A multi-element alloy catalyst, its preparation method and application

By employing a multi-element alloy catalyst preparation method involving gradient magnetron sputtering and nitrogen doping, the dual functionality and stability issues of water electrolysis catalysts have been resolved, enabling efficient hydrogen and oxygen production through water electrolysis, which is suitable for industrial production.

CN123108625APending Publication Date: 2026-11-17SHANGHAI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611234088.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-14
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing water electrolysis catalysts suffer from weak bifunctional catalytic performance, poor structural stability, insufficient adaptability to operating conditions, and low refinement of preparation processes, failing to meet the needs of large-scale industrial alkaline water electrolysis production.

Method used

A multi-element alloy catalyst consisting of a Cr adhesion layer, a dense support layer, and a Mo/N-rich functional surface layer was constructed using a three-step gradient magnetron sputtering process. Combined with segmented nitrogen doping and cyclic voltammetry activation, a catalytic system with strong adhesion, high stability, and abundant defective active sites was formed.

Benefits of technology

It significantly improves the efficiency of hydrogen and oxygen production through water electrolysis, extends the service life of the catalyst, reduces the energy consumption of total water electrolysis, and is suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention relates to the field of electrocatalysis technology, and discloses a multi-element alloy catalyst, its preparation method, and its application. The method includes: performing a first magnetron sputtering on a conductive substrate using a pure Cr target to obtain a Cr adhesion layer; independently setting FeCrNi, Co, and Mo targets, and introducing a trace amount of nitrogen gas to perform a second magnetron sputtering on the Cr adhesion layer to obtain a support layer; increasing the nitrogen gas introduction rate to perform a third magnetron sputtering to obtain a Mo / N-rich layer; and activating the composite material using cyclic voltammetry after sputtering to obtain the multi-element alloy catalyst. This invention strengthens the film-substrate bonding through a substrate adhesion layer, achieves structural stability and activity zoning through gradient functional layers, optimizes electronic configuration through precise nitrogen doping, and constructs a porous, defective active structure through electrochemical activation. Relying on the synergistic catalytic effect of multiple metal components, the catalyst possesses excellent dual-function catalytic performance for hydrogen evolution and oxygen evolution.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of electrocatalysis technology, and more specifically, to a multi-element alloy catalyst, its preparation method, and its application. Background Technology

[0002] Green hydrogen energy, as a core carrier of clean and renewable energy, has become a key path to solve the pollution problem of traditional fossil fuels and achieve the transformation and upgrading of the energy structure. Water electrolysis for hydrogen production can achieve zero-carbon emission hydrogen production using renewable energy sources such as wind power and photovoltaics. It is currently the mainstream technology for large-scale production of high-purity green hydrogen. Among them, alkaline water electrolysis technology has become the core development direction of the hydrogen energy industry due to its advantages of low equipment cost, mature process, and suitability for large-scale industrial production. The water electrolysis process includes two core electrochemical reactions: the hydrogen evolution reaction (HER) at the cathode and the oxygen evolution reaction (OER) at the anode. However, the OER reaction suffers from the slow kinetics of four-proton, four-electron coupling transfer, and the HER reaction also suffers from the lag in elementary reaction rates in alkaline media. These dual reaction bottlenecks lead to high overall energy consumption and insufficient conversion efficiency in water electrolysis. High-performance electrocatalysts are the core components for reducing reaction energy barriers, improving water electrolysis efficiency, and ensuring long-term stable operation of equipment.

[0003] Currently, water electrolysis catalysts in commercial and research fields are mainly divided into two categories: noble metal-based catalysts and non-noble metal-based catalysts. Among them, noble metal-based catalysts such as platinum, iridium, and ruthenium possess excellent catalytic activity, but their crustal reserves are scarce, their preparation costs are high, and they are prone to particle agglomeration and deactivation under long-term operating conditions, making them unsuitable for large-scale industrial water electrolysis production. Therefore, the industry focuses on developing low-cost, high-stability transition metal-based non-noble metal catalysts, especially nickel-based, iron-based, molybdenum-based, and cobalt-based alloy materials, which have been extensively studied. Due to their good conductivity, tunable electronic structure, and excellent electrochemical activity, they have become the optimal alternative to noble metal catalysts.

[0004] Existing transition metal alloy catalysts still suffer from numerous technical shortcomings, hindering the industrialization and upgrading of alkaline water electrolysis technology. Firstly, single or binary alloys have limited active sites, failing to simultaneously meet the dual-functional catalytic requirements of HER and OER reactions. This makes it difficult to achieve efficient and synergistic catalysis for complete water electrolysis. Most catalysts are only suitable for anode or cathode reactions, resulting in poor equipment adaptability and high integration costs. Secondly, traditional alloy catalysts often employ single-target sputtering and simple mixing and doping processes, leading to poor material structure uniformity, low precision in component control, and an inability to construct gradient functional structures. This results in easy detachment of active sites on the catalyst surface and weak substrate bonding. Under the harsh electrolysis conditions of high current, high temperature, and concentrated alkali, problems such as structural distortion, active phase dissolution, and carbon substrate corrosion and diffusion easily occur, significantly shortening the service life. Thirdly, conventional alloy catalysts lack precise defect control and in-situ activation mechanisms. Their fixed electronic structure and stable crystal structure prevent adaptive reconstruction and optimization of active sites under various operating conditions. The high energy barrier for adsorbing reaction intermediates makes further improvement in catalytic activity difficult, and the operational stability at high current densities cannot meet industrial production standards.

