A bismuth-doped nickel-cobalt spinel catalyst, its preparation method and application

By growing nickel-cobalt layered double hydroxides in situ on nickel foam and introducing Bi3+ ion exchange to form a bismuth-doped nickel-cobalt spinel catalyst, the problem of intense competition for oxygen evolution side reactions in nickel-cobalt spinel catalysts at high potentials was solved, achieving efficient oxidation of glycerol to formic acid, which has broad prospects for industrial application.

CN123108628APending Publication Date: 2026-11-17KUNMING UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611312167.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-27
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing nickel-cobalt spinel catalysts face intense competition from oxygen evolution side reactions in alkaline environments and at high potentials, leading to decreased catalyst activity and product selectivity. Furthermore, their dependence on precious metals makes large-scale commercial application difficult.

Method used

Nickel-cobalt layered double hydroxide nanosheets were grown in situ on nickel foam using an electrochemical deposition-ion exchange-calcination method. By introducing Bi3+ ions for exchange to form a bismuth-doped nickel-cobalt spinel catalyst, the crystal structure and active centers were controlled, thereby improving the activity and selectivity of glycerol oxidation.

Benefits of technology

It significantly improves the glycerol oxidation activity and formic acid selectivity of the catalyst at industrial-grade current densities, reduces energy consumption, and provides high Faradaic efficiency and high selectivity, making it suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108628A_ABST
    Figure CN123108628A_ABST
Patent Text Reader

Abstract

This invention discloses a bismuth-doped nickel-cobalt spinel catalyst, its preparation method, and its application, belonging to the field of electrochemical catalysis technology. The method of this invention involves electrodepositing a nickel-cobalt layered double hydroxide (NiCo-LDH) on a pretreated nickel foam substrate, followed by ion exchange to obtain Bi... 3+ A bismuth-doped NiCo₂O₄ catalyst was prepared by introducing a precursor and calcining it. This method is simple, controllable, and inexpensive. The prepared bismuth-doped NiCo₂O₄ catalyst has a nanosheet array structure and can efficiently electrocatalyze the oxidation of glycerol to formic acid at high current densities, exhibiting high activity, high selectivity, and high Faradaic efficiency. The current density reached 436 mA·cm⁻¹ at 1.51 V vs. RHE. ‑2 The Faraday efficiency is 82.98%. This invention solves the problems of intense competition for oxygen evolution side reactions, low activity and product selectivity in existing nickel-cobalt spinel catalysts under alkaline conditions and at higher potentials, and has broad application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of electrochemical catalysis technology, specifically to a bismuth-doped nickel-cobalt spinel catalyst, its preparation method, and its application. Background Technology

[0002] The continuous consumption of fossil fuels has created a huge market demand for renewable biodiesel, promoting the rapid development of the biodiesel industry. However, this has also led to a massive surplus of glycerol, a byproduct of biodiesel production. Typically, about 1 ton of crude glycerol is produced for every 10 tons of biodiesel produced, with global annual crude glycerol production reaching millions of tons. How to efficiently and economically transform this surplus glycerol from a "burden" into "wealth" has become one of the key bottlenecks restricting the sustainable development of the biodiesel industry. Glycerol molecules contain three hydroxyl groups, and oxidation can yield high-value-added chemicals such as glyceric acid, dihydroxyacetone, glyceraldehyde, glycolic acid, and formic acid. Among these, electrocatalytic oxidation technology, with its mild reaction conditions, clean electrical energy drive, easily precise controllable process via potential or current, and the absence of expensive or hazardous chemical oxidants, is considered a highly promising green and sustainable conversion pathway.

[0003] Existing nickel-based catalyst technologies still have significant shortcomings at industrial-grade current densities and higher potentials: on the one hand, nickel-cobalt spinel struggles to maintain stable crystal structures and active sites under strongly alkaline and high-potential environments; on the other hand, intense competition from the oxygen evolution reaction (OER) at high potentials leads to decreased current efficiency, formic acid selectivity, and Faradaic efficiency in glycerol oxidation. Furthermore, existing glycerol electro-oxidation catalysts largely rely on precious metals such as Au, Pt, and Pd, which are limited in reserves and expensive, hindering large-scale commercial application.

