicates that its catalytic activity, catalytic efficiency, and catalytic impedance for the OER reaction under alkaline conditions are superior to IrO2 / Co3O4 and commercial RuO2.
[0062] In summary, the two-step hydrothermal preparation method of the present invention can obtain an iridium oxide / cobalt hydroxyoxide heterojunction catalyst, which exhibits excellent oxygen evolution reaction (OER) catalytic performance in both acidic and alkaline environments for electrocatalytic water splitting, opening up new avenues for the research and development of hydrogen production catalysts by water electrolysis.
Claims
1. A method for preparing an iridium oxide / cobalt hydroxyoxide heterojunction catalyst, characterized in that... Includes the following steps: S1, first dissolve ammonium persulfate and cobalt salt in water, then react the mixed solution hydrothermally at 80~100℃ for 20~30h, and after washing and drying the reaction product, cobalt hydroxyl oxide is obtained; S2, first disperse cobalt hydroxyoxide in water, add ammonium persulfate and iridium salt, then react the mixed solution hydrothermally at 150~200℃ for 8~15h to obtain IrO2 / CoOOH heterostructure catalyst.
2. The method for preparing the iridium oxide / cobalt hydroxyoxide heterojunction catalyst according to claim 1; characterized in that: In step S1, the concentrations of cobalt salt and ammonium persulfate in the mixed solution are both 0.01~0.1M.
3. The method for preparing the iridium oxide / cobalt hydroxyoxide heterojunction catalyst according to claim 1; characterized in that: In step S1, the hydrothermal reaction temperature is 85~95℃ and the time is 20~25h.
4. The method for preparing the iridium oxide / cobalt hydroxyoxide heterojunction catalyst according to claim 1; characterized in that: In step S2, the concentration of ammonium persulfate in the mixed solution is 5-50 mM, and the concentration of iridium salt is 1-10 mM.
5. The method for preparing the iridium oxide / cobalt hydroxyoxide heterojunction catalyst according to claim 1; characterized in that: In step S2, the hydrothermal reaction temperature is 175~185℃ and the time is 8~12h.
6. The method for preparing the iridium oxide / cobalt hydroxyoxide heterojunction catalyst according to claim 1; characterized in that: The cobalt salt is cobalt sulfate.
7. The method for preparing the iridium oxide / cobalt hydroxyoxide heterojunction catalyst according to claim 1; characterized in that: The iridium salt is iridium chloride.
8. The application of the iridium oxide / cobalt hydroxyoxide heterojunction catalyst obtained by any one of claims 1-7 as an OER catalyst in water electrolysis for hydrogen production.