Catalyst and Preparation Method
By constructing a nitrogen-doped porous carbon-nitrogen single-atom catalyst with an M-N3 coordination structure, the structural degradation problem of Ni-NC catalyst under high current density and long-term electrolysis conditions was solved, the selectivity and stability of CO2 electroreduction to CO were improved, and efficient CO2 resource conversion was achieved.
Patent Information
- Application Number
- CN202611441063.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-16
- Publication Date
- 2026-11-17
AI Technical Summary
Existing Ni-NC single-atom catalysts are prone to structural degradation under ultra-high current density and long-term electrolysis conditions, leading to the dissolution of metal active atoms, breakage of coordination bonds, and aggregation of active sites, which affects the efficiency of CO2 electroreduction to CO.
A nitrogen-doped porous carbon-nitrogen single-atom catalyst with an M-N3 coordination structure enhances the adsorption and activation capacity of CO2 and inhibits the competitive hydrogen evolution reaction by constructing a low-coordination, unsaturated M–N3 configuration, thereby improving the selectivity and activity of CO2 electroreduction to CO.
Under high current density and long-term electrolysis conditions, the structural stability and CO selectivity of the catalyst are maintained, the efficiency of CO2 electroreduction to CO is improved, and efficient CO2 resource conversion is achieved.
Smart Images

Figure CN123108630A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the fields of electrocatalytic carbon dioxide resource conversion and preparation of single-atom catalytic materials, and more specifically, to catalysts and their preparation methods. Background Technology
[0002] Green aviation kerosene (green jet fuel) boasts significant advantages such as low carbon emissions, direct compatibility with existing aviation fuel supply systems, and no need for modifications to aircraft engines. Currently, utilizing renewable electricity to drive the electroreduction of CO2 to produce high-purity CO is a key pre-processing technology for synthesizing green jet fuel. Ni-NC single-atom catalysts, with their advantages of being free of precious metals and exhibiting high CO selectivity, have become the mainstream catalytic system in the field of CO2 electroreduction to CO production. However, existing Ni-NC single-atom catalysts, once applied to industrial production, require the necessary 200-500 mA / cm² / g ... 2 The harsh operating conditions of ultra-high current density and continuous electrolysis for thousands of hours can lead to a series of structural degradation problems, such as the dissolution and loss of active metal atoms, the breaking and reconstruction of metal-heteroatom coordination bonds, the aggregation and deactivation of active sites, and the oxidation and collapse of the carbon substrate.
[0003] In view of this, the present invention is proposed. Summary of the Invention
[0004] The purpose of this invention is to provide a catalyst and a method for its preparation.
[0005] This invention is implemented as follows: In a first aspect, the present invention provides a catalyst comprising a nitrogen-doped porous carbon-nitrogen single-atom material having an M-N3 coordination structure, wherein M is selected from at least one of Ni, Co and Fe elements.
[0006] In an optional embodiment, the mass fraction of element M in the catalyst is 0.1-10 wt%.
[0007] Secondly, the present invention provides a method for preparing the catalyst described in the foregoing embodiments, comprising: A solution containing an M salt, a zinc salt, and a ligand is reacted to generate a ZIF precursor; the ligand includes 2-methylimidazole and cyanuric acid. The ZIF precursor was calcined to obtain the catalyst.
[0008] In an optional embodiment, both the M salt and the zinc salt are acetates; And / or, the molar ratio of zinc to M in the catalyst is (5-20):1; And / or, the ratio of the amount of 2-methylimidazole to the total amount of M and zinc is (6-10):1; And / or, the molar ratio of the 2-methylimidazole to cyanuric acid is (8-10):1.
[0009] In an optional embodiment, the reaction temperature is 15-30°C and the reaction time is 24-36 hours. And / or, it also includes solid-liquid separation and washing of the product obtained from the reaction to obtain the ZIF precursor.
[0010] In an optional embodiment, the calcination includes a first-stage calcination and a second-stage calcination, wherein the temperature of the first-stage calcination is 400-600℃ and the temperature of the second-stage calcination is 800-1000℃.
[0011] In an optional embodiment, the calcination time is 1-3 hours; And / or, the heating rate corresponding to the calcination stage is 2-5℃ / min; And / or, the calcination time for the two stages is 1-3 hours; And / or, the heating rate corresponding to the two-stage calcination is 5-10℃ / min.
[0012] In an optional embodiment, the process further includes refining: the calcined product is sequentially subjected to acid washing and reflux, water washing, and drying to obtain the refined catalyst.
[0013] In an optional embodiment, the washing solution used for the pickling reflux is a sulfuric acid solution with a molar concentration of 0.5 to 4 mol / L; And / or, the pickling reflux temperature is 50-70°C, and the time is 10-14 hours.
[0014] Thirdly, the present invention provides the application of a catalyst in the electrocatalytic reduction of carbon dioxide to carbon monoxide.
[0015] The present invention has the following beneficial effects: This application constructs a low-coordinate, unsaturated M–N3 configuration, breaking the electronic saturation state of traditional symmetrical coordination, thereby regulating the d-band center position and charge distribution of the nickel center, enhancing its adsorption and activation ability for CO2 molecules, and inhibiting the competitive hydrogen evolution reaction (HER) pathway, thus improving the selectivity and activity of CO2 electroreduction to CO. Attached Figure Description
[0016] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly introduced below. It should be understood that the following drawings only show some embodiments of the present invention and should not be regarded as a limitation on the scope. For those skilled in the art, other related drawings can be obtained based on these drawings without creative effort.
[0017] Figure 1 The CO Faradaic efficiency is the CO reduction to carbon monoxide catalyzed by the catalyst in Example 1. Detailed Implementation
[0018] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments whose manufacturers are not specified are all conventional products that can be purchased commercially.
[0019] This invention provides a catalyst comprising a nitrogen-doped porous carbon-nitrogen single-atom material having an M-N3 coordination structure, wherein M is selected from at least one of Ni, Co, and Fe elements.
[0020] This application constructs a low-coordinate, unsaturated M–N3 configuration, breaking the electronic saturation state of traditional symmetrical coordination, thereby regulating the d-band center position and charge distribution of the nickel center, enhancing its adsorption and activation ability for CO2 molecules, and inhibiting the competitive hydrogen evolution reaction (HER) pathway, thus improving the selectivity and activity of CO2 electroreduction to CO.
[0021] It should be noted that the coordination vacancy (i.e., "V") formed by the absence of a nitrogen ligand in the M–N3 coordination makes the M atom exhibit higher Lewis acidity, better stability of the COOH intermediate, and lower CO desorption energy barrier. These three factors together constitute the structural basis for achieving high CO selectivity and stable operation at high current density.
[0022] In an optional embodiment, the mass fraction of element M in the catalyst is 0.1-10 wt%; this is beneficial for achieving a balance between the high dispersion of M single atoms in the carbon matrix and structural stability.
[0023] This invention also provides a method for preparing the catalyst described in the foregoing embodiments, comprising: A solution containing an M salt, a zinc salt, and a ligand is reacted to generate a ZIF precursor; the ligand includes 2-methylimidazole and cyanuric acid. The ZIF precursor was calcined to obtain the catalyst.
[0024] This application achieves in-situ, homogeneous doping of M atoms in the ZIF lattice through one-step co-crystallization of M salt and zinc salt in a 2-methylimidazole / cyanuric acid mixed ligand system, avoiding uneven dispersion or bond weakening caused by post-processing. Cyanuric acid introduces an additional nitrogen source and structural perturbation, synergistically regulating crystal defect density and nitrogen coordination configuration, providing a precursor structure basis for the formation of vacancy-rich M–N3 sites after pyrolysis. The subsequent gradient calcination process relies on the preferential volatilization of zinc and carbon framework rearrangement to spontaneously construct a nitrogen defect microenvironment anchoring M single atoms under conditions without external templates or etchants, thereby obtaining the catalyst.
[0025] In an optional embodiment, both the M salt and the zinc salt are acetates; compared to nitrates or chlorides, using acetates avoids the release of NO during the pyrolysis process. x Toxic waste gases are eliminated, thus removing the risks associated with the storage and use of easily explosive hazardous chemicals. Meanwhile, acetate is a weak ligand and a low-corrosive anion, which dissolves uniformly and reacts mildly in the methanol system. This is conducive to the atomic-level co-doping of metal ions during ZIF crystallization, reducing the damage to the MOF crystal structure and subsequent single-atom anchoring points caused by halogen residues or strong oxidizing byproducts.
[0026] In an optional embodiment, the molar ratio of zinc to M in the catalyst is (5-20):1, with a high zinc ratio resulting in Zn² + The dominant ZIF lattice construction, M as a trace heterometal is forced to be confined to lattice defects, edges or surface adsorption sites, and cannot form an independent M coordination phase; this heterogeneous doping is conducive to inducing the generation of M-rich vacancy precursors.