[0005] In recent years, medium-entropy / high-entropy multi-element alloy catalysts have become a research hotspot in the field of electrocatalysis due to their ability to simultaneously provide abundant HER and OER active sites through the synergistic effect of multi-metal components. However, the existing preparation processes for multi-element alloy catalysts are immature, generally suffering from disordered component ratios, crude doping control, and unclear structural stratification, making it impossible to achieve functional zoning designs that enable substrate adhesion, structural support, and activity enrichment. Furthermore, most multi-element alloy catalysts lack targeted post-treatment activation processes, failing to effectively release the metastable structure and lattice distortion advantages within the material, making it difficult to form porous defect active structures. This results in defects such as insufficient specific surface area, scarce unsaturated coordination sites, and weak hydrogen overflow capacity, ultimately manifesting as high overpotential, high energy consumption for total water electrolysis, and poor long-term operational stability, making them unsuitable for the high current density and long-cycle requirements of industrial water electrolysis production.

[0006] In summary, current water electrolysis catalysts generally suffer from technical challenges such as weak bifunctional catalytic performance, poor structural stability, insufficient adaptability to operating conditions, low refinement of preparation processes, and inadequate long-term service life, severely limiting the large-scale application of alkaline water electrolysis for hydrogen production. To address these shortcomings, this invention proposes a method for preparing a gradient-structured multi-element alloy catalyst. Through an integrated process of multi-target co-sputtering layered preparation, precise nitrogen doping control, and electrochemical in-situ activation and reconstruction, a five-element alloy catalytic system with strong adhesion, high stability, and abundant defective active sites is constructed. This solves the problems of insufficient activity, easy structural failure, and poor bifunctional adaptability of traditional catalysts, significantly improving the efficiency of hydrogen and oxygen production from water electrolysis and extending catalyst lifespan, making it suitable for large-scale industrial alkaline water electrolysis production scenarios. Summary of the Invention

[0007] In view of this, the present invention proposes a multi-element alloy catalyst, its preparation method and application, aiming to solve the problems of insufficient bifunctional catalytic capacity, poor membrane-substrate bonding strength, easy structural failure under high current alkaline environment, low precision of component and defect control, high catalytic overpotential and difficulty in meeting the long-term stability requirements of industrial applications in current non-precious metal catalysts for water electrolysis.

[0008] This invention proposes a method for preparing a multi-element alloy catalyst, comprising the following steps: 1) A Cr adhesion layer was obtained by first magnetron sputtering on the surface of a conductive substrate using a pure Cr target as the target material; 2) FeCrNi target, Co target and Mo target are set independently, and a trace amount of nitrogen gas is introduced to perform a second magnetron sputtering on the Cr adhesion layer to obtain the support layer; 3) Based on step 2), keep the target material unchanged, increase the nitrogen gas flow rate and perform a third magnetron sputtering to obtain a Mo / N-rich layer; 4) Using the sputtered composite material as the working electrode and potassium hydroxide solution as the electrolyte, the composite material was activated by cyclic voltammetry to obtain a multi-element alloy catalyst.

[0009] Preferably, the conductive substrate is a high-purity graphite sheet or carbon paper; The carbon content of the high-purity graphite sheet is ≥99.99wt%.

[0010] Preferably, the conditions for the first magnetron sputtering are as follows: The atmosphere in the sputtering chamber is argon with a purity ≥99.999%, the argon flow rate is 70~90 sccm, and the gas pressure in the magnetron sputtering equipment chamber is 0.4~0.6 Pa; The initial temperature of the substrate is 95~105℃, and the substrate temperature is increased to 145~155℃ when sputtering reaches 1 / 3~2 / 3. The total sputtering time is 5~10 minutes, and the target power is 90~110W.

[0011] Preferably, the atomic ratio of Fe, Cr, and Ni in the FeCrNi target is 1:1:1; The purity of Co in the Co target is ≥99.95%, and the purity of Mo in the Mo target is ≥99.95%.

[0012] Preferably, the conditions for the second magnetron sputtering are as follows: The working gases are argon and nitrogen, with an argon flow rate of 70-90 sccm and a nitrogen flow rate of 5-8 sccm. The gas pressure inside the magnetron sputtering equipment cavity is 0.4-0.6 Pa. The temperature of the substrate is 95~105℃; The power of the FeCrNi target is 90~110W, the power of the Co target is 15~20W, and the power of the Mo target is 8~12W. The total sputtering time is 50-70 minutes.

