An electrocatalyst M-Ni2P / NF, its preparation method and application

By growing a high-valence metal-controlled Ni2P catalyst in situ on a nickel foam substrate, the problem of insufficient activity of a single Ni2P catalyst was solved, and a highly efficient electrocatalytic process for the synergistic hydrogen evolution of furfural oxidation was achieved, reducing energy consumption and improving catalytic activity.

CN123108632APending Publication Date: 2026-11-17HENAN UNIVERSITY OF TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611484292.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-22
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing single Ni2P catalysts have insufficient catalytic activity in the oxygen evolution reaction (OER), resulting in high energy consumption and making it difficult to meet practical needs.

Method used

Using nickel foam as a substrate, an electrocatalyst M-Ni2P/NF was prepared by in-situ growth of Ni2P controlled by high-valence metal M (such as Re or Mo). Ammonium fluoride and urea were used to activate the substrate and promote the formation of Ni-based precursors during the hydrothermal process, resulting in a more active catalyst.

Benefits of technology

The improved electronic structure and surface chemical environment of the catalyst significantly enhanced the electrocatalytic efficiency of furfural oxidation and synergistic hydrogen evolution, reduced cell voltage, and improved catalytic activity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108632A_ABST
    Figure CN123108632A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of electrocatalyst technology, and discloses an electrocatalyst M-Ni2P / NF, its preparation method and application. The catalyst uses NF as a substrate, and Ni2P regulated by metal M is grown in situ on the substrate. The metal M is a high-valence metal. Preparation method: (1) After cutting the foamed nickel, it is acid washed and dried for later use; (2) The M source, nickel salt, ammonium fluoride, urea and water are stirred together to obtain a mixed solution; (3) The foamed nickel and the mixed solution are transferred to a hydrothermal reaction device and the foamed nickel is immersed in the mixed solution. The hydrothermal reaction device is sealed and hydrothermally reacted at 80~200℃ for 200~900min; after the reaction is completed, it is naturally cooled to room temperature, the foamed nickel is taken out, washed and dried to obtain a solid precursor; (4) The phosphating material and the solid precursor are calcined at 200~800℃ for 30~200min under an inert atmosphere or protective atmosphere to obtain the target catalyst. This invention effectively regulates the electronic structure and surface chemical environment of the catalyst by introducing high-valence metal elements, thereby improving the intrinsic activity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of electrocatalyst technology, specifically relating to an electrocatalyst M-Ni2P / NF, its preparation method, and its application. Background Technology

[0002] Hydrogen, as a clean energy carrier with high energy density and zero carbon emissions, is considered an ideal alternative to traditional fossil fuels. Electrolysis of water is an important route for producing green hydrogen, but it is limited by the slow kinetics and high overpotential of the oxygen evolution reaction (OER), resulting in high energy consumption. Replacing OER with biomass electro-oxidation, which has better thermodynamics, can significantly reduce cell voltage and simultaneously produce high-value-added chemicals. Furfural is widely available, and its oxidation product, furoic acid, is an important chemical intermediate. Therefore, developing a system for synergistic hydrogen evolution through furfural oxidation (FFOR) has significant research value.

[0003] Transition metal phosphides (TMPs), especially nickel phosphide (Ni2P), have become a research hotspot for replacing noble metal catalysts due to their platinum-like electronic structure and low cost. However, the catalytic activity of Ni2P alone still falls short of practical requirements. Summary of the Invention

[0004] To address the problem of insufficient catalytic activity in existing single Ni2P catalysts, the present invention aims to provide an electrocatalyst M-Ni2P / NF, its preparation method, and its applications.

[0005] To achieve the above objectives, the technical solution adopted by the present invention is as follows: An electrocatalyst M-Ni2P / NF is disclosed, wherein the catalyst is based on NF (nickel foam), and Ni2P (nickel phosphide) regulated by metal M is grown in situ on the substrate, wherein the metal M is a high-valence metal.