[0004] Therefore, developing a non-precious metal nickel-cobalt spinel-based electrocatalyst that exhibits both high activity and high formic acid selectivity at industrial-grade current densities remains a pressing technical problem to be solved in this field. Summary of the Invention

[0005] In view of the above-mentioned defects in the prior art, the purpose of this invention is to provide a bismuth-doped nickel-cobalt spinel catalyst, its preparation method, and its application, so as to solve the problem that the existing nickel-cobalt spinel catalysts suffer from intense competition from oxygen evolution side reactions in alkaline environments and at higher potentials, leading to a decrease in catalyst activity and product selectivity. Specifically, the invention includes the following steps: using pretreated nickel foam as a substrate, nickel-cobalt layered double hydroxide nanosheets, denoted as NiCo-LDH / NF, are grown in situ on the nickel foam using an electrodeposition method; subsequently, the substrate is immersed in a solution containing Bi... 3+ The mixture was stirred to obtain a bismuth-doped nickel-cobalt layered double hydroxide precursor, denoted as Bi-NiCo-LDH / NF; after calcination, a bismuth-doped nickel-cobalt spinel catalyst, denoted as Bi-NiCo2O4 / NF, was obtained.

[0006] Preferably, the pretreatment steps for nickel foam are as follows: the nickel foam is sequentially treated with acetone and 2 mol... L -1 Ultrasonic cleaning with hydrochloric acid solution for 30 minutes was performed, followed by rinsing with water after each cleaning with different solvents to prevent residual organic solvents and Cl. - .

[0007] Preferably, the electrodeposition adopts a three-electrode system, with pretreated nickel foam as the working electrode, a platinum sheet as the counter electrode, a saturated Ag / AgCl electrode as the reference electrode, and a mixed solution of nickel nitrate, cobalt nitrate, ammonium fluoride and ammonium chloride as the electrolyte.

[0008] Preferably, the concentration of nickel nitrate in the electrolyte is 0.02~0.08 mol. L -1 The concentration of cobalt nitrate is 0.04~0.16 mol. L -1 The concentration of ammonium fluoride is 0.06~0.24 mol. L -1 The concentration of ammonium chloride is 0.05~0.2 mol. L -1 .

[0009] Preferably, the electrodeposition method is a constant potential method, with a deposition voltage of -1.0 V vs. Ag / AgCl and a deposition time of 900~1800 s.

[0010] Preferably, the Bi-containing 3+ The mixed solution includes bismuth nitrate, deionized water and ethylene glycol at a mass percentage concentration of 1% to 7%, wherein the volume ratio of deionized water to ethylene glycol is 2:1.

[0011] Preferably, the stirring conditions are stirring under magnetic force for 6 to 24 hours.

[0012] Preferably, the calcination temperature is 250~350℃ and the time is 2~4h.

[0013] Another object of the present invention is to prepare a bismuth-doped nickel-cobalt spinel catalyst.

[0014] This invention employs a three-step method of electrochemical deposition-ion exchange-calcination. First, nickel-cobalt layered double hydroxide nanosheets are grown in situ on nickel foam. Then, larger Bi nanosheets are deposited through ion exchange. 3+ Introducing precursors, Bi 3+The introduction of [a specific ingredient] causes spinel lattice distortion, modulates the electronic structure of Ni and Co active centers, promotes the adsorption of glycerol molecules and the breaking of C-C bonds, thereby increasing the formation rate and selectivity of formic acid. Simultaneously, the in-situ grown nanosheet array can be directly used as an electrode without a binder, exposing more active sites and facilitating electrolyte wetting and mass transfer. The entire preparation process uses inexpensive raw materials, involves simple steps, and operates under mild and controllable conditions, making it suitable for industrial scale-up.

[0015] Another object of the present invention is the application of the bismuth-doped nickel-cobalt spinel catalyst in the electrocatalytic oxidation of glycerol.

[0016] Preferably, the initial glycerol concentration is 0.01~0.05 mol. L -1 .

[0017] Preferably, in the three-electrode system, a bismuth-doped nickel-cobalt spinel catalyst is used as the working electrode, a platinum mesh as the counter electrode, and saturated Hg / HgO as the reference electrode. The reaction vessel is an H-type electrolytic cell, and the glycerol content is no higher than 0.05 mol / L. L -1 1 mol L -1 KOH solution is the anolyte, 1 mol L -1 KOH solution is used as the cathode electrolyte, which electrocatalyzes the selective oxidation of glycerol to formic acid under high current density.

[0018] Preferably, the anolyte and the catholyte are separated by an ion exchange membrane.