[0013] Preferably, the conditions for the third magnetron sputtering are as follows: The working gases are argon and nitrogen, with an argon flow rate of 60-70 sccm and a nitrogen flow rate of 25-30 sccm. The gas pressure inside the magnetron sputtering equipment cavity is 0.4-0.6 Pa. The temperature of the substrate is 95~105℃; The power of the FeCrNi target is 70~80W, the power of the Co target is 25~30W, and the power of the Mo target is 40~45W. The total sputtering time is 30-40 minutes.

[0014] Preferably, the concentration of the potassium hydroxide solution is 1 mol / L; The activation process has a potential window of 0.2~1.6V, a scan speed of 50mV / s, and a number of revolutions of 300~500.

[0015] This invention provides a multi-element alloy catalyst prepared by the above-described preparation method.

[0016] The present invention also provides an application of the aforementioned multi-element alloy catalyst in the electrolysis of water to produce oxygen and / or hydrogen, comprising the following steps: The multi-element alloy catalyst serves as both the anode and cathode for electrolyzing potassium hydroxide solution.

[0017] Preferably, the concentration of the sodium hydroxide solution is 1 mol / L, and the temperature is 60~80℃; The current density during the electrolysis process is 500~2000 mA / cm². 2 .

[0018] Compared with the prior art, the beneficial effects of the present invention are as follows: This invention employs a three-step gradient magnetron sputtering process to construct a three-layer composite gradient structure consisting of a "Cr adhesion layer - dense support layer - Mo / N-rich functional surface layer". The bottom pure Cr adhesion layer forms strong chemical bonds with high-purity graphite and carbon paper substrates, significantly improving the overall adhesion of the film. Simultaneously, it acts as a barrier layer, effectively inhibiting the outward diffusion of carbon elements from the substrate, preventing carbon contamination of the alloy active layer, and blocking electrolyte erosion of the substrate, thus protecting the structural integrity of the conductive substrate. The middle low-nitrogen-doped FeCrNiCoMo dense support layer, with its highly stable Ni and Co components as the framework, has a dense and regular structure and strong mechanical stability. It serves as a rigid support core, effectively resisting structural distortion and stress cracking under high current conditions. This fundamentally solves the defects of traditional catalyst structures, such as easy collapse and short service life, providing a structural basis for long-term catalyst operation.

[0019] This invention constructs a pentagonal medium-entropy alloy system of Fe, Cr, Ni, Co, and Mo, achieving precise functional division based on the synergistic catalytic principle of multiple metal components: Fe and Ni components, as core OER active sites, can efficiently promote the four-electron proton transfer process and reduce the oxygen evolution reaction energy barrier; Mo component possesses excellent hydrogen adsorption and overflow characteristics and can serve as a dedicated HER active site to optimize the adsorption and desorption behavior of hydrogen intermediates; Co and Cr components can effectively regulate the overall electronic configuration of the alloy, improve the material's conductivity and structural robustness, and compensate for the performance shortcomings of single-metal catalysis. This multi-element synergistic system does not require multiple catalysts and can simultaneously serve as both anode and cathode materials for water electrolysis, achieving highly efficient catalysis of complete water splitting, significantly simplifying the structure of electrolysis equipment and reducing the cost of industrial applications.

[0020] This invention employs a segmented nitrogen flow rate precision control strategy. The second sputtering introduces a trace amount of nitrogen to achieve low-concentration interstitial solid solution doping of the support layer, moderately optimizing the framework's electronic conductivity. The third sputtering significantly increases the nitrogen flow rate, achieving N atom supersaturation solid solution in the surface layer. Combined with a simultaneous increase in Mo content, this induces strong lattice distortion in the amorphous alloy matrix, precisely controlling the d-band center position of the material. This design effectively optimizes the adsorption and desorption balance of reaction intermediates such as hydroxyl and hydrogen, significantly reducing the energy barriers of HER and OER elementary reactions. Simultaneously, the metastable Mo / N-rich surface layer can store a large number of active defect precursors, providing sufficient structural raw materials for subsequent in-situ activation and reconstruction, fundamentally improving the intrinsic catalytic activity from an electronic structure perspective.

[0021] This invention employs a precise pre-activation process using cyclic voltammetry, relying on the principle of selective dissolution and reconstruction under operating conditions to achieve in-situ modification of the catalyst surface. During activation, the metastable Mo component on the surface selectively dissolves in the form of molybdate, while interstitial nitrogen atoms are oxidized and escaped, constructing a uniform nanoscale mesoporous three-dimensional porous network structure on the material surface, greatly increasing the catalyst's specific surface area. Simultaneously, it induces an in-situ phase transformation in the alloy, generating a highly active amorphous / nanocrystalline mixed-state (Ni,Fe)OOH hydroxy oxide core active phase, while simultaneously generating a large number of oxygen vacancies and unsaturated coordination sites. Furthermore, the residual high-valence Mo-O bonds can stabilize local charges and inhibit excessive oxidation and dissolution of Fe and Ni active components, achieving the dual effect of "high-activity site construction + active component stabilization." Compared to unactivated catalysts, the catalytic performance is exponentially improved. Detailed Implementation

[0022] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as a limitation of the present invention, but rather as a more detailed description of certain aspects, features, and embodiments of the present invention. It should be understood that the terminology used in this invention is merely for describing particular embodiments and is not intended to limit the present invention.