[0027] In an optional embodiment, the ratio of the amount of 2-methylimidazole to the total amount of M and zinc is (6-10):1; this is beneficial for Zn / M to form structurally complete but edge-defect-rich ZIF microcrystals under the dominant coordination of 2-methylimidazole, providing a suitable precursor for the generation of high-density M–N3 vacancy sites after pyrolysis.
[0028] In an optional embodiment, the molar ratio of 2-methylimidazole to cyanuric acid is (8-10):1. Cyanuric acid is introduced as a co-ligand, and through its rigid planar triazine ring structure and strong hydrogen bonding ability, it works synergistically with 2-methylimidazole to modulate the growth direction and interlayer stacking of ZIF crystals, inducing the generation of directional nitrogen vacancies and micro-strain lattices. This ratio range ensures that cyanuric acid effectively participates in the construction of the coordination network without dominating nucleation, thereby directionally enriching the key nitrogen-coordination unsaturated environment required for the Ni–N3 configuration in the carbon matrix after pyrolysis.
[0029] In an optional embodiment, the reaction temperature is 15-30℃ and the reaction time is 24-36h. The room temperature crystallization condition avoids the risk of metal hydrolysis or ligand decomposition caused by high temperature, and ensures the stable existence of the acetate system in methanol. This reaction time is conducive to the full progress of the metal-ligand coordination reaction, and avoids excessive aging that leads to abnormal grain growth or phase separation, thereby obtaining a ZIF precursor with uniform particle size and controllable defect distribution, which prepares for the precise anchoring of nickel atoms to nitrogen vacancies in subsequent pyrolysis.
[0030] In an optional embodiment, the product obtained from the reaction is further subjected to solid-liquid separation and washing to obtain the ZIF precursor. The purpose of this step is to remove unreacted free metal salts, excess ligands, and by-product acetic acid, and to prevent impurities from interfering with the carbonization process, clogging pores, or inducing nickel agglomeration during the pyrolysis stage.
[0031] In an optional embodiment, the calcination includes a first-stage calcination and a second-stage calcination. The first-stage calcination temperature is 400-600℃, and the second-stage calcination temperature is 800-1000℃. The first-stage calcination mainly removes the template agent, volatilizes small molecules, and performs preliminary carbonization, while retaining the rudimentary nitrogen-doped framework. The second-stage calcination promotes the graphitization and reconstruction of the carbon framework, enhances the thermal stability of the Ni–N bonds, and drives zinc volatilization to form vacancies, synergistically constructing a Ni–N3-rich coordination environment. The two-stage calcination helps avoid the violent migration and aggregation of M atoms caused by a single high-temperature step.
[0032] In an optional embodiment, the calcination time is 1-3 hours; In an optional embodiment, the heating rate corresponding to the first stage of calcination is 2-5℃ / min; slow heating and moderate heat preservation are conducive to the gradual decomposition of organic components and avoid the sudden collapse of the MOF framework caused by local exothermic shocks; at the same time, it provides time for the phased volatilization of zinc and the initial migration of M atoms to nitrogen defect sites, so that nickel can complete the initial anchoring when the carbon framework has just taken shape, laying the foundation for the formation of a stable M-N3 configuration in the subsequent high-temperature stage.
[0033] In an optional embodiment, the second-stage calcination time is 1-3 hours; In an optional embodiment, the heating rate corresponding to the two-stage calcination is 5-10℃ / min. The faster heating rate combined with high-temperature calcination promotes deep graphitization and pore ordering of the carbon matrix, enhancing conductivity and mass transfer capacity; at the same time, it accelerates the complete volatilization of zinc and the rearrangement of the carbon-nitrogen framework, driving the M atoms to finally locate in the three-coordinate nitrogen vacancy, completing the thermodynamically stable construction of the M–N3 active center, and avoiding M aggregation caused by excessively long holding time.
[0034] In an optional embodiment, the process further includes purification: the calcined product is sequentially subjected to acid washing and reflux, water washing, and drying to obtain the purified catalyst. Acid washing selectively dissolves uncoordinated metallic zinc, zinc oxide, and M clusters, among other inactive impurities, while retaining chemically bonded M–N3 single atoms; reflux improves mass transfer efficiency and ensures that the acid fully penetrates the porous carbon; water washing thoroughly removes residual acid and soluble salts, preventing side reactions or ion interference in subsequent electrocatalysis and ensuring the purity of the catalyst's intrinsic activity expression.
[0035] In an optional embodiment, the washing solution used for the pickling reflux is a sulfuric acid solution with a molar concentration of 0.5 to 4 mol / L; In an optional embodiment, the pickling reflux temperature is 50-70°C and the time is 10-14 hours.
[0036] Within this parameter range, it is beneficial to ensure the selective dissolution of zinc while avoiding excessive etching of the carbon skeleton by strong acids or damage to M–N coordination bonds.
[0037] The present invention also provides an application of a catalyst in the electrocatalytic reduction of carbon dioxide to carbon monoxide.
[0038] The features and performance of the present invention will be further described in detail below with reference to embodiments.
[0039] Example 1 This embodiment provides a nitrogen-doped porous carbon-nitrogen single-atom catalyst with an M-N3 coordination structure, and its preparation method is as follows: S1: Preparation of Ni@ZIF; S101: Weigh 2.94g of zinc acetate dihydrate and 0.33g of nickel acetate tetrahydrate, dissolve the two drugs in 100mL of anhydrous methanol, and stir at 800r / min for 30min at room temperature until completely dissolved, so that the molar ratio of zinc to nickel is 10:1. S102: Weigh 7.25g of 2-methylimidazole and 1.27g of cyanuric acid and dissolve them in 100mL of anhydrous methanol. Stir at 800r / min for 30min at room temperature until completely dissolved, so that the molar ratio of 2-methylimidazole to cyanuric acid is 9:1 and the molar ratio of 2-methylimidazole to total metals is 6:1. S103: The ligand solution prepared in S102 was quickly poured into the metal salt solution in S101, the flask was sealed, and the mixture was stirred at 800 r / min at room temperature for 30 h. After crystallization, the mixture was taken out and centrifuged at 9000 r / min. After washing three times with anhydrous methanol, it was dried in a vacuum drying oven at 60 ℃ for 12 h to obtain Ni@ZIF white powder. S2: Ni@ZIF temperature-programmed gradient pyrolysis to produce a nitrogen-doped porous carbon and nitrogen single-atom catalyst with an M-N3 coordination structure: S201: 1.00g of Ni@ZIF white powder was transferred to a tube furnace for calcination. During the calcination process, the flow rate of N2 was 100mL / min. The temperature was first increased to 600℃ at a heating rate of 5℃ / min and calcined for 1h, and then increased to 800℃ at a heating rate of 10℃ / min and calcined for 1h. The mixture was then allowed to cool naturally to room temperature, and the resulting black solid product was collected. S202: The solid product obtained from S201 is added to 50 ml of 0.5 mol / L H2SO4 solution, mixed evenly, and then placed in an oil bath. It is refluxed and washed at 60 °C for 12 h to fully dissolve uncoordinated elemental zinc, agglomerated metal particles and other impurities. The mixture is washed with deionized water and filtered until the filtrate is neutral. It is then vacuum dried at 60 °C for 12 h to obtain the Ni-N3-rich coordinated single-atom catalyst, denoted as Ni-N3 catalyst.
[0040] Catalyst Application Electrode preparation: Weigh 5 mg of Ni-N3 catalyst and 1 mg of conductive carbon black, and disperse them in a mixed solvent of 1 mL anhydrous ethanol and 50 μL of 5 wt% Nafion solution; place the mixed solvent in an ultrasonic cleaner and ultrasonically disperse in an ice-water bath for 30 min to obtain a uniform, stable, and non-agglomerated catalytic ink; uniformly spray the catalytic ink onto the surface of hydrophobic carbon paper using a spraying method, controlling the catalyst loading to be 1 mg·cm³. -2 After spraying, dry at room temperature.
[0041] Electrochemical performance testing of CO2RR was conducted. The electrochemical tests were performed on a Shanghai Chenhua CHI760E electrochemical workstation using a three-chamber GDE flow electrolyzer. The electrolyte used was a 0.5 mol / L KHCO3 solution. High-purity CO2 was continuously purged for 30 min before testing at a CO2 inlet flow rate of 20 sccm, and the electrolyte was circulated at a constant temperature of 25℃. All potentials were uniformly converted to a reversible hydrogen electrode (vs. RHE). Electrolysis was performed continuously for 2 hours under constant potential (0.8V vs. RHE) and constant current density (300mA / cm²), with exhaust gas collected every 10 minutes using online gas chromatography to calculate the CO and H₂ Faradaic efficiencies. To simulate industrial conditions, electrolysis was further performed continuously for 100 hours at a constant current density of 300mA / cm², with products automatically sampled and detected every 10 minutes using online gas chromatography to calculate the CO Faradaic efficiency in real time. The obtained long-term stability data are shown in […]. Figure 1 .
[0042] Example 2 This embodiment provides a nitrogen-doped porous carbon-nitrogen single-atom catalyst with an M-N3 coordination structure, and its preparation method is as follows: S1: Preparation of Ni@ZIF; S101: Weigh 2.35g zinc acetate dihydrate and 0.33g nickel acetate tetrahydrate, dissolve the two drugs in 100mL anhydrous methanol, stir at 800r / min for 30min at room temperature until completely dissolved, so that the molar ratio of zinc to nickel is 8:1. S102: Weigh 5.81g of 2-methylimidazole and 1.02g of cyanuric acid and dissolve them in 100mL of anhydrous methanol. Stir at 800r / min for 30min at room temperature until completely dissolved, so that the molar ratio of 2-methylimidazole to cyanuric acid is 9:1 and the molar ratio of 2-methylimidazole to total metals is 6:1. S103: The ligand solution prepared in S102 was quickly poured into the metal salt solution in S101, the flask was sealed, and the mixture was stirred at 800 r / min at room temperature for 30 h. After crystallization, the mixture was taken out and centrifuged at 9000 r / min. After washing three times with anhydrous methanol, it was dried in a vacuum drying oven at 60 ℃ for 12 h to obtain Ni@ZIF white powder. S2: Ni@ZIF temperature-programmed gradient pyrolysis was used to prepare Ni-N3-rich coordinated single-atom catalysts. S201: 1.00g of Ni@ZIF white powder was transferred to a tube furnace for calcination. During the calcination process, the flow rate of N2 was 100mL / min. The temperature was first increased to 600℃ at a heating rate of 5℃ / min and calcined for 1h, and then increased to 800℃ at a heating rate of 10℃ / min and calcined for 1h. The mixture was then allowed to cool naturally to room temperature, and the resulting black solid product was collected. S202: The solid product obtained from S201 is added to 50 ml of 0.5 mol / L H2SO4 solution, mixed evenly, and then placed in an oil bath. It is refluxed and washed at 60 °C for 12 h to fully dissolve uncoordinated elemental zinc, agglomerated metal particles and other impurities. The mixture is washed with deionized water and filtered until the filtrate is neutral. It is then vacuum dried at 60 °C for 12 h to obtain the Ni-N3-rich coordinated single-atom catalyst, denoted as Ni-N3 catalyst.
[0043] Catalyst Application Electrode preparation: Weigh 5 mg of Ni-N3 catalyst and 1 mg of conductive carbon black, and disperse them in a mixed solvent of 1 mL anhydrous ethanol and 50 μL of 5 wt% Nafion solution; place the mixed solvent in an ultrasonic cleaner and ultrasonically disperse in an ice-water bath for 30 min to obtain a uniform, stable, and non-agglomerated catalytic ink; uniformly spray the catalytic ink onto the surface of hydrophobic carbon paper using a spraying method, controlling the catalyst loading to be 1 mg·cm³. - ², After spraying, dry at room temperature.
[0044] Electrochemical performance testing of CO2RR was conducted. The electrochemical tests were performed on a Shanghai Chenhua CHI760E electrochemical workstation using a three-chamber GDE flow electrolyzer. The electrolyte used was a 0.5 mol / L KHCO3 solution. High-purity CO2 was continuously purged for 30 min before testing at a CO2 inlet flow rate of 20 sccm, and the electrolyte was circulated at a constant temperature of 25℃. All potentials were uniformly converted to a reversible hydrogen electrode (vs. RHE). Electrolysis was performed continuously for 2 hours under constant potential (0.8V vs. RHE) and constant current density (300mA / cm²). The tail gas was collected every 10 minutes by online gas chromatography, and the Faraday efficiency of CO and H2 was calculated.
[0045] Example 3 This embodiment provides a nitrogen-doped porous carbon-nitrogen single-atom catalyst with an M-N3 coordination structure, and its preparation method is as follows: S1: Preparation of Ni@ZIF; S101: Weigh 2.94g of zinc acetate dihydrate and 0.55g of nickel acetate tetrahydrate, dissolve the two drugs in 100mL of anhydrous methanol, and stir at 800r / min for 30min at room temperature until completely dissolved, so that the molar ratio of zinc to nickel is 6:1. S102: Weigh 7.69g of 2-methylimidazole and 1.35g of cyanuric acid and dissolve them in 100mL of anhydrous methanol. Stir at 800r / min for 30min at room temperature until completely dissolved, so that the molar ratio of 2-methylimidazole to cyanuric acid is 9:1 and the molar ratio of 2-methylimidazole to total metals is 6:1. S103: The ligand solution prepared in S102 was quickly poured into the metal salt solution in S101, the flask was sealed, and the mixture was stirred at 800 r / min at room temperature for 30 h. After crystallization, the mixture was taken out and centrifuged at 9000 r / min. After washing three times with anhydrous methanol, it was dried in a vacuum drying oven at 60 ℃ for 12 h to obtain Ni@ZIF white powder. S2: Ni@ZIF temperature-programmed gradient pyrolysis to produce a nitrogen-doped porous carbon and nitrogen single-atom catalyst with an M-N3 coordination structure: S201: 1.00g of Ni@ZIF white powder was transferred to a tube furnace for calcination. During the calcination process, the flow rate of N2 was 100mL / min. The temperature was first increased to 600℃ at a heating rate of 5℃ / min and calcined for 1h, and then increased to 800℃ at a heating rate of 10℃ / min and calcined for 1h. The mixture was then allowed to cool naturally to room temperature, and the resulting black solid product was collected. S202: The solid product obtained from S201 is added to 50 ml of 0.5 mol / L H2SO4 solution, mixed evenly, and then placed in an oil bath. It is refluxed and washed at 60 °C for 12 h to fully dissolve uncoordinated elemental zinc, agglomerated metal particles and other impurities. The mixture is washed with deionized water and filtered until the filtrate is neutral. It is then vacuum dried at 60 °C for 12 h to obtain the Ni-N3-rich coordinated single-atom catalyst, denoted as Ni-N3 catalyst.
[0046] Catalyst Application Electrode preparation: Weigh 5 mg of Ni-N3 catalyst and 1 mg of conductive carbon black, and disperse them in a mixed solvent of 1 mL anhydrous ethanol and 50 μL of 5 wt% Nafion solution; place the mixed solvent in an ultrasonic cleaner and ultrasonically disperse in an ice-water bath for 30 min to obtain a uniform, stable, and non-agglomerated catalytic ink; uniformly spray the catalytic ink onto the surface of hydrophobic carbon paper using a spraying method, controlling the catalyst loading to be 1 mg·cm³. -2 After spraying, dry at room temperature.
[0047] Electrochemical performance testing of CO2RR was conducted. The electrochemical tests were performed on a Shanghai Chenhua CHI760E electrochemical workstation using a three-chamber GDE flow electrolyzer. The electrolyte used was a 0.5 mol / L KHCO3 solution. High-purity CO2 was continuously purged for 30 min before testing at a CO2 inlet flow rate of 20 sccm, and the electrolyte was circulated at a constant temperature of 25℃. All potentials were uniformly converted to a reversible hydrogen electrode (vs. RHE). Electrolysis was performed continuously for 2 hours under constant potential (0.8V vs. RHE) and constant current density (300mA / cm²). The tail gas was collected every 10 minutes by online gas chromatography, and the Faraday efficiency of CO and H2 was calculated.
[0048] Example 4 This embodiment provides a nitrogen-doped porous carbon-nitrogen single-atom catalyst with an M-N3 coordination structure, and its preparation method is as follows: S1: Preparation of Ni@ZIF; S101: Weigh 2.94g of zinc acetate dihydrate and 0.33g of nickel acetate tetrahydrate, dissolve the two drugs in 100mL of anhydrous methanol, and stir at 800r / min for 30min at room temperature until completely dissolved, so that the molar ratio of zinc to nickel is 10:1. S102: Weigh 9.67g of 2-methylimidazole and 1.69g of cyanuric acid and dissolve them in 100mL of anhydrous methanol. Stir at 800r / min for 30min at room temperature until completely dissolved, so that the molar ratio of 2-methylimidazole to cyanuric acid is 9:1 and the molar ratio of 2-methylimidazole to total metals is 8:1. S103: The ligand solution prepared in S102 was quickly poured into the metal salt solution in S101, the flask was sealed, and the mixture was stirred at 800 r / min at room temperature for 30 h. After crystallization, the mixture was taken out and centrifuged at 9000 r / min. After washing three times with anhydrous methanol, it was dried in a vacuum drying oven at 60 ℃ for 12 h to obtain Ni@ZIF white powder. S2: Ni@ZIF temperature-programmed gradient pyrolysis to produce a nitrogen-doped porous carbon and nitrogen single-atom catalyst with an M-N3 coordination structure: S201: 1.00g of Ni@ZIF white powder was transferred to a tube furnace for calcination. During the calcination process, the flow rate of N2 was 100mL / min. The temperature was first increased to 600℃ at a heating rate of 5℃ / min and calcined for 1h, and then increased to 800℃ at a heating rate of 10℃ / min and calcined for 1h. The mixture was then allowed to cool naturally to room temperature, and the resulting black solid product was collected. S202: The solid product obtained from S201 is added to 50 ml of 0.5 mol / L H2SO4 solution, mixed evenly, and then placed in an oil bath. It is refluxed and washed at 60 °C for 12 h to fully dissolve uncoordinated elemental zinc, agglomerated metal particles and other impurities. The mixture is washed with deionized water and filtered until the filtrate is neutral. It is then vacuum dried at 60 °C for 12 h to obtain the Ni-N3-rich coordinated single-atom catalyst, denoted as Ni-N3 catalyst.
[0049] Catalyst Application Electrode preparation: Weigh 5 mg of Ni-N3 catalyst and 1 mg of conductive carbon black, and disperse them in a mixed solvent of 1 mL anhydrous ethanol and 50 μL of 5 wt% Nafion solution; place the mixed solvent in an ultrasonic cleaner and ultrasonically disperse in an ice-water bath for 30 min to obtain a uniform, stable, and non-agglomerated catalytic ink; uniformly spray the catalytic ink onto the surface of hydrophobic carbon paper using a spraying method, controlling the catalyst loading to be 1 mg·cm³. - ², After spraying, dry at room temperature.
[0050] Electrochemical performance testing of CO2RR was conducted. The electrochemical tests were performed on a Shanghai Chenhua CHI760E electrochemical workstation using a three-chamber GDE flow electrolyzer. The electrolyte used was a 0.5 mol / L KHCO3 solution. High-purity CO2 was continuously purged for 30 min before testing at a CO2 inlet flow rate of 20 sccm, and the electrolyte was circulated at a constant temperature of 25℃. All potentials were uniformly converted to a reversible hydrogen electrode (vs. RHE). Electrolysis was performed continuously for 2 hours under constant potential (0.8V vs. RHE) and constant current density (300mA / cm²). The tail gas was collected every 10 minutes by online gas chromatography, and the Faraday efficiency of CO and H2 was calculated.
[0051] Example 5 This embodiment provides a nitrogen-doped porous carbon-nitrogen single-atom catalyst with an M-N3 coordination structure, and its preparation method is as follows: S1: Preparation of Ni@ZIF; S101: Weigh 2.94g of zinc acetate dihydrate and 0.33g of nickel acetate tetrahydrate, dissolve the two drugs in 100mL of anhydrous methanol, and stir at 800r / min for 30min at room temperature until completely dissolved, so that the molar ratio of zinc to nickel is 10:1. S102: Weigh 12.08g of 2-methylimidazole and 2.12g of cyanuric acid and dissolve them in 100mL of anhydrous methanol. Stir at 800r / min for 30min at room temperature until completely dissolved, so that the molar ratio of 2-methylimidazole to cyanuric acid is 9:1 and the molar ratio of 2-methylimidazole to total metals is 10:1. S103: The ligand solution prepared in S102 was quickly poured into the metal salt solution in S101, the flask was sealed, and the mixture was stirred at 800 r / min at room temperature for 30 h. After crystallization, the mixture was taken out and centrifuged at 9000 r / min. After washing three times with anhydrous methanol, it was dried in a vacuum drying oven at 60 ℃ for 12 h to obtain Ni@ZIF white powder. S2: Ni@ZIF temperature-programmed gradient pyrolysis to produce a nitrogen-doped porous carbon and nitrogen single-atom catalyst with an M-N3 coordination structure: S201: 1.00g of Ni@ZIF white powder was transferred to a tube furnace for calcination. During the calcination process, the flow rate of N2 was 100mL / min. The temperature was first increased to 600℃ at a heating rate of 5℃ / min and calcined for 1h, and then increased to 800℃ at a heating rate of 10℃ / min and calcined for 1h. The mixture was then allowed to cool naturally to room temperature, and the resulting black solid product was collected. S202: The solid product obtained from S201 is added to 50 ml of 0.5 mol / L H2SO4 solution, mixed evenly, and then placed in an oil bath. It is refluxed and washed at 60 °C for 12 h to fully dissolve uncoordinated elemental zinc, agglomerated metal particles and other impurities. The mixture is washed with deionized water and filtered until the filtrate is neutral. It is then vacuum dried at 60 °C for 12 h to obtain the Ni-N3-rich coordinated single-atom catalyst, denoted as Ni-N3 catalyst.
[0052] Catalyst Application Electrode preparation: Weigh 5 mg of Ni-N3 catalyst and 1 mg of conductive carbon black, and disperse them in a mixed solvent of 1 mL anhydrous ethanol and 50 μL of 5 wt% Nafion solution; place the mixed solvent in an ultrasonic cleaner and ultrasonically disperse in an ice-water bath for 30 min to obtain a uniform, stable, and non-agglomerated catalytic ink; uniformly spray the catalytic ink onto the surface of hydrophobic carbon paper using a spraying method, controlling the catalyst loading to be 1 mg·cm³. - ², After spraying, dry at room temperature.
[0053] Electrochemical performance testing of CO2RR was conducted. The electrochemical tests were performed on a Shanghai Chenhua CHI760E electrochemical workstation using a three-chamber GDE flow electrolyzer. The electrolyte used was a 0.5 mol / L KHCO3 solution. High-purity CO2 was continuously purged for 30 min before testing at a CO2 inlet flow rate of 20 sccm, and the electrolyte was circulated at a constant temperature of 25℃. All potentials were uniformly converted to a reversible hydrogen electrode (vs. RHE). Electrolysis was performed continuously for 2 hours under constant potential (0.8V vs. RHE) and constant current density (300mA / cm²), with tail gas collected every 10 minutes by online gas chromatography. The CO Faraday efficiency was calculated.
[0054] Example 6 This embodiment provides a nitrogen-doped porous carbon-nitrogen single-atom catalyst with an M-N3 coordination structure, and its preparation method is as follows: S1: Preparation of Ni@ZIF; S101: Weigh 2.94g of zinc acetate dihydrate and 0.33g of nickel acetate tetrahydrate, dissolve the two drugs in 100mL of anhydrous methanol, and stir at 800r / min for 30min at room temperature until completely dissolved, so that the molar ratio of zinc to nickel is 10:1. S102: Weigh 7.25g of 2-methylimidazole and 1.27g of cyanuric acid and dissolve them in 100mL of anhydrous methanol. Stir at 800r / min for 30min at room temperature until completely dissolved, so that the molar ratio of 2-methylimidazole to cyanuric acid is 9:1 and the molar ratio of 2-methylimidazole to total metals is 6:1. S103: The ligand solution prepared in S102 was quickly poured into the metal salt solution in S101, the flask was sealed, and the mixture was stirred at 800 r / min at room temperature for 24 h. After crystallization, the mixture was taken out and centrifuged at 9000 r / min. After washing with anhydrous methanol three times, the mixture was dried in a vacuum drying oven at 60 ℃ for 12 h to obtain Ni@ZIF white powder. S2: Ni@ZIF temperature-programmed gradient pyrolysis to produce a nitrogen-doped porous carbon and nitrogen single-atom catalyst with an M-N3 coordination structure: S201: 1.00g of Ni@ZIF white powder was transferred to a tube furnace for calcination. During the calcination process, the flow rate of N2 was 100mL / min. The temperature was first increased to 600℃ at a heating rate of 5℃ / min and calcined for 1h, and then increased to 800℃ at a heating rate of 10℃ / min and calcined for 1h. The mixture was then allowed to cool naturally to room temperature, and the resulting black solid product was collected. S202: The solid product obtained from S201 is added to 50 ml of 0.5 mol / L H2SO4 solution, mixed evenly, and then placed in an oil bath. It is refluxed and washed at 60 °C for 12 h to fully dissolve uncoordinated elemental zinc, agglomerated metal particles and other impurities. The mixture is washed with deionized water and filtered until the filtrate is neutral. It is then vacuum dried at 60 °C for 12 h to obtain the Ni-N3-rich coordinated single-atom catalyst, denoted as Ni-N3 catalyst.
[0055] Catalyst Application Electrode preparation: Weigh 5 mg of Ni-N3 catalyst and 1 mg of conductive carbon black, and disperse them in a mixed solvent of 1 mL anhydrous ethanol and 50 μL of 5 wt% Nafion solution; place the mixed solvent in an ultrasonic cleaner and ultrasonically disperse in an ice-water bath for 30 min to obtain a uniform, stable, and non-agglomerated catalytic ink; uniformly spray the catalytic ink onto the surface of hydrophobic carbon paper using a spraying method, controlling the catalyst loading to be 1 mg·cm³. - ², After spraying, dry at room temperature.
[0056] Electrochemical performance testing of CO2RR was conducted. The electrochemical tests were performed on a Shanghai Chenhua CHI760E electrochemical workstation using a three-chamber GDE flow electrolyzer. The electrolyte used was a 0.5 mol / L KHCO3 solution. High-purity CO2 was continuously purged for 30 min before testing at a CO2 inlet flow rate of 20 sccm, and the electrolyte was circulated at a constant temperature of 25℃. All potentials were uniformly converted to a reversible hydrogen electrode (vs. RHE). Electrolysis was performed continuously for 2 hours under constant potential (0.8V vs. RHE) and constant current density (300mA / cm²). The tail gas was collected every 10 minutes by online gas chromatography, and the Faraday efficiency of CO and H2 was calculated.
[0057] Example 7 This embodiment provides a nitrogen-doped porous carbon-nitrogen single-atom catalyst with an M-N3 coordination structure, and its preparation method is as follows: S1: Preparation of Ni@ZIF; S101: Weigh 2.94g of zinc acetate dihydrate and 0.33g of nickel acetate tetrahydrate, dissolve the two drugs in 100mL of anhydrous methanol, and stir at 800r / min for 30min at room temperature until completely dissolved, so that the molar ratio of zinc to nickel is 10:1. S102: Weigh 7.25g of 2-methylimidazole and 1.27g of cyanuric acid and dissolve them in 100mL of anhydrous methanol. Stir at 800r / min for 30min at room temperature until completely dissolved, so that the molar ratio of 2-methylimidazole to cyanuric acid is 9:1 and the molar ratio of 2-methylimidazole to total metals is 6:1. S103: The ligand solution prepared in S102 was quickly poured into the metal salt solution in S101, the flask was sealed, and the mixture was stirred at 800 r / min at room temperature for 36 h. After crystallization, the mixture was taken out and centrifuged at 9000 r / min. After washing with anhydrous methanol three times, the mixture was dried in a vacuum drying oven at 60 ℃ for 12 h to obtain Ni@ZIF white powder. S2: Ni@ZIF temperature-programmed gradient pyrolysis to produce a nitrogen-doped porous carbon and nitrogen single-atom catalyst with an M-N3 coordination structure: S201: 1.00g of Ni@ZIF white powder was transferred to a tube furnace for calcination. During the calcination process, the flow rate of N2 was 100mL / min. The temperature was first increased to 600℃ at a heating rate of 5℃ / min and calcined for 1h, and then increased to 800℃ at a heating rate of 10℃ / min and calcined for 1h. The mixture was then allowed to cool naturally to room temperature, and the resulting black solid product was collected. S202: The solid product obtained from S201 is added to 50 ml of 0.5 mol / L H2SO4 solution, mixed evenly, and then placed in an oil bath. It is refluxed and washed at 60 °C for 12 h to fully dissolve uncoordinated elemental zinc, agglomerated metal particles and other impurities. The mixture is washed with deionized water and filtered until the filtrate is neutral. It is then vacuum dried at 60 °C for 12 h to obtain the Ni-N3-rich coordinated single-atom catalyst, denoted as Ni-N3 catalyst.
[0058] Catalyst Application Electrode preparation: Weigh 5 mg of Ni-N3 catalyst and 1 mg of conductive carbon black, and disperse them in a mixed solvent of 1 mL anhydrous ethanol and 50 μL of 5 wt% Nafion solution; place the mixed solvent in an ultrasonic cleaner and ultrasonically disperse in an ice-water bath for 30 min to obtain a uniform, stable, and non-agglomerated catalytic ink; uniformly spray the catalytic ink onto the surface of hydrophobic carbon paper using a spraying method, controlling the catalyst loading to be 1 mg·cm³. - ², After spraying, dry at room temperature.
[0059] Electrochemical performance testing of CO2RR was conducted. The electrochemical tests were performed on a Shanghai Chenhua CHI760E electrochemical workstation using a three-chamber GDE flow electrolyzer. The electrolyte used was a 0.5 mol / L KHCO3 solution. High-purity CO2 was continuously purged for 30 min before testing at a CO2 inlet flow rate of 20 sccm, and the electrolyte was circulated at a constant temperature of 25℃. All potentials were uniformly converted to a reversible hydrogen electrode (vs. RHE). Electrolysis was performed continuously for 2 hours under constant potential (0.8V vs. RHE) and constant current density (300mA / cm²). The tail gas was collected every 10 minutes by online gas chromatography, and the Faraday efficiency of CO and H2 was calculated.
[0060] Example 8 This embodiment provides a nitrogen-doped porous carbon-nitrogen single-atom catalyst with an M-N3 coordination structure, and its preparation method is as follows: S1: Preparation of Ni@ZIF; S101: Weigh 2.94g of zinc acetate dihydrate and 0.33g of nickel acetate tetrahydrate, dissolve the two drugs in 100mL of anhydrous methanol, and stir at 800r / min for 30min at room temperature until completely dissolved, so that the molar ratio of zinc to nickel is 10:1. S102: Weigh 7.25g of 2-methylimidazole and 1.27g of cyanuric acid and dissolve them in 100mL of anhydrous methanol. Stir at 800r / min for 30min at room temperature until completely dissolved, so that the molar ratio of 2-methylimidazole to cyanuric acid is 9:1 and the molar ratio of 2-methylimidazole to total metals is 6:1. S103: The ligand solution prepared in S102 was quickly poured into the metal salt solution in S101, the flask was sealed, and the mixture was stirred at 800 r / min at room temperature for 30 h. After crystallization, the mixture was taken out and centrifuged at 9000 r / min. After washing three times with anhydrous methanol, it was dried in a vacuum drying oven at 60 ℃ for 12 h to obtain Ni@ZIF white powder. S2: Ni@ZIF temperature-programmed gradient pyrolysis to produce a nitrogen-doped porous carbon and nitrogen single-atom catalyst with an M-N3 coordination structure: S201: 1.00g of Ni@ZIF white powder was transferred to a tube furnace for calcination. During the calcination process, the flow rate of N2 was 100mL / min. The temperature was first increased to 600℃ at a heating rate of 5℃ / min and calcined for 1h, and then increased to 900℃ at a heating rate of 10℃ / min and calcined for 1h. The mixture was then allowed to cool naturally to room temperature, and the resulting black solid product was collected. S202: The solid product obtained from S201 is added to 50 ml of 0.5 mol / L H2SO4 solution, mixed evenly, and then placed in an oil bath. It is refluxed and washed at 60 °C for 12 h to fully dissolve uncoordinated elemental zinc, agglomerated metal particles and other impurities. The mixture is washed with deionized water and filtered until the filtrate is neutral. It is then vacuum dried at 60 °C for 12 h to obtain the Ni-N3-rich coordinated single-atom catalyst, denoted as Ni-N3 catalyst.
[0061] Catalyst Application Electrode preparation: Weigh 5 mg of Ni-N3 catalyst and 1 mg of conductive carbon black, and disperse them in a mixed solvent of 1 mL anhydrous ethanol and 50 μL of 5 wt% Nafion solution; place the mixed solvent in an ultrasonic cleaner and ultrasonically disperse in an ice-water bath for 30 min to obtain a uniform, stable, and non-agglomerated catalytic ink; uniformly spray the catalytic ink onto the surface of hydrophobic carbon paper using a spraying method, controlling the catalyst loading to be 1 mg·cm³. - ², After spraying, dry at room temperature.
[0062] Electrochemical performance testing of CO2RR was conducted. The electrochemical tests were performed on a Shanghai Chenhua CHI760E electrochemical workstation using a three-chamber GDE flow electrolyzer. The electrolyte used was a 0.5 mol / L KHCO3 solution. High-purity CO2 was continuously purged for 30 min before testing at a CO2 inlet flow rate of 20 sccm, and the electrolyte was circulated at a constant temperature of 25℃. All potentials were uniformly converted to a reversible hydrogen electrode (vs. RHE). Electrolysis was performed continuously for 2 hours under constant potential (0.8V vs. RHE) and constant current density (300mA / cm²). The tail gas was collected every 10 minutes by online gas chromatography, and the Faraday efficiency of CO and H2 was calculated.
[0063] Example 9 This embodiment provides a nitrogen-doped porous carbon-nitrogen single-atom catalyst with an M-N3 coordination structure, and its preparation method is as follows: S1: Preparation of Ni@ZIF; S101: Weigh 2.94g of zinc acetate dihydrate and 0.33g of nickel acetate tetrahydrate, dissolve the two drugs in 100mL of anhydrous methanol, and stir at 800r / min for 30min at room temperature until completely dissolved, so that the molar ratio of zinc to nickel is 10:1. S102: Weigh 7.25g of 2-methylimidazole and 1.27g of cyanuric acid and dissolve them in 100mL of anhydrous methanol. Stir at 800r / min for 30min at room temperature until completely dissolved, so that the molar ratio of 2-methylimidazole to cyanuric acid is 9:1 and the molar ratio of 2-methylimidazole to total metals is 6:1. S103: The ligand solution prepared in S102 was quickly poured into the metal salt solution in S101, the flask was sealed, and the mixture was stirred at 800 r / min at room temperature for 30 h. After crystallization, the mixture was taken out and centrifuged at 9000 r / min. After washing three times with anhydrous methanol, it was dried in a vacuum drying oven at 60 ℃ for 12 h to obtain Ni@ZIF white powder. S2: Ni@ZIF temperature-programmed gradient pyrolysis to produce a nitrogen-doped porous carbon and nitrogen single-atom catalyst with an M-N3 coordination structure: S201: 1.00g of Ni@ZIF white powder was transferred to a tube furnace for calcination. During the calcination process, the flow rate of N2 was 100mL / min. The temperature was first increased to 600℃ at a heating rate of 5℃ / min and calcined for 1h, and then increased to 800℃ at a heating rate of 10℃ / min and calcined for 2h. The product was then naturally cooled to room temperature and the resulting black solid product was collected. S202: The solid product obtained from S201 is added to 50 ml of 0.5 mol / L H2SO4 solution, mixed evenly, and then placed in an oil bath. It is refluxed and washed at 60 °C for 12 h to fully dissolve uncoordinated elemental zinc, agglomerated metal particles and other impurities. The mixture is washed with deionized water and filtered until the filtrate is neutral. It is then vacuum dried at 60 °C for 12 h to obtain the Ni-N3-rich coordinated single-atom catalyst, denoted as Ni-N3 catalyst.
[0064] Catalyst Application Electrode preparation: Weigh 5 mg of Ni-N3 catalyst and 1 mg of conductive carbon black, and disperse them in a mixed solvent of 1 mL anhydrous ethanol and 50 μL of 5 wt% Nafion solution; place the mixed solvent in an ultrasonic cleaner and ultrasonically disperse in an ice-water bath for 30 min to obtain a uniform, stable, and non-agglomerated catalytic ink; uniformly spray the catalytic ink onto the surface of hydrophobic carbon paper using a spraying method, controlling the catalyst loading to be 1 mg·cm³. - ², After spraying, dry at room temperature.
[0065] Electrochemical performance testing of CO2RR was conducted. The electrochemical tests were performed on a Shanghai Chenhua CHI760E electrochemical workstation using a three-chamber GDE flow electrolyzer. The electrolyte used was a 0.5 mol / L KHCO3 solution. High-purity CO2 was continuously purged for 30 min before testing at a CO2 inlet flow rate of 20 sccm, and the electrolyte was circulated at a constant temperature of 25℃. All potentials were uniformly converted to a reversible hydrogen electrode (vs. RHE). Electrolysis was performed continuously for 2 hours under constant potential (0.8V vs. RHE) and constant current density (300mA / cm²). The tail gas was collected every 10 minutes by online gas chromatography, and the Faraday efficiency of CO and H2 was calculated.
[0066] Example 10 This embodiment provides a nitrogen-doped porous carbon-nitrogen single-atom catalyst with an M-N3 coordination structure, and its preparation method is as follows: S1: Preparation of Ni@ZIF; S101: Weigh 2.94g of zinc acetate dihydrate and 0.33g of nickel acetate tetrahydrate, dissolve the two drugs in 100mL of anhydrous methanol, and stir at 800r / min for 30min at room temperature until completely dissolved, so that the molar ratio of zinc to nickel is 10:1. S102: Weigh 7.25g of 2-methylimidazole and 1.27g of cyanuric acid and dissolve them in 100mL of anhydrous methanol. Stir at 800r / min for 30min at room temperature until completely dissolved, so that the molar ratio of 2-methylimidazole to cyanuric acid is 9:1 and the molar ratio of 2-methylimidazole to total metals is 6:1. S103: The ligand solution prepared in S102 was quickly poured into the metal salt solution in S101, the flask was sealed, and the mixture was stirred at 800 r / min at room temperature for 30 h. After crystallization, the mixture was taken out and centrifuged at 9000 r / min. After washing three times with anhydrous methanol, it was dried in a vacuum drying oven at 60 ℃ for 12 h to obtain Ni@ZIF white powder. S2: Ni@ZIF temperature-programmed gradient pyrolysis to produce a nitrogen-doped porous carbon and nitrogen single-atom catalyst with an M-N3 coordination structure: S201: 1.00g of Ni@ZIF white powder was transferred to a tube furnace for calcination. During the calcination process, the flow rate of N2 was 100mL / min. The temperature was first increased to 500℃ at a heating rate of 5℃ / min and calcined for 1h, and then increased to 800℃ at a heating rate of 10℃ / min and calcined for 1h. The product was then naturally cooled to room temperature and the resulting black solid product was collected. S202: The solid product obtained from S201 is added to 50 ml of 0.5 mol / L H2SO4 solution, mixed evenly, and then placed in an oil bath. It is refluxed and washed at 60 °C for 12 h to fully dissolve uncoordinated elemental zinc, agglomerated metal particles and other impurities. The mixture is washed with deionized water and filtered until the filtrate is neutral. It is then vacuum dried at 60 °C for 12 h to obtain the Ni-N3-rich coordinated single-atom catalyst, denoted as Ni-N3 catalyst.
[0067] Catalyst Application Electrode preparation: Weigh 5 mg of Ni-N3 catalyst and 1 mg of conductive carbon black, and disperse them in a mixed solvent of 1 mL anhydrous ethanol and 50 μL of 5 wt% Nafion solution; place the mixed solvent in an ultrasonic cleaner and ultrasonically disperse in an ice-water bath for 30 min to obtain a uniform, stable, and non-agglomerated catalytic ink; uniformly spray the catalytic ink onto the surface of hydrophobic carbon paper using a spraying method, controlling the catalyst loading to be 1 mg·cm³. - ², After spraying, dry at room temperature.
[0068] Electrochemical performance testing of CO2RR was conducted. The electrochemical tests were performed on a Shanghai Chenhua CHI760E electrochemical workstation using a three-chamber GDE flow electrolyzer. The electrolyte used was a 0.5 mol / L KHCO3 solution. High-purity CO2 was continuously purged for 30 min before testing at a CO2 inlet flow rate of 20 sccm, and the electrolyte was circulated at a constant temperature of 25℃. All potentials were uniformly converted to a reversible hydrogen electrode (vs. RHE). Electrolysis was performed continuously for 2 hours under constant potential (0.8V vs. RHE) and constant current density (300mA / cm²). The tail gas was collected every 10 minutes by online gas chromatography, and the Faraday efficiency of CO and H2 was calculated.
[0069] Example 11 This embodiment provides a nitrogen-doped porous carbon-nitrogen single-atom catalyst with an M-N3 coordination structure, and its preparation method is as follows: S1: Preparation of Ni@ZIF; S101: Weigh 2.94g of zinc acetate dihydrate and 0.33g of nickel acetate tetrahydrate, dissolve the two drugs in 100mL of anhydrous methanol, and stir at 800r / min for 30min at room temperature until completely dissolved, so that the molar ratio of zinc to nickel is 10:1. S102: Weigh 7.25g of 2-methylimidazole and 1.27g of cyanuric acid and dissolve them in 100mL of anhydrous methanol. Stir at 800r / min for 30min at room temperature until completely dissolved, so that the molar ratio of 2-methylimidazole to cyanuric acid is 9:1 and the molar ratio of 2-methylimidazole to total metals is 6:1. S103: The ligand solution prepared in S102 was quickly poured into the metal salt solution in S101, the flask was sealed, and the mixture was stirred at 800 r / min at room temperature for 30 h. After crystallization, the mixture was taken out and centrifuged at 9000 r / min. After washing three times with anhydrous methanol, it was dried in a vacuum drying oven at 60 ℃ for 12 h to obtain Ni@ZIF white powder. S2: Ni@ZIF temperature-programmed gradient pyrolysis to produce a nitrogen-doped porous carbon and nitrogen single-atom catalyst with an M-N3 coordination structure: S201: 1.00g of Ni@ZIF white powder was transferred to a tube furnace for calcination. During the calcination process, the flow rate of N2 was 100mL / min. The temperature was first increased to 600℃ at a rate of 5℃ / min and calcined for 3h. Then the temperature was increased to 800℃ at a rate of 10℃ / min and calcined for 1h. The product was then naturally cooled to room temperature and the resulting black solid product was collected. S202: The solid product obtained from S201 is added to 50 ml of 0.5 mol / L H2SO4 solution, mixed evenly, and then placed in an oil bath. It is refluxed and washed at 60 °C for 12 h to fully dissolve uncoordinated elemental zinc, agglomerated metal particles and other impurities. The mixture is washed with deionized water and filtered until the filtrate is neutral. It is then vacuum dried at 60 °C for 12 h to obtain the Ni-N3-rich coordinated single-atom catalyst, denoted as Ni-N3 catalyst.
[0070] Catalyst Application Electrode preparation: Weigh 5 mg of Ni-N3 catalyst and 1 mg of conductive carbon black, and disperse them in a mixed solvent of 1 mL anhydrous ethanol and 50 μL of 5 wt% Nafion solution; place the mixed solvent in an ultrasonic cleaner and ultrasonically disperse in an ice-water bath for 30 min to obtain a uniform, stable, and non-agglomerated catalytic ink; uniformly spray the catalytic ink onto the surface of hydrophobic carbon paper using a spraying method, controlling the catalyst loading to be 1 mg·cm³. - ², After spraying, dry at room temperature.
[0071] Electrochemical performance testing of CO2RR was conducted. The electrochemical tests were performed on a Shanghai Chenhua CHI760E electrochemical workstation using a three-chamber GDE flow electrolyzer. The electrolyte used was a 0.5 mol / L KHCO3 solution. High-purity CO2 was continuously purged for 30 min before testing at a CO2 inlet flow rate of 20 sccm, and the electrolyte was circulated at a constant temperature of 25℃. All potentials were uniformly converted to a reversible hydrogen electrode (vs. RHE). Electrolysis was performed continuously for 2 hours under constant potential (0.8V vs. RHE) and constant current density (300mA / cm²). The tail gas was collected every 10 minutes by online gas chromatography, and the Faraday efficiency of CO and H2 was calculated.
[0072] Example 12 This embodiment provides a nitrogen-doped porous carbon-nitrogen single-atom catalyst with an M-N3 coordination structure, and its preparation method is as follows: S1: Preparation of Ni@ZIF; S101: Weigh 2.94g of zinc acetate dihydrate and 0.33g of nickel acetate tetrahydrate, dissolve the two drugs in 100mL of anhydrous methanol, and stir at 800r / min for 30min at room temperature until completely dissolved, so that the molar ratio of zinc to nickel is 10:1. S102: Weigh 7.25g of 2-methylimidazole and 1.27g of cyanuric acid and dissolve them in 100mL of anhydrous methanol. Stir at 800r / min for 30min at room temperature until completely dissolved, so that the molar ratio of 2-methylimidazole to cyanuric acid is 9:1 and the molar ratio of 2-methylimidazole to total metals is 6:1. S103: The ligand solution prepared in S102 was quickly poured into the metal salt solution in S101, the flask was sealed, and the mixture was stirred at 800 r / min at room temperature for 30 h. After crystallization, the mixture was taken out and centrifuged at 9000 r / min. After washing three times with anhydrous methanol, it was dried in a vacuum drying oven at 60 ℃ for 12 h to obtain Ni@ZIF white powder. S2: Ni@ZIF temperature-programmed gradient pyrolysis to produce a nitrogen-doped porous carbon and nitrogen single-atom catalyst with an M-N3 coordination structure: S201: 1.00g of Ni@ZIF white powder was transferred to a tube furnace for calcination. During the calcination process, the flow rate of N2 was 100mL / min. The temperature was first increased to 500℃ at a heating rate of 5℃ / min and calcined for 1h. Then the temperature was increased to 800℃ at a heating rate of 10℃ / min and calcined for 3h. The product was then naturally cooled to room temperature and the resulting black solid product was collected. S202: The solid product obtained from S201 is added to 50 ml of 0.5 mol / L H2SO4 solution, mixed evenly, and then placed in an oil bath. It is refluxed and washed at 60 °C for 12 h to fully dissolve uncoordinated elemental zinc, agglomerated metal particles and other impurities. The mixture is washed with deionized water and filtered until the filtrate is neutral. It is then vacuum dried at 60 °C for 12 h to obtain the Ni-N3-rich coordinated single-atom catalyst, denoted as Ni-N3 catalyst.
[0073] Catalyst Application Electrode preparation: Weigh 5 mg of Ni-N3 catalyst and 1 mg of conductive carbon black, and disperse them in a mixed solvent of 1 mL anhydrous ethanol and 50 μL of 5 wt% Nafion solution; place the mixed solvent in an ultrasonic cleaner and ultrasonically disperse in an ice-water bath for 30 min to obtain a uniform, stable, and non-agglomerated catalytic ink; uniformly spray the catalytic ink onto the surface of hydrophobic carbon paper using a spraying method, controlling the catalyst loading to be 1 mg·cm³. - ², After spraying, dry at room temperature.
[0074] Electrochemical performance testing of CO2RR was conducted. The electrochemical tests were performed on a Shanghai Chenhua CHI760E electrochemical workstation using a three-chamber GDE flow electrolyzer. The electrolyte used was a 0.5 mol / L KHCO3 solution. High-purity CO2 was continuously purged for 30 min before testing at a CO2 inlet flow rate of 20 sccm, and the electrolyte was circulated at a constant temperature of 25℃. All potentials were uniformly converted to a reversible hydrogen electrode (vs. RHE). Electrolysis was performed continuously for 2 hours under constant potential (0.8V vs. RHE) and constant current density (300mA / cm²), with tail gas collected every 10 minutes by online gas chromatography. The CO Faraday efficiency was calculated.
[0075] Example 13 This embodiment provides a nitrogen-doped porous carbon-nitrogen single-atom catalyst with an M-N3 coordination structure, and its preparation method is as follows: S1: Preparation of Ni@ZIF; S101: Weigh 2.94g of zinc acetate dihydrate and 0.33g of nickel acetate tetrahydrate, dissolve the two drugs in 100mL of anhydrous methanol, and stir at 800r / min for 30min at room temperature until completely dissolved, so that the molar ratio of zinc to nickel is 10:1. S102: Weigh 7.25g of 2-methylimidazole and 1.27g of cyanuric acid and dissolve them in 100mL of anhydrous methanol. Stir at 800r / min for 30min at room temperature until completely dissolved, so that the molar ratio of 2-methylimidazole to cyanuric acid is 9:1 and the molar ratio of 2-methylimidazole to total metals is 6:1. S103: The ligand solution prepared in S102 was quickly poured into the metal salt solution in S101, the flask was sealed, and the mixture was stirred at 800 r / min at room temperature for 30 h. After crystallization, the mixture was taken out and centrifuged at 9000 r / min. After washing three times with anhydrous methanol, it was dried in a vacuum drying oven at 60 ℃ for 12 h to obtain Ni@ZIF white powder. S2: Ni@ZIF temperature-programmed gradient pyrolysis to produce a nitrogen-doped porous carbon and nitrogen single-atom catalyst with an M-N3 coordination structure: S201: 1.00g of Ni@ZIF white powder was transferred to a tube furnace for calcination. During the calcination process, the flow rate of N2 was 100mL / min. The temperature was first increased to 300℃ at a heating rate of 5℃ / min and calcined for 1h, and then increased to 1000℃ at a heating rate of 10℃ / min and calcined for 3h. The product was then naturally cooled to room temperature and the resulting black solid product was collected. S202: The solid product obtained from S201 is added to 50 ml of 0.5 mol / L H2SO4 solution, mixed evenly, and then placed in an oil bath. It is refluxed and washed at 60 °C for 12 h to fully dissolve uncoordinated elemental zinc, agglomerated metal particles and other impurities. The mixture is washed with deionized water and filtered until the filtrate is neutral. It is then vacuum dried at 60 °C for 12 h to obtain the Ni-N3-rich coordinated single-atom catalyst, denoted as Ni-N3 catalyst.
[0076] Catalyst Application Electrode preparation: Weigh 5 mg of Ni-N3 catalyst and 1 mg of conductive carbon black, and disperse them in a mixed solvent of 1 mL anhydrous ethanol and 50 μL of 5 wt% Nafion solution; place the mixed solvent in an ultrasonic cleaner and ultrasonically disperse in an ice-water bath for 30 min to obtain a uniform, stable, and non-agglomerated catalytic ink; uniformly spray the catalytic ink onto the surface of hydrophobic carbon paper using a spraying method, controlling the catalyst loading to be 1 mg·cm³. - ², After spraying, dry at room temperature.
[0077] Electrochemical performance testing of CO2RR was conducted. The electrochemical tests were performed on a Shanghai Chenhua CHI760E electrochemical workstation using a three-chamber GDE flow electrolyzer. The electrolyte used was a 0.5 mol / L KHCO3 solution. High-purity CO2 was continuously purged for 30 min before testing at a CO2 inlet flow rate of 20 sccm, and the electrolyte was circulated at a constant temperature of 25℃. All potentials were uniformly converted to a reversible hydrogen electrode (vs. RHE). Electrolysis was performed continuously for 2 hours under constant potential (0.8V vs. RHE) and constant current density (300mA / cm²), with tail gas collected every 10 minutes by online gas chromatography. The CO Faraday efficiency was calculated.
[0078] Example 14 The only difference between this embodiment and Example 1 is that in step S101, zinc acetate dihydrate and nickel acetate tetrahydrate are replaced with zinc nitrate and nickel nitrate in equal amounts of metallic substances. The remaining steps are the same. The molar ratio of metallic nickel to metallic zinc is 1:10, the molar ratio of 2-methylimidazole to cyanuric acid is 9:1, and the molar ratio of 2-methylimidazole to total metals is 6:1. Similarly, in... Electrolysis was performed continuously for 2 hours under constant potential (0.8V vs. RHE) and constant current density (300mA / cm²). The tail gas was collected every 10 minutes by online gas chromatography, and the CO Faraday efficiency was calculated.
[0079] Example 15 The only difference between this embodiment and Embodiment 1 is that in step S101, nickel acetate tetrahydrate is replaced with an equal amount of cobalt acetate; the remaining steps are the same. The molar ratio of cobalt to zinc is 1:10, the molar ratio of 2-methylimidazole to cyanuric acid is 9:1, and the molar ratio of 2-methylimidazole to total metals is 6:1. Similarly, in... Electrolysis was performed continuously for 2 hours under constant potential (0.8V vs. RHE) and constant current density (300mA / cm²), with tail gas collected every 10 minutes by online gas chromatography. The CO Faraday efficiency was calculated.
[0080] Example 16 The only difference between this embodiment and Example 1 is that in step S102, only 2-methylimidazole is used as the ligand, and the resulting catalyst is a Ni-N4 catalyst; the remaining steps are the same. The molar ratio of nickel to zinc is 1:10, and the molar ratio of 2-methylimidazole to total metals is 6:1. Similarly, in... Electrolysis was performed continuously for 2 hours under constant potential (0.8V vs. RHE) and constant current density (300mA / cm²), with tail gas collected every 10 minutes by online gas chromatography. The CO Faraday efficiency was calculated.
[0081] Comparative Example 1 The only difference between this comparative example and Example 1 is that the ligand selected in step S102 is 2-ethylimidazole, the molar ratio of nickel to zinc is 1:10, the molar ratio of 2-ethylimidazole to cyanuric acid is 9:1, and the molar ratio of 2-ethylimidazole to total metals is 6:1. The resulting catalyst precursor is named Ni@ZIF-14. The remaining steps are the same. Similarly, in... Electrolysis was performed continuously for 2 hours under constant potential (0.8V vs. RHE) and constant current density (300mA / cm²). The tail gas was collected every 10 minutes by online gas chromatography, and the CO Faraday efficiency was calculated.
[0082] Comparative Example 2 The only difference between this comparative example and Example 1 is that in step S2, the programmed pyrolysis only involves the first stage of pyrolysis. During calcination, the N2 flow rate is 100 mL / min, and the temperature is increased to 600°C at a rate of 5°C / min for calcination for 1 hour. After natural cooling to room temperature, the resulting solid product is collected. The remaining steps are the same. Electrolysis was performed continuously for 2 hours under constant potential (0.8V vs. RHE) and constant current density (300mA / cm²), with tail gas collected every 10 minutes by online gas chromatography. The CO Faraday efficiency was calculated.
[0083] Results Analysis High-purity argon (Ar) was used as an internal standard gas to analyze the products by gas chromatography. The volume concentrations (ppm) of CO and H2 in the tail gas were determined by the internal standard method. The molar formation rate of the products was calculated based on the total CO2 inlet flow rate, and the CO Faradaic efficiency was finally calculated. The catalyst reactivity results are shown in Table 1. Specifically, the specific parameter changes and corresponding CO and H2 Faradaic efficiencies of Examples 1-16 and Comparative Examples 1-2 are shown in Table 1. The long-term stability of continuous electrolysis for 100 h in Example 1 is shown in Table 1. Figure 1 .
[0084] Table 1
[0085] The results from the above embodiments show that the Ni-N3-site single-atom catalyst prepared from an acetate precursor based on a MOF template, as provided by this invention, achieves a CO Faradaic efficiency of up to 95% in the electroreduction of CO from CO2, while significantly reducing the H2 Faradaic efficiency to 4%. In this invention, the CO and H2 Faradaic efficiencies of the catalyst can be adjusted by modifying the metal molar ratio, the metal-to-ligand molar ratio, the crystallization reaction time, and the calcination time and temperature during catalyst calcination. Figure 1 As can be seen, at 300mA / cm 2 After 100 hours of continuous electrolysis at a constant current density, the catalyst achieved an initial CO Faradaic efficiency of 94%, which remained above 80% after 100 hours. The cathode potential fluctuated little during the test, and the catalyst exhibited excellent catalytic selectivity and electrochemical stability.
[0086] In summary, this application has the following beneficial effects: (1) The catalyst of this application has no risk of storage or use of easily explosive hazardous chemicals, the synthesis process is simple, and it is suitable for large-scale industrial production.
[0087] (2) The catalyst prepared by this method can significantly improve the CO2RR catalytic activity of carbon-supported nickel single-atom materials, reduce the CO2 activation energy barrier, and suppress hydrogen evolution side reactions.
[0088] (3) The catalyst prepared by this method has high selectivity and partial current density for carbon monoxide, which can meet the requirements of large-scale conversion of CO2RR to carbon monoxide.
[0089] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A catalyst, characterized in that, This includes nitrogen-doped porous carbon-nitrogen single-atom materials with an M-N3 coordination structure, wherein M is selected from at least one of Ni, Co, and Fe.
2. The catalyst according to claim 1, characterized in that, The mass fraction of element M in the catalyst is 0.1-10 wt%.
3. A method for preparing the catalyst according to claim 1, characterized in that, include: A solution containing M salt, zinc salt and ligand is reacted to generate ZIF precursor; The ligand comprises 2-methylimidazolium and cyanuric acid; The ZIF precursor was calcined to obtain the catalyst.
4. The method for preparing the catalyst according to claim 3, characterized in that, Both the M salt and the zinc salt are acetates; And / or, the molar ratio of zinc to M in the catalyst is (5-20):1; And / or, the ratio of the amount of 2-methylimidazole to the total amount of M and zinc is (6-10):1; And / or, the molar ratio of the 2-methylimidazole to cyanuric acid is (8-10):
1.
5. The method for preparing the catalyst according to claim 3, characterized in that, The reaction temperature is 15-30℃, and the reaction time is 24-36h; And / or, it also includes solid-liquid separation and washing of the product obtained from the reaction to obtain the ZIF precursor.
6. The method for preparing the catalyst according to claim 3, characterized in that, The calcination includes a first-stage calcination and a second-stage calcination. The temperature of the first-stage calcination is 400-600℃, and the temperature of the second-stage calcination is 800-1000℃.
7. The method for preparing the catalyst according to claim 3, characterized in that, The calcination time for the first stage is 1-3 hours; And / or, the heating rate corresponding to the calcination stage is 2-5℃ / min; And / or, the calcination time for the two stages is 1-3 hours; And / or, the heating rate corresponding to the two-stage calcination is 5-10℃ / min.
8. The method for preparing the catalyst according to claim 3, characterized in that, It also includes refining: the calcined product is sequentially subjected to acid washing and reflux, water washing and drying to obtain the refined catalyst.
9. The method for preparing the catalyst according to claim 3, characterized in that, The washing solution used for the acid pickling reflux is a sulfuric acid solution with a molar concentration of 0.5–4 mol / L; And / or, the pickling reflux temperature is 50-70°C, and the time is 10-14 hours.
10. Application of a catalyst in the electrocatalytic reduction of carbon dioxide to carbon monoxide.