[0019] Preferably, the reaction potential for the electrocatalytic oxidation of glycerol is 1.1~2.0 V vs. RHE, and the applied potential is 1.1~2.0 V vs. RHE.

[0020] Preferably, the anolyte is stirred at a speed of 300-1000 rpm during the reaction.

[0021] The catalyst prepared by this invention can achieve industrial-grade current density at low potentials, replacing the slow-kind oxygen evolution reaction with the glycerol oxidation reaction, significantly reducing anode energy consumption, while suppressing the formation of oxygen byproducts, improving formic acid yield and Faraday efficiency, and is expected to achieve energy-saving co-production by coupling with cathode hydrogen evolution.

[0022] The beneficial effects of this invention are: (1) The method for preparing bismuth-doped nickel-cobalt spinel catalyst material provided by the present invention is simple and controllable, and the raw material cost is low (only common and inexpensive salts such as nickel nitrate and cobalt nitrate are used). The catalyst obtained can be used directly as an electrode, avoiding the problem of the active material falling off in traditional coated electrodes.

[0023] (2) This invention modulates the crystal structure of nickel-cobalt spinel by bismuth doping, exposing more active sites and significantly improving the activity of the catalyst in the glycerol oxidation reaction. The catalyst exhibits high activity, high selectivity and high Faradaic efficiency in the electrocatalytic oxidation of glycerol to formic acid at industrial-grade current densities: at a working potential of 1.51 V vs. RHE, the current density reaches 436 mA·cm. -2 Faraday efficiency is 82.98%.

[0024] (3) This invention solves the problem of intense competition for oxygen evolution side reactions in existing nickel-cobalt spinel catalysts at high potentials, and has broad prospects for industrial application.

[0025] (4) In this invention, the spinel lattice distortion caused by bismuth doping is used to regulate the electronic structure of the active centers of Ni and Co to achieve high selectivity and high Faradaic efficiency in the directional conversion of glycerol into formic acid. The overall performance is better than that of catalyst samples without bismuth doping and those doped with other metals. Attached Figure Description

[0026] Figure 1 This is a schematic diagram of the synthesis of the electrocatalyst in Example 1 of the present invention.

[0027] Figure 2 The images shown are scanning electron microscope (SEM) images of the electrocatalysts of Examples 1 and 2 of the present invention. 2A is the SEM image of NiCo2O4 prepared in Example 2, and 2B is the SEM image of 3% Bi-NiCo2O4 prepared in Example 1.

[0028] Figure 3 The images show the X-ray diffraction (XRD) patterns of the electrocatalysts in Examples 1-4 of this invention. The inset on the right is a magnified view of the characteristic diffraction peaks of the (311) crystal plane.

[0029] Figure 4 The X-ray diffraction (XRD) full spectra of the electrocatalysts of Examples 1-4 of this invention are shown.

[0030] Figure 5 The electrocatalysts of Examples 1-4 of this invention were used at 1.51 V vs. RHE, containing 0.05 mol L -1 1 mol of glycerol L -1 A comparison of the performance of electrocatalytic oxidation of glycerol to formic acid in KOH electrolyte. In the figure, FA represents formic acid yield, Cov. represents glycerol conversion rate, Sel. represents formic acid selectivity, C Bal. represents carbon balance, FE represents Faraday efficiency, and GLY represents glycerol.

[0031] Figure 6The electrocatalysts of Examples 1-4 of this invention are in 1 mol L -1 KOH electrolyte (A) and containing 0.05 mol L -1 1 mol of glycerol L -1 Linear sweep voltammetry (LSV) curves in KOH electrolyte (B), where curve a represents NiCo2O4, curve b represents 1% Bi-NiCo2O4, curve c represents 3% Bi-NiCo2O4, curve d represents 5% Bi-NiCo2O4, and curve e represents 7% Bi-NiCo2O4.

[0032] Figure 7 The electrocatalysts of Examples 1-4 of this invention are in 1 mol L -1 KOH electrolyte (A) and containing 0.05 mol L -1 1 mol of glycerol L -1 Cyclic voltammetry (CV) curves in KOH electrolyte (B). Detailed Implementation

[0033] The present invention will now be described in further detail with reference to the accompanying drawings, but the scope of protection of the present invention is not limited to the contents described herein.