[0023] Furthermore, regarding the numerical ranges in this invention, it should be understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. Every smaller range between any stated value or intermediate value within a stated range, and any other stated value or intermediate value within said range, is also included within this invention. The upper and lower limits of these smaller ranges may be independently included or excluded from the range.

[0024] Unless otherwise stated, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art. While only preferred methods and materials have been described herein, any methods and materials similar or equivalent to those described herein may be used in the implementation or testing of this invention. All references to this specification are incorporated by way of citation to disclose and describe methods and / or materials associated with those references. In the event of any conflict with any incorporated reference, the content of this specification shall prevail.

[0025] Various modifications and variations can be made to the specific embodiments described in this specification without departing from the scope or spirit of the invention, as will be apparent to those skilled in the art. Other embodiments derived from this specification will also be apparent to those skilled in the art. This specification and embodiments are merely exemplary.

[0026] The terms “include,” “including,” “have,” “contain,” etc., used in this article are all open-ended terms, meaning that they include but are not limited to.

[0027] This invention proposes a method for preparing a multi-element alloy catalyst, comprising the following steps: 1) A Cr adhesion layer was obtained by first magnetron sputtering on the surface of a conductive substrate using a pure Cr target as the target material; 2) FeCrNi target, Co target and Mo target are set independently, and a trace amount of nitrogen gas is introduced to perform a second magnetron sputtering on the Cr adhesion layer to obtain the support layer; 3) Based on step 2), keep the target material unchanged, increase the nitrogen gas flow rate and perform a third magnetron sputtering to obtain a Mo / N-rich layer; 4) Using the sputtered composite material as the working electrode and potassium hydroxide solution as the electrolyte, the composite material was activated by cyclic voltammetry to obtain a multi-element alloy catalyst.

[0028] In this invention, the conductive substrate is a high-purity graphite sheet or carbon paper; The carbon content of the high-purity graphite sheet is ≥99.99wt%.

[0029] In this invention, the conductive substrate further includes a pretreatment step before use, as follows: The graphite sheet was polished with 600-grit, 1500-grit, and 6000-grit sandpaper in sequence until the surface was smooth; polished to a mirror finish with a polishing cloth and diamond polishing paste (0.5μm); ultrasonically cleaned in acetone for 15 minutes, then ultrasonically cleaned in anhydrous ethanol for 15 minutes; dried with high-purity nitrogen gas, and placed in a vacuum drying oven at 100°C for 2 hours to remove adsorbed water.

[0030] In this invention, the process before magnetron sputtering includes a step of purging the magnetron sputtering chamber, specifically as follows: closing the chamber, turning on the molecular pump, and evacuating to a vacuum level of ≤5×10⁻⁶. -5 Pa; High-purity Ar (99.999%) was introduced to a concentration of 2 × 10⁻⁶. -2 After purging the gas for 5 minutes, vacuum the gas again and repeat the "purging Ar-vacuuming" cycle 3 times to completely remove oxygen and moisture.

[0031] In this invention, the conditions for the first magnetron sputtering are as follows: The atmosphere in the sputtering chamber is argon with a purity ≥99.999%, the argon flow rate is 70~90 sccm, and the gas pressure in the magnetron sputtering equipment chamber is 0.4~0.6 Pa; The initial temperature of the substrate is 95~105℃, and the substrate temperature is increased to 145~155℃ when sputtering reaches 1 / 3~2 / 3. The total sputtering time is 5~10 minutes, and the target power is 90~110W.

[0032] In this invention, the atomic ratio of Fe, Cr, and Ni in the FeCrNi target is 1:1:1; The purity of Co in the Co target is ≥99.95%, and the purity of Mo in the Mo target is ≥99.95%.

[0033] In this invention, the conditions for the second magnetron sputtering are as follows: The working gases are argon and nitrogen, with an argon flow rate of 70-90 sccm and a nitrogen flow rate of 5-8 sccm. The gas pressure inside the magnetron sputtering equipment cavity is 0.4-0.6 Pa. The temperature of the substrate is 95~105℃; The power of the FeCrNi target is 90~110W, the power of the Co target is 15~20W, and the power of the Mo target is 8~12W. The total sputtering time is 50-70 minutes.

[0034] In this invention, the conditions for the third magnetron sputtering are as follows: The working gases are argon and nitrogen, with an argon flow rate of 60-70 sccm and a nitrogen flow rate of 25-30 sccm. The gas pressure inside the magnetron sputtering equipment cavity is 0.4-0.6 Pa. The temperature of the substrate is 95~105℃; The power of the FeCrNi target is 70~80W, the power of the Co target is 25~30W, and the power of the Mo target is 40~45W. The total sputtering time is 30-40 minutes.

[0035] In this invention, the pressure in the magnetron sputtering cavity is controlled at 0.4~0.6 Pa by adjusting the slide valve.

[0036] In this invention, the concentration of the potassium hydroxide solution is 1 mol / L; The activation process has a potential window of 0.2~1.6V, a scan speed of 50mV / s, and a number of revolutions of 300~500.