[0006] The metal M is Re or Mo.

[0007] A method for preparing the electrocatalyst M-Ni2P / NF, comprising the following steps: (1) After cutting the nickel foam, pickle and dry it for later use; (2) Mix M source, nickel salt, ammonium fluoride, urea and water together to obtain a mixed solution; (3) Transfer the nickel foam and the mixed solution to the hydrothermal reaction apparatus and immerse the nickel foam in the mixed solution. Seal the hydrothermal reaction apparatus and perform a hydrothermal reaction at 80~200℃ for 200~900 min. After the reaction is completed, allow it to cool naturally to room temperature, remove the nickel foam, wash it, and dry it to obtain a solid precursor. (4) Calcine the phosphating material and solid precursor at 200-800℃ for 30-200 min under an inert or protective atmosphere to obtain the target catalyst; In step (2), the M source is calculated based on the M element it provides, and the nickel salt is calculated based on the nickel element it provides. The ratio of raw materials used is M source: nickel salt: ammonium fluoride: urea: water = (0.1~1) mmol: (0.5~5) mmol: (2~10) mmol: (2~10) mmol: (15~35) mL; Based on the amount of nickel provided, for every 3 mmol of nickel salt described in step (2), the area of ​​the nickel foam used in step (3) is 2-7 cm². 2 ; Every 2cm 2 The nickel foam described in step (3) corresponds to the amount of phosphating material used in step (4) of 150~250mg.

[0008] Preferably, the M source is perrhenate or ammonium molybdate.

[0009] Furthermore, the perrhenate is ammonium perrhenate, sodium perrhenate, or potassium perrhenate.

[0010] Preferably, the nickel salt is nickel nitrate, nickel sulfate, or nickel acetate.

[0011] Preferably, in step (4), the phosphating material and the solid precursor obtained in step (3) are placed upstream and downstream of a tube furnace, respectively, and then calcined at 200~800℃ for 30~200min under an inert atmosphere or protective atmosphere.

[0012] Preferably, the phosphating material is sodium hypophosphite.

[0013] Preferably, in step (4), the temperature is increased to the calcination temperature at a heating rate of 1~25℃ / min.

[0014] Application of the electrocatalyst M-Ni2P / NF in the synergistic hydrogen evolution of furfural oxidation.

[0015] In this invention, ammonium fluoride is used to activate the substrate surface during the hydrothermal process to form more Ni-based nucleation sites; urea is rapidly hydrolyzed during the hydrothermal process to promote the formation of Ni-based precursors.

[0016] Beneficial effects: (1) The present invention can effectively regulate the electronic structure and surface chemical environment of the catalyst by introducing high-valence metal elements, thereby improving the intrinsic activity; (2) The catalyst preparation method of the present invention has the advantages of ingenious design concept and simple preparation process. It exhibits excellent electrocatalytic efficiency in the coupled reaction of furfural oxidation and cathode hydrogen production, and has good economic applicability. Attached Figure Description

[0017] Figure 1: Physical images of the precursors and catalysts prepared in Example 3 and Comparative Example 1 of the present invention.

[0018] Figure 2 XRD pattern of the Re-Ni2P / NF catalyst prepared in Example 3 of this invention.

[0019] Figure 3 SEM images of the Re-Ni2P / NF catalyst prepared in Example 3 of this invention and the Ni2P / NF catalyst prepared in Comparative Example 1.

[0020] Figure 4 EDX elemental mapping of the Re-Ni2P / NF catalyst prepared in Example 3 of this invention.

[0021] Figure 5 : Electrochemical testing apparatus diagram and LSV linear sweep voltammetry curves of the Re-Ni2P / NF catalyst prepared in Example 3 of this invention and the Ni2P / NF catalyst prepared in Comparative Example 1.

[0022] Figure 6 EIS diagrams of the Re-Ni2P / NF catalyst prepared in Example 3 of this invention and the Ni2P / NF catalyst prepared in Comparative Example 1. Detailed Implementation

[0023] To enable those skilled in the art to better understand the technical solutions of the present invention, the present invention will be further described below in conjunction with specific embodiments. Obviously, the described embodiments are only some, not all, of the embodiments of the present invention. Based on the described embodiments, all other embodiments obtained by those skilled in the art without creative effort are within the protection scope of the present invention.

[0024] Example 1

[0025] A method for preparing an electrocatalyst Re-Ni2P / NF, comprising the following steps: (1) Cut nickel foam (abbreviated as NF) into pieces with an area of ​​4cm². 2 Afterwards, it is pickled and dried using conventional techniques for later use; (2) Add 0.1 mmol of ammonium perrhenate (NH4ReO4), 3 mmol of nickel nitrate hexahydrate (Ni(NO3)2·6H2O), 5 mmol of ammonium fluoride, 5 mmol of urea, and 22 mL of deionized water to a polytetrafluoroethylene-lined hydrothermal reactor and stir until homogeneous to obtain a mixed solution. (3) Transfer the mixed solution from step (2) to the hydrothermal reactor, and at the same time place the nickel foam from step (1) into the hydrothermal reactor and immerse the nickel foam in the mixed solution. Tighten the reactor lid and transfer the hydrothermal reactor to the oven. (4) Set the oven heating temperature to 120℃ and the heating time to 360min; (5) After the oven is cooled to room temperature, the foamed nickel is taken out and repeatedly rinsed with deionized water and anhydrous ethanol, and then dried to obtain a solid precursor, which is labeled as Re-Ni precursor. (6) Place the solid precursor obtained in step (5) and 200 mg of sodium hypophosphite in a small porcelain boat, and then place them in a tube furnace (with sodium hypophosphite upstream and solid precursor downstream). Replace the air in the furnace with Ar gas three times, and then heat the furnace to the calcination temperature of 300°C at a heating rate of 5°C / min under Ar atmosphere. Calcinate for 60 min to obtain the target catalyst.

[0026] Example 2 The difference from Example 1 is that in step (2), the amount of ammonium perrhenate is changed to 0.3 mmol; everything else is the same as in Example 1.

[0027] Example 3 The difference from Example 1 is that in step (2), the amount of ammonium perrhenate is changed to 0.5 mmol; everything else is the same as in Example 1.

[0028] Example 4 The difference from Example 1 is that in step (2), the amount of ammonium perrhenate is changed to 0.7 mmol; all other steps are the same as in Example 1.

[0029] Example 5 The difference from Example 1 is that in step (2), the amount of ammonium perrhenate is changed to 1 mmol; everything else is the same as in Example 1.

[0030] Example 6 The difference from Example 1 is that in step (6), the calcination temperature is changed to 600℃; all other aspects are the same as in Example 1.

[0031] Example 7 The difference from Example 1 is that in step (6), the calcination time is changed to 30 min; all other steps are the same as in Example 1.

[0032] Example 8 The difference from Example 1 is that in step (2), ammonium perrhenate is replaced with ammonium molybdate ((NH4)6Mo7O). 24 (·4H2O) and the amount of ammonium molybdate was 0.07 mmol, and the amount of nickel nitrate hexahydrate was 3 mmol; everything else was the same as in Example 1.

[0033] The catalyst prepared in this comparative example is Mo-Ni2P / NF.

[0034] Compare with Example 1 The difference from Example 1 is that in step (2), the amount of ammonium perrhenate is 0; everything else is the same as in Example 1.

[0035] The solid precursor obtained in step (5) of this comparative example is labeled as Ni precursor, and the catalyst prepared in this comparative example is Ni2P / NF.

[0036] Compare with Example 2 The difference from Example 1 is that step (6) is omitted; everything else is the same as in Example 1.

[0037] The solid precursor obtained in step (5) of this comparative example is the catalyst, abbreviated as Re-Ni. pre / NF.

[0038] Catalyst characterization Figure 1 The images show the precursors and catalysts prepared in Example 3 and Comparative Example 1 of this invention: the left image shows the preparation in Comparative Example 1, and the right image shows the preparation in Example 3.

[0039] Figure 2 The image shows the XRD pattern of the Re-Ni2P / NF catalyst prepared in Example 3 of this invention. Figure 2 It can be seen that, after comparison with the standard card, the two stronger peaks (~44.5° and 51.8°) are peaks of nickel foam, and the relatively weaker peaks (~40.8° and 47.3°) are peaks of Ni2P, confirming that the product prepared in Example 3 of this invention is Re-Ni2P / NF.

[0040] Figure 3 SEM images of the Re-Ni2P / NF catalyst prepared in Example 3 of this invention and the Ni2P / NF catalyst prepared in Comparative Example 1. Figure 3 It can be seen that the introduction of high-valence metal Re modulates the morphology of Ni2P.

[0041] Figure 4 This is an EDX elemental mapping diagram of the Re-Ni2P / NF catalyst prepared in Example 3 of this invention. Figure 4 It can be seen that Re is uniformly dispersed in the Ni2P substrate.

[0042] Catalyst evaluation (a) Electrochemical evaluation was conducted using an RST electrochemical workstation and an H-type electrolytic cell. The electrolytic cell was divided into cell A and cell B by an ion exchange membrane. Cell A was the electrolytic cell containing the working electrode, and cell B was the electrolytic cell containing the counter electrode. The catalysts prepared in Examples 1-8 and Comparative Examples 1-2 were respectively prepared according to a nickel foam area of ​​1 cm². 2 The electrode was cut and used as both the working electrode and the counter electrode. 20 mL of 1 M KOH electrolyte was added to each of cells A and B. An additional 1 mmol of furfural was added to cell A. The voltage range was set to 1~2 V.

[0043] Figure 5 The diagram shows the electrochemical testing setup and the LSV linear sweep voltammetry curves (scan rate 20 mV s) of the Re-Ni2P / NF catalyst prepared in Example 3 of this invention and the Ni2P / NF catalyst prepared in Comparative Example 1. -1 ).Depend on Figure 5 It can be seen that the introduction of high-valence metal Re improves the performance of Ni2P / NF furfural oxidation synergistic hydrogen evolution.

[0044] At 300mA cm -2 The cell voltages measured at the current density are listed in Table 1. As can be seen from Table 1, the cell voltages (HER||FFOR) of the coupled systems of the Re-modified catalysts of Examples 1-7 and the Mo-modified catalyst of Example 8 are significantly lower than those of the unmodified pure Ni2P / NF control sample (Control Example 1), confirming that the introduction of high-valence metals Re or Mo has a significant promoting effect on improving the synergistic hydrogen evolution activity of furfural oxidation.

[0045]

[0046] (ii) Electrochemical evaluation was conducted using an RST electrochemical workstation and an H-type electrolytic cell. This electrolytic cell was divided into cell A and cell B by an ion-exchange membrane. Cell A contained the working electrode and reference electrode, while cell B contained the counter electrode. The catalysts prepared in Example 3 and Comparative Example 1 were respectively arranged according to a nickel foam area of ​​1 cm². 2 The electrode was cut to serve as the working electrode, the stone rod as the counter electrode, and the silver / silver chloride electrode as the reference electrode. 20 mL of 1 M KOH electrolyte was added to each of cells A and B. An additional 1 mmol of furfural was added to cell A. The testing frequency was 0.01 Hz to 10 Hz. 6 Hz, amplitude is 0.007V.

[0047] Figure 6 The images show the EIS spectra of the Re-Ni2P / NF catalyst prepared in Example 3 of this invention and the Ni2P / NF catalyst prepared in Comparative Example 1. Figure 