[0034] Example 1 A method for preparing a bismuth-doped nickel-cobalt spinel catalyst, the schematic diagram of the electrocatalyst synthesis is shown below. Figure 1 As shown, the specific steps include the following: (1) The nickel foam was ultrasonically cleaned with acetone for 30 min, washed three times with deionized water, and then rinsed with 2 mol of acetone. L -1 After ultrasonic cleaning with hydrochloric acid for 30 minutes, the nickel foam was washed three times with deionized water to obtain pretreated nickel foam.

[0035] (2) Electrodeposition was performed using a three-electrode system, with pretreated nickel foam as the working electrode and a 1×1 cm electrode. 2 A platinum sheet was used as the counter electrode, a saturated Ag / AgCl electrode as the reference electrode, and the electrolyte was 0.04 mol / L. L -1 Ni(NO3)2 6H₂O, 0.08 mol L -1 Co(NO3)2 6H₂O, 0.12 mol L -1 Ammonium fluoride and 0.1 mol L -1A mixed solution of ammonium chloride was electrodeposited for 900 s using a potentiostatic method at -1.0 V vs. Ag / AgCl. After deposition, the nickel foam was rinsed three times with deionized water to obtain in-situ grown nickel-cobalt layered double hydroxide nanosheets, denoted as NiCo-LDH / NF.

[0036] (3) NiCo-LDH / NF was placed in a 9 mL mixed solution of bismuth nitrate, ethylene glycol and deionized water (wherein, the mass percentage concentration of bismuth nitrate in the mixed solution was 3%, ethylene glycol was 3 mL and deionized water was 6 mL), and ion exchange was performed for 12 h under magnetic stirring. After the ion exchange was completed, the nickel foam was rinsed three times with ultrapure water and calcined in a muffle furnace at 300 °C for 3 h to obtain 3% Bi-NiCo2O4 / NF catalyst.

[0037] like Figure 2 As shown in B, the catalyst doped with 3% Bi exists in the form of a nanosheet array, compared to Comparative Example 1. Figure 2 Compared to A, the nanosheets in this embodiment are significantly larger in size, thicker in layer, and more densely and upright in arrangement. Surface Bi doping does not destroy the self-supporting array structure of NiCo2O4 nanosheets, but it changes the nucleation and growth behavior of the crystals. This type of vertically grown nanosheet array is beneficial for electrolyte wetting and mass transfer, exposes more surface active sites, and provides a rapid transport channel for glycerol molecules and their oxidation intermediates.

[0038] like Figure 3 As shown, the 3% Bi-NiCo2O4 / NF catalyst prepared in this embodiment exhibits diffraction peaks around 2θ of approximately 18.9°, 31.1°, 36.6°, and 44.4°, corresponding to the (111), (220), (311), and (400) crystal planes of the spinel phase NiCo2O4 (standard card PDF#97-002-4211), indicating that the prepared catalyst has a single cubic spinel structure. No diffraction peaks of Bi2O3 or other Bi-containing impurity phases were detected, indicating that Bi is introduced into the NiCo2O4 lattice in the form of doping, rather than existing as an independent oxide phase. As can be seen from the local magnified image of the characteristic peak of the (311) crystal plane on the right, with the increase of Bi doping amount, the peak position of the (311) diffraction peak shifts to the right in a regular manner, indicating that the larger radius Bi 3+ The introduction of ions caused spinel lattice distortion and changes in lattice parameters, further confirming that Bi was successfully incorporated into the NiCo2O4 lattice.

[0039] like Figure 4As shown in the figure, the catalyst prepared by Bi doping in this embodiment shows a Bi 4f characteristic signal peak at a binding energy of 159 eV, indicating the successful introduction of Bi. The C 1s peak in the figure comes from the environmental carbon adsorbed on the sample surface and the conductive carbon adhesive used for testing, and serves as an internal standard for binding energy correction.

[0040] The preparation of formic acid by the electrocatalytic oxidation of glycerol using a bismuth-doped nickel-cobalt spinel catalyst is as follows: In a three-electrode system, the reaction vessel is an H-type electrolytic cell, with the cathode and anode chambers separated by an ion-exchange membrane. The anolyte contains 10 mL of 0.05 mol / L formic acid. L -1 1 mol of glycerol L -1 The KOH mixed solution and the cathode electrolyte are 10 mL of 1 mol / L KOH solution. L -1 The actual immersion area of ​​the KOH solution with the anode inserted is 1 × 1 cm. 2 The electrocatalyst is used as the working electrode, and the actual immersion area of ​​the cathode end is 1×1 cm. 2 A platinum sheet electrode is used as the counter electrode, and the interior is filled with 1 mol L -1 Using the Hg / HgO electrode of KOH solution as a reference electrode, the electrocatalytic oxidation of glycerol to formic acid is highly selective under high current density.