[0037] This invention provides a multi-element alloy catalyst prepared by the above-described preparation method.

[0038] The present invention also provides an application of the aforementioned multi-element alloy catalyst in the electrolysis of water to produce oxygen and / or hydrogen, comprising the following steps: The multi-element alloy catalyst serves as both the anode and cathode for electrolyzing potassium hydroxide solution.

[0039] In this invention, the concentration of the sodium hydroxide solution is 1 mol / L, and the temperature is 60~80℃; The current density during the electrolysis process is 500~2000 mA / cm². 2 .

[0040] Example 1 The conductive substrate used in this embodiment is a high-purity graphite sheet with a carbon content of ≥99.99wt%; The target parameters are as follows: the atomic ratio of Fe, Cr and Ni in the FeCrNi target is 1:1:1; the purity of both the Co and Mo targets is ≥99.95%; and the purity of the argon gas used for sputtering is ≥99.999%.

[0041] (1) Substrate pretreatment: High-purity graphite sheets were polished to a smooth surface using 600-grit, 1500-grit, and 6000-grit sandpaper in sequence, and polished to a mirror finish using 0.5μm diamond polishing paste and polishing cloth. After polishing, the graphite sheets were ultrasonically cleaned in acetone for 15 minutes, and then ultrasonically cleaned again with anhydrous ethanol for 15 minutes. After drying with high-purity nitrogen, the sheets were placed in a vacuum drying oven at 100℃ for 2 hours to remove adsorbed water and were ready for use.

[0042] (2) Sputtering chamber pretreatment: Close the magnetron sputtering chamber and turn on the molecular pump to evacuate to ≤5×10 -5 Pa; High-purity argon gas is introduced until the chamber pressure is 2 × 10⁻⁶. -2 After purging the gas for 5 minutes, evacuate again and repeat the "argon filling-evacuation" cycle 3 times to completely remove oxygen and moisture from the chamber. The chamber is then ready for use. Throughout the process, the sputtering pressure in the chamber is kept stable at 0.4~0.6 Pa using a slide gate valve.

[0043] (3) Preparation of Cr adhesion layer: Pure Cr target was used as target material, and the first magnetron sputtering was performed on the surface of pretreated high-purity graphite sheet; the sputtering atmosphere was pure argon gas, the argon gas flow rate was 80 sccm, the chamber pressure was 0.5 Pa; the initial temperature of the substrate was 100℃, and the temperature was raised to 150℃ when sputtering reached 1 / 2 time. The total sputtering time was 8 min, the target power was 100 W, and the Cr adhesion layer was prepared.

[0044] (4) Preparation of support layer: Keep the substrate and chamber state unchanged, independently turn on the FeCrNi target, Co target and Mo target, and perform a second magnetron sputtering; the working gas is argon + trace amount of nitrogen, the argon flow rate is 80 sccm, the nitrogen flow rate is 6 sccm, the substrate temperature is 100℃; the FeCrNi target power is 100W, the Co target power is 18W, the Mo target power is 10W, the total sputtering time is 60min, and a dense support layer is prepared on the Cr adhesion layer surface.

[0045] (5) Preparation of Mo / N rich layer: Keep all targets in the on state, adjust the gas parameters and target power, and perform the third magnetron sputtering; argon flow rate 65 sccm, nitrogen flow rate 28 sccm, substrate temperature 100℃; FeCrNi target power 75W, Co target power 28W, Mo target power 42W, total sputtering time 35min, to prepare Mo / N rich functional layer and obtain multilayer composite material.

[0046] (6) Electrochemical activation: The composite material obtained by sputtering above is used as the working electrode, and 1 mol / L potassium hydroxide solution is used as the electrolyte. Activation is carried out by cyclic voltammetry with a potential window of 0.2~1.6V, a scan rate of 50mV / s, and 400 scans. Finally, the multi-element alloy catalyst of the present invention is obtained.

[0047] Example 2 This embodiment provides a method for preparing a multi-element alloy catalyst. The conductive substrate used is a high-purity graphite sheet with a carbon content ≥99.99 wt%. The target parameters are as follows: the atomic ratio of Fe, Cr, and Ni in the FeCrNi target is 1:1:1; the purity of both the Co and Mo targets is ≥99.95%; and the purity of the argon gas used for sputtering is ≥99.999%. The specific preparation steps are as follows: (1) Substrate pretreatment: High-purity graphite sheets were polished to a smooth surface using 600-grit, 1500-grit, and 6000-grit sandpaper in sequence, and polished to a mirror finish using 0.5μm diamond polishing paste and polishing cloth. After polishing, the graphite sheets were ultrasonically cleaned in acetone for 15 minutes, and then ultrasonically cleaned again with anhydrous ethanol for 15 minutes. After drying with high-purity nitrogen, the sheets were placed in a vacuum drying oven at 100℃ for 2 hours to remove adsorbed water and were ready for use.

[0048] (2) Sputtering chamber pretreatment: Close the magnetron sputtering chamber and turn on the molecular pump to evacuate to ≤5×10 -5 Pa; High-purity argon gas is introduced until the chamber pressure is 2 × 10⁻⁶. -2 After purging the gas for 5 minutes, evacuate again and repeat the "argon filling-evacuation" cycle 3 times to completely remove oxygen and moisture from the chamber. The chamber is then ready for use. Throughout the process, the sputtering pressure in the chamber is kept stable at 0.4~0.6 Pa using a slide gate valve.

[0049] (3) Preparation of Cr adhesion layer: Pure Cr target was used as target material, and the first magnetron sputtering was performed on the surface of pretreated high-purity graphite sheet; the sputtering atmosphere was pure argon gas, the argon gas flow rate was 70 sccm, the chamber pressure was 0.4 Pa; the initial temperature of the substrate was 95℃, and the temperature was raised to 145℃ when sputtering was 1 / 3 of the time, the total sputtering time was 5 min, the target power was 90 W, and the Cr adhesion layer was prepared.

[0050] (4) Preparation of support layer: Keep the substrate and chamber state unchanged, independently turn on the FeCrNi target, Co target and Mo target, and perform a second magnetron sputtering; the working gas is argon + trace amount of nitrogen, the argon flow rate is 70 sccm, the nitrogen flow rate is 5 sccm, the substrate temperature is 95℃; the FeCrNi target power is 90W, the Co target power is 15W, the Mo target power is 8W, the total sputtering time is 50min, and a dense support layer is prepared.

[0051] (5) Preparation of Mo / N rich layer: Keep all target materials in the on state, adjust the process parameters, and perform the third magnetron sputtering; argon flow rate 60 sccm, nitrogen flow rate 25 sccm, substrate temperature 95℃; FeCrNi target power 70W, Co target power 25W, Mo target power 40W, total sputtering time 30min, and Mo / N rich functional layer is prepared.

[0052] (6) Electrochemical activation: The composite material was used as the working electrode, and 1 mol / L potassium hydroxide solution was used as the electrolyte. The activation was carried out by cyclic voltammetry with a potential window of 0.2~1.6V, a scan rate of 50mV / s, and 300 scans to obtain a multi-element alloy catalyst.

[0053] Example 3 This embodiment provides a method for preparing a multi-element alloy catalyst. The conductive substrate used is a high-purity graphite sheet with a carbon content ≥99.99 wt%. The target parameters are as follows: the atomic ratio of Fe, Cr, and Ni in the FeCrNi target is 1:1:1; the purity of both the Co and Mo targets is ≥99.95%; and the purity of the argon gas used for sputtering is ≥99.999%. The specific preparation steps are as follows: (1) Substrate pretreatment: High-purity graphite sheets were polished to a smooth surface using 600-grit, 1500-grit, and 6000-grit sandpaper in sequence, and polished to a mirror finish using 0.5μm diamond polishing paste and polishing cloth. After polishing, the graphite sheets were ultrasonically cleaned in acetone for 15 minutes, and then ultrasonically cleaned again with anhydrous ethanol for 15 minutes. After drying with high-purity nitrogen, the sheets were placed in a vacuum drying oven at 100℃ for 2 hours to remove adsorbed water and were ready for use.

[0054] (2) Sputtering chamber pretreatment: Close the magnetron sputtering chamber and turn on the molecular pump to evacuate to ≤5×10 -5 Pa; High-purity argon gas is introduced until the chamber pressure is 2 × 10⁻⁶. -2 After purging the gas for 5 minutes, evacuate again and repeat the "argon filling-evacuation" cycle 3 times to completely remove oxygen and moisture from the chamber. The chamber is then ready for use. Throughout the process, the sputtering pressure in the chamber is kept stable at 0.4~0.6 Pa using a slide gate valve.

[0055] (3) Preparation of Cr adhesion layer: Pure Cr target was used as target material, and the first magnetron sputtering was performed on the surface of pretreated high-purity graphite sheet; the sputtering atmosphere was pure argon gas, the argon gas flow rate was 90 sccm, the chamber pressure was 0.6 Pa; the initial temperature of the substrate was 105℃, and the temperature was raised to 155℃ when sputtering was 2 / 3 of the time, the total sputtering time was 10 min, the target power was 110 W, and the Cr adhesion layer was prepared.

[0056] (4) Preparation of support layer: Keep the substrate and chamber state unchanged, independently turn on the FeCrNi target, Co target and Mo target, and perform a second magnetron sputtering; the working gas is argon + trace amount of nitrogen, the argon flow rate is 90 sccm, the nitrogen flow rate is 8 sccm, the substrate temperature is 105℃; the FeCrNi target power is 110W, the Co target power is 20W, the Mo target power is 12W, the total sputtering time is 70min, and a dense support layer is prepared.

[0057] (5) Preparation of Mo / N rich layer: Keep all target materials in the on state, adjust the process parameters, and perform the third magnetron sputtering; argon flow rate 70 sccm, nitrogen flow rate 30 sccm, substrate temperature 105℃; FeCrNi target power 80W, Co target power 30W, Mo target power 45W, total sputtering time 40min, and Mo / N rich functional layer is prepared.

[0058] (6) Electrochemical activation: The composite material was used as the working electrode, and 1 mol / L potassium hydroxide solution was used as the electrolyte. The activation was carried out by cyclic voltammetry with a potential window of 0.2~1.6V, a scan rate of 50mV / s, and 500 scans to obtain a multi-element alloy catalyst.

[0059] Comparative Example 1 The substrate, target specifications, substrate pretreatment process, chamber pretreatment process, sputtering pressure control, electrochemical activation parameters, and electrolysis application conditions used in this comparative example are exactly the same as those in Example 1. The only difference is that nitrogen is not introduced during the second and third magnetron sputtering processes, and only high-purity argon is used as the working gas. All other process parameters remain unchanged, and a nitrogen-free multi-element alloy catalyst is finally prepared.

[0060] Comparative Example 2 The substrate, target specifications, substrate pretreatment process, chamber pretreatment process, activation and electrolysis conditions used in this comparative example are completely consistent with those in Example 1. The difference is that the Cr adhesion layer preparation step and the support layer preparation step are omitted. Instead, a Mo / N rich layer is directly sputtered on the surface of the pretreated high-purity graphite sheet substrate using the complete process parameters of the third magnetron sputtering in Example 1 to obtain a single-layer thin film composite material. The same cyclic voltammetric activation process as in Example 1 is used for subsequent treatment.

[0061] Comparative Example 3 The substrate, target specifications, substrate pretreatment process, chamber pretreatment process, activation and electrolysis conditions used in this comparative example are completely consistent with those in Example 1. The only difference is that the first magnetron sputtering step to prepare the Cr adhesion layer is omitted. Instead, the second magnetron sputtering to prepare the support layer and the third magnetron sputtering to prepare the Mo / N rich layer are performed directly on the pretreated high-purity graphite substrate, resulting in a bilayer composite thin film catalyst without a Cr adhesion layer. The subsequent activation process is completely consistent with that in Example 1.

[0062] The properties of the catalysts prepared in the examples and comparative examples were tested. The specific test items and methods are as follows: Testing instruments: electrochemical workstation; three-electrode system for half-cell testing; two-electrode system for complete water splitting testing; electrolyte is uniformly 1 mol / L KOH solution.

[0063] Reference electrode: Hg / HgO electrode; Counter electrode: Platinum sheet; Working electrode: Catalyst graphite sheet electrode prepared in this invention.

[0064] 1. Electrochemical performance testing of half-cells with a three-electrode system 1.1 Linear Scan Voltmeter-Surveillance (LSV) Test Scan rate: 5mV / s; OER potential range: 0.2–1.8V (vs RHE); HER potential range: -0.2 to -1.0V (vs RHE).

[0065] Read and record from LSV curves: 1) OER: Current density 10 mA·cm -2 500mA·cm -2 The corresponding overpotential η 10 -OER, η 500 -OER; 2) HER: Current density 10 mA·cm -2 500mA·cm -2 The corresponding overpotential η 10 -HER、η 500 -HER.

[0066] 1.2 Tafel slope The slopes of OER-Tafel and HER-Tafel were obtained by fitting LSV data; the smaller the Tafel slope, the faster the reaction kinetics.

[0067] 1.3 Electrochemical Impedance (EIS) Test conditions: Apply OER 10mA·cm -2 The corresponding potential, frequency range 10 -2 ~10 5 Hz, amplitude 5mV; Output: Charge transfer resistance Rct. The smaller Rct is, the lower the charge transfer resistance at the electrode / electrolyte interface.

[0068] 1.4 Electrochemical Active Area (ECSA) Cyclic voltammetry (CV), non-redox range, scan rates: 20, 40, 60, 80, 100 mV / s, calculate double-layer capacitance Cdl. Cdl is proportional to ECSA; a larger Cdl indicates more exposed effective catalytic sites.

[0069] 2. Dual-electrode full water electrolysis test (simulating actual water electrolysis conditions) The catalyst serves as both the anode and cathode, the electrolyte is 1 mol / L KOH, and the electrolyte temperature is 70℃.

[0070] Record: 1) Current density 10 mA·cm -2 500mA·cm -2 2000mA·cm -2 Voltage of the fully dissolved water tank under the given conditions.

[0071] 2. Dual-electrode full water electrolysis test (simulating actual water electrolysis conditions) The catalyst serves as both the anode and cathode, the electrolyte is 1 mol / L KOH, and the electrolyte temperature is 70℃.

[0072] Record: 1) Current density 10 mA·cm -2 500mA·cm -2 2000mA·cm -2 Voltage of the fully dissolved water tank under the given conditions.

[0073] 3. Long-term stability test under high current Two-electrode system, constant current density 500 mA·cm -2 The temperature was 70℃, and the system was run continuously for 300 hours. The change in tank voltage over time was recorded. The condition of the film was observed to see if it peeled or detached.

[0074] The test results are shown in Table 1.

[0075] Table 1. Performance test results of catalysts prepared in the examples and comparative examples. Compared to comparative studies that lack nitrogen doping modification, have no gradient layered structure, or omit the Cr adhesion layer, this invention produces a multi-element alloy catalyst prepared through a three-layer gradient structure design, segmented precise nitrogen doping control, and synergistic modification via electrochemical in-situ activation. This catalyst effectively enhances the electrochemical active area, accelerates the hydrogen and oxygen evolution reaction kinetics in water electrolysis, significantly reduces the overall water electrolysis operating voltage, and substantially strengthens the membrane bonding stability by leveraging the interfacial reinforcement and substrate protection of the Cr adhesion layer, the structural stability effect of the dense support layer, the optimized electronic structure of the molybdenum-nitrogen-rich functional layer, and the porous defective active sites constructed after activation. It also significantly strengthens the membrane bonding stability, suppresses performance degradation and membrane detachment under long-term high-current conditions, and fully verifies the positive gain effect of the layered structure, nitrogen doping modification, multi-element metal synergy, and electrochemical activation. Each process step is indispensable, effectively balancing the intrinsic catalytic activity and long-term service stability of the catalyst.

[0076] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and not to limit it. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should understand that modifications or equivalent substitutions can still be made to the specific implementation of the present invention. Any modifications or equivalent substitutions that do not depart from the spirit and scope of the present invention should be covered within the scope of protection of the claims of the present invention.

Claims

1. A method for preparing a multi-element alloy catalyst, characterized in that, Includes the following steps: 1) A Cr adhesion layer was obtained by first magnetron sputtering on the surface of a conductive substrate using a pure Cr target as the target material; 2) FeCrNi target, Co target and Mo target are set independently, and a trace amount of nitrogen gas is introduced to perform a second magnetron sputtering on the Cr adhesion layer to obtain the support layer; 3) Based on step 2), keep the target material unchanged, increase the nitrogen gas flow rate and perform a third magnetron sputtering to obtain a Mo / N-rich layer; 4) Using the sputtered composite material as the working electrode and potassium hydroxide solution as the electrolyte, the composite material was activated by cyclic voltammetry to obtain a multi-element alloy catalyst.

2. The method for preparing a multi-element alloy catalyst according to claim 1, characterized in that, The conductive substrate is a high-purity graphite sheet or carbon paper; The carbon content of the high-purity graphite sheet is ≥99.99wt%.

3. The method for preparing a multi-element alloy catalyst according to claim 1, characterized in that, The conditions for the first magnetron sputtering are as follows: The atmosphere in the sputtering chamber is argon with a purity ≥99.999%, the argon flow rate is 70~90 sccm, and the gas pressure in the magnetron sputtering equipment chamber is 0.4~0.6 Pa; The initial temperature of the substrate is 95~105℃, and the substrate temperature is increased to 145~155℃ when sputtering reaches 1 / 3~2 / 3. The total sputtering time is 5~10 minutes, and the target power is 90~110W.

4. The method for preparing a multi-element alloy catalyst according to claim 1, characterized in that, The atomic ratio of Fe, Cr, and Ni in the FeCrNi target is 1:1:1; The purity of Co in the Co target is ≥99.95%, and the purity of Mo in the Mo target is ≥99.95%.

5. The method for preparing a multi-element alloy catalyst according to claim 1, characterized in that, The conditions for the second magnetron sputtering are as follows: The working gases are argon and nitrogen, with an argon flow rate of 70-90 sccm and a nitrogen flow rate of 5-8 sccm. The gas pressure inside the magnetron sputtering equipment cavity is 0.4-0.6 Pa. The temperature of the substrate is 95~105℃; The power of the FeCrNi target is 90~110W, the power of the Co target is 15~20W, and the power of the Mo target is 8~12W. The total sputtering time is 50~70 minutes.

6. The method for preparing a multi-element alloy catalyst according to claim 1, characterized in that, The conditions for the third magnetron sputtering are as follows: The working gases are argon and nitrogen, with an argon flow rate of 60-70 sccm and a nitrogen flow rate of 25-30 sccm. The gas pressure inside the magnetron sputtering equipment cavity is 0.4-0.6 Pa. The temperature of the substrate is 95~105℃; The power of the FeCrNi target is 70~80W, the power of the Co target is 25~30W, and the power of the Mo target is 40~45W. The total sputtering time is 30-40 minutes.

7. The method for preparing a multi-element alloy catalyst according to claim 1, characterized in that, The concentration of the potassium hydroxide solution is 1 mol / L; The activation process has a potential window of 0.2~1.6V, a scan speed of 50mV / s, and a number of revolutions of 300~500.

8. The multi-element alloy catalyst prepared by the method of any one of claims 1 to 7.

9. The application of the multi-element alloy catalyst according to claim 8 in the electrolysis of water to produce oxygen and / or hydrogen, characterized in that, Includes the following steps: The multi-element alloy catalyst serves as both the anode and cathode for electrolyzing potassium hydroxide solution.

10. The application of the multi-element alloy catalyst according to claim 9 in the electrolysis of water to produce oxygen and / or hydrogen, characterized in that, The concentration of the sodium hydroxide solution is 1 mol / L, and the temperature is 60~80℃; The current density during the electrolysis process is 500~2000 mA / cm². 2 .