[0041] Quantitative detection of the product formic acid: The product was quantitatively analyzed using liquid chromatography (equipped with an ion exchange column and an RI detector), with a mobile phase of 0.5 mmol. L -1 A dilute sulfuric acid solution, with a flow rate of 0.5 mL. min -1 The column oven temperature is 65℃.

[0042] like Figure 5 As shown, the formic acid yield using a 3% Bi-NiCo2O4 / NF catalyst was 142 mmol. L -1 It was significantly higher than that of control group 1 (110 mmol). L -1 The glycerol conversion rate, formic acid selectivity, carbon balance, and Faradaic efficiency of the present invention are the best among all embodiments, with a formic acid Faradaic efficiency of 82.98% and a formic acid selectivity of 99.9%. This indicates that the Bi-doped NiCo2O4 electrocatalyst of the present invention can electrocatalytically oxidize glycerol to formic acid with high selectivity and high Faradaic efficiency at industrial-grade current densities.

[0043] After assembling the electrolytic cell according to the above method, linear sweep voltammetry (LSV) tests were performed on all materials. The scan potential range was 1.0~1.6 V vs. RHE, and the scan rate was 5 mV·s. -1 The cathode electrolyte used in the test was 1 mol. L -1 KOH solution, anolyte containing 0.05 mol L -1 1 mol of glycerol L -1 KOH mixed solution.

[0044] like Figure 6 As shown in Figure A, it can be seen from the graph that at 1 mol L -1 In the KOH electrolyte, the catalyst prepared in this example exhibits a rapid increase in current density near 1.5 V vs. RHE, corresponding to the oxygen evolution reaction (OER) process. The anodic peak near 1.28 V corresponds to Ni. 2+ / Ni 3+ Surface oxidation. For example... Figure 6 As shown in Figure B, after the addition of glycerol, the anodic current response potential of the catalyst in this embodiment shifted significantly negatively, and the potential required to reach the same current density was greatly reduced, indicating that the electrocatalytic oxidation of glycerol is thermodynamically and kinetically preferential to the oxygen evolution reaction. Compared with other embodiments, the 3% Bi-NiCo2O4 / NF catalyst in this embodiment achieved the maximum current density at the lowest potential, exhibiting the best catalytic activity for glycerol oxidation. Figure 5 The product performance results are consistent.

[0045] like Figure 7 As shown in Figure A, it can be seen from the graph that at 1 mol L -1 The catalyst prepared in this example in KOH electrolyte exhibits a pair of redox peaks in the 1.3–1.45 V range, corresponding to the reversible redox transition of Ni / Co species on the catalyst surface. For example... Figure 7 As shown in Figure B, after the addition of glycerol, the anodic oxidation current increases significantly from about 1.13V, indicating that glycerol molecules undergo electrochemical oxidation on the catalyst surface. Among them, 3% Bi-NiCo2O4 exhibits the largest glycerol oxidation current and the lowest initial oxidation potential, further confirming its optimal intrinsic activity for the electrocatalytic oxidation of glycerol.

[0046] Example 2 The experimental steps in this embodiment are the same as those in Example 1. The difference is that the mass percentage concentration of bismuth nitrate in the mixed solution in step (3) is 1%, and the other experimental conditions are the same as those in Example 1, so that a 1% Bi-NiCo2O4 / NF catalyst is prepared.

[0047] like Figure 3 As shown in the figure, no diffraction peaks of Bi2O3 or other Bi-containing impurity phases were detected in this embodiment, indicating that Bi is introduced into the NiCo2O4 lattice in the form of doping.

[0048] like Figure 4 As shown in the figure, the catalyst prepared by Bi doping in this embodiment exhibits a Bi 4f characteristic signal peak at a binding energy of 159 eV, indicating the successful introduction of Bi.

[0049] like Figure 5 As shown in the figure, the formic acid yield for the preparation of formic acid using a 1% Bi-NiCo2O4 / NF catalyst is 129.4 mmol. L -1 The formic acid faradaic efficiency reached 78.2%, and the formic acid selectivity reached 100%.

[0050] Example 3 The experimental steps in this embodiment are the same as those in Example 1. The difference is that the mass percentage concentration of bismuth nitrate in the mixed solution in step (3) is 5%, and the other experimental conditions are the same as those in Example 1. A 5% Bi-NiCo2O4 / NF catalyst was prepared.

[0051] like Figure 3 As shown in the figure, no diffraction peaks of Bi2O3 or other Bi-containing impurity phases were detected in this embodiment, indicating that Bi is introduced into the NiCo2O4 lattice in the form of doping.

[0052] like Figure 4 As shown in the figure, the catalyst prepared by Bi doping in this embodiment exhibits a Bi 4f characteristic signal peak at a binding energy of 159 eV, indicating the successful introduction of Bi.

[0053] like Figure 5 As shown in the figure, the formic acid yield of the 5% Bi-NiCo2O4 / NF catalyst was 134.1 mmol. L -1 The formic acid Faraday efficiency reached 74.6%, and the formic acid selectivity reached 99.2%. When the Bi doping amount increased to 5%, the formic acid conversion rate decreased instead, indicating that appropriate Bi doping can optimize the electronic structure of the catalyst surface and the adsorption behavior of reactants, while excessive Bi is not conducive to the exposure of active sites.

[0054] Example 4 The experimental steps in this embodiment are the same as those in Example 1. The difference is that the mass percentage concentration of bismuth nitrate in the mixed solution in step (3) is 7%, and the other experimental conditions are the same as those in Example 1. A 7% Bi-NiCo2O4 / NF catalyst was prepared.

[0055] like Figure 3 As shown in the figure, no diffraction peaks of Bi2O3 or other Bi-containing impurity phases were detected in this embodiment, indicating that Bi was introduced into the NiCo2O4 lattice in the form of doping. As the Bi doping amount increases, the peak position of (311) diffraction peak shifts to the right in a regular manner, indicating that the larger Bi doping radius... 3+ The introduction of ions caused spinel lattice distortion and changes in lattice parameters, further confirming that Bi was successfully incorporated into the NiCo2O4 lattice.

[0056] like Figure 4 As shown in the figure, the catalyst prepared by Bi doping in this embodiment exhibits a Bi 4f characteristic signal peak at a binding energy of 159 eV, indicating the successful introduction of Bi. Furthermore, the peak intensity increases with the increase of Bi doping amount, which is consistent with the theoretical trend of doping amount change.

[0057] like Figure 5 As shown in the figure, the formic acid yield of the 7% Bi-NiCo2O4 / NF catalyst was 126.4 mmol. L -1 The formic acid faradaic efficiency reached 76.4%, and the formic acid selectivity reached 100%.

[0058] Example 5 A method for preparing a bismuth-doped nickel-cobalt spinel catalyst, and a schematic diagram of the electrocatalyst synthesis are shown below. Figure 1 As shown, the specific steps include the following: (1) The nickel foam was ultrasonically cleaned with acetone for 30 min, washed three times with deionized water, and then rinsed with 2 mol of acetone. L -1 After ultrasonic cleaning with hydrochloric acid for 30 minutes, the nickel foam was washed three times with deionized water to obtain pretreated nickel foam.

[0059] (2) Electrodeposition was performed using a three-electrode system, with pretreated nickel foam as the working electrode and a 1×1 cm electrode. 2 A platinum sheet was used as the counter electrode, a saturated Ag / AgCl electrode as the reference electrode, and the electrolyte was 0.04 mol / L. L -1 Ni(NO3)2 6H₂O, 0.08 mol L -1 Co(NO3)2 6H₂O, 0.12 mol L -1 Ammonium fluoride and 0.002 mol L -1A mixed solution of ammonium chloride was electrodeposited for 900 s using a potentiostatic method at -1.0 V vs. Ag / AgCl. After deposition, the nickel foam was rinsed three times with deionized water to obtain in-situ grown nickel-cobalt layered double hydroxide nanosheets, denoted as NiCo-LDH / NF.

[0060] (3) NiCo-LDH / NF was placed in a 9 mL mixed solution of bismuth nitrate, ethylene glycol and deionized water (wherein, the mass percentage concentration of bismuth nitrate in the mixed solution was 3%, ethylene glycol was 3 mL and deionized water was 6 mL), and ion exchange was performed for 6 h under magnetic stirring. After the ion exchange was completed, the nickel foam was rinsed three times with ultrapure water and calcined in a muffle furnace at 250 °C for 4 h to obtain the Bi-NiCo2O4 / NF catalyst.

[0061] In this example, the formic acid prepared by the Bi-NiCo2O4 / NF catalyst achieved a formic acid yield of 137.3 mmol. L -1 The formic acid faradaic efficiency reached 83%, and the formic acid selectivity reached 99.9%. The Bi-NiCo2O4 / NF catalyst exhibits excellent formic acid formation performance in the electrocatalytic oxidation of glycerol to formic acid.

[0062] Example 6 A method for preparing a bismuth-doped nickel-cobalt spinel catalyst, and a schematic diagram of the electrocatalyst synthesis are shown below. Figure 1 As shown, the specific steps include the following: (1) The nickel foam was ultrasonically cleaned with acetone for 30 min, washed three times with deionized water, and then rinsed with 2 mol of acetone. L -1 After ultrasonic cleaning with hydrochloric acid for 30 minutes, the nickel foam was washed twice with deionized water to obtain pretreated nickel foam.

[0063] (2) Electrodeposition was performed using a three-electrode system, with pretreated nickel foam as the working electrode and a 1×1 cm electrode. 2 A platinum sheet was used as the counter electrode, a saturated Ag / AgCl electrode as the reference electrode, and the electrolyte was 0.08 mol / L. L -1 Ni(NO3)2 6H₂O, 0.04 mol L -1 Co(NO3)2 6H₂O, 0.002 mol L -1 Ammonium fluoride and 0.12 mol L -1A mixed solution of ammonium chloride was electrodeposited for 1800 s using a potentiostatic method at -1.0 V vs. Ag / AgCl. After deposition, the nickel foam was rinsed three times with deionized water to obtain in-situ grown nickel-cobalt layered double hydroxide nanosheets, denoted as NiCo-LDH / NF.

[0064] (3) NiCo-LDH / NF was placed in a 9 mL mixed solution of bismuth nitrate, ethylene glycol and deionized water (wherein, the mass percentage concentration of bismuth nitrate in the mixed solution was 3%, ethylene glycol was 3 mL and deionized water was 6 mL), and ion exchange was performed for 12 h under magnetic stirring. After the ion exchange was completed, the nickel foam was rinsed three times with ultrapure water and calcined in a muffle furnace at 350 °C for 2 h to obtain the Bi-NiCo2O4 / NF catalyst.

[0065] The formic acid yield of the Bi-NiCo2O4 / NF catalyst prepared in this embodiment was 124.5 mmol. L -1 The formic acid Faradaic efficiency reached 75.2%, and the formic acid selectivity reached 99.6%. The Bi-NiCo2O4 / NF catalyst exhibited excellent formic acid formation performance in the electrocatalytic oxidation of glycerol to formic acid.

[0066] Comparative Example 1 A method for preparing a pure nickel-cobalt spinel catalyst (NiCo2O4 / NF) specifically includes the following steps: (1) The nickel foam was ultrasonically cleaned with acetone for 30 min, washed three times with deionized water, and then rinsed with 2 mol of acetone. L -1 After ultrasonic cleaning with hydrochloric acid for 30 minutes, the nickel foam was washed three times with deionized water to obtain pretreated nickel foam.

[0067] (2) Electrodeposition was performed using a three-electrode system, with pretreated nickel foam as the working electrode and a 1×1 cm electrode. 2 A platinum sheet was used as the counter electrode, a saturated Ag / AgCl electrode as the reference electrode, and the electrolyte was 0.04 mol / L. L -1 Ni(NO3)2 6H₂O, 0.08 mol L -1 Co(NO3)2 6H₂O, 0.12 mol L -1 Ammonium fluoride and 0.1 mol L -1A mixed solution of ammonium chloride was electrodeposited for 900 s using a potentiostatic method at -1.0 V vs. Ag / AgCl. After deposition, the nickel foam was rinsed three times with deionized water to obtain in-situ grown nickel-cobalt layered double hydroxide nanosheets, denoted as NiCo-LDH / NF.

[0068] (3) NiCo-LDH / NF was calcined in a muffle furnace at 300°C for 3 hours to obtain NiCo2O4 / NF catalyst.

[0069] like Figure 2 As shown in Figure A, the NiCo2O4 (A) grown in situ on a conductive substrate by electrodeposition exhibits an interwoven two-dimensional nanosheet array structure. The nanosheets grow perpendicular to the substrate, are thin with sharp edges, and form open three-dimensional through-holes between the sheets.

[0070] like Figure 4 As shown in the figure, the NiCo2O4 / NF catalyst prepared in this comparative example only shows Ni 2p, Co 2p, and O 1s signal peaks.

[0071] The formic acid yield was 109.7 mmol / L in the NiCo2O4 / NF catalyst. L -1 The formic acid faradaic efficiency reached 66.3%, and the formic acid selectivity reached 99.8%.

[0072] like Figure 2 As shown, both the prepared pure NiCo2O4 / NF and 3% Bi-NiCo2O4 / NF catalysts exhibit a two-dimensional nanosheet hierarchical structure (Figures A and B). The introduction of Bi did not significantly change the microstructure of the catalyst. This two-dimensional porous hierarchical structure retains the high conductivity framework advantage of nickel foam while providing a larger electrochemically active surface area and a shorter ion diffusion path through the nanosheets. In summary, this invention provides a bismuth-doped nickel-cobalt spinel catalyst material, its preparation method, and its application. The catalyst is synthesized in situ on a conductive support, nickel foam, using a three-step method of electrochemical deposition-ion exchange-calcination, and then used for the electrocatalytic oxidation of glycerol to formic acid. This preparation strategy is simple, the raw material cost is low, and the formic acid production performance is excellent. The catalyst exhibits both high selectivity and high conversion rate at industrial-grade current densities, confirming the feasibility of this invention in industrial applications and demonstrating broad application prospects.

[0073] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a bismuth-doped nickel-cobalt spinel catalyst, characterized in that, The process includes the following steps: using pretreated nickel foam as a substrate, in-situ growth of nickel-cobalt layered double hydroxides on the nickel foam is performed by electrodeposition, followed by immersion in a solution containing Bi. 3+ The mixture was stirred to obtain a bismuth-doped nickel-cobalt layered double hydroxide precursor, which was then calcined to obtain a bismuth-doped nickel-cobalt spinel catalyst.

2. The method for preparing the bismuth-doped nickel-cobalt spinel catalyst according to claim 1, characterized in that: The pretreatment steps for the nickel foam are as follows: the nickel foam is ultrasonically cleaned with acetone and hydrochloric acid respectively, and washed with water after cleaning with different solvents.

3. The method for preparing the bismuth-doped nickel-cobalt spinel catalyst according to claim 1, characterized in that: The electrodeposition method employs a three-electrode system, with pretreated nickel foam as the working electrode, a platinum sheet as the counter electrode, a saturated Ag / AgCl electrode as the reference electrode, and a mixed solution of nickel nitrate, cobalt nitrate, ammonium fluoride, and ammonium chloride as the electrolyte.

4. The method for preparing the bismuth-doped nickel-cobalt spinel catalyst according to claim 3, characterized in that: The concentration of nickel nitrate in the electrolyte is 0.02~0.08 mol. L -1 The concentration of cobalt nitrate is 0.04~0.16 mol. L -1 The concentration of ammonium fluoride is 0.06~0.24 mol. L -1 The concentration of ammonium chloride is 0.05~0.2 mol. L -1 .

5. The method for preparing the bismuth-doped nickel-cobalt spinel catalyst according to claim 1, characterized in that: The electrodeposition method is a constant potential method, with a deposition voltage of -1.0 V vs. Ag / AgCl and a deposition time of 900~1800s.

6. The method for preparing the bismuth-doped nickel-cobalt spinel catalyst according to claim 1, characterized in that: The Bi-containing 3 + The mixed solution includes bismuth nitrate, water, and ethylene glycol at a mass percentage concentration of 1% to 7%, wherein the volume ratio of water to ethylene glycol is 2:

1.

7. The method for preparing the bismuth-doped nickel-cobalt spinel catalyst according to claim 1, characterized in that: The stirring time is 6~24h; the calcination temperature is 250~350℃, and the time is 2~4h.

8. The bismuth-doped nickel-cobalt spinel catalyst is prepared by the method according to any one of claims 1 to 7.

9. The application of the bismuth-doped nickel-cobalt spinel catalyst according to claim 8 in the electrocatalytic oxidation of glycerol.

10. The application according to claim 9, characterized in that: In the three-electrode system, a bismuth-doped nickel-cobalt spinel catalyst was used as the working electrode, a platinum mesh as the counter electrode, and saturated Hg / HgO as the reference electrode, with a glycerol content not exceeding 0.05 mol / L. L -1 The KOH solution is used as the anolyte and the KOH solution is used as the catholyte to electrocatalyze the oxidation of glycerol to formic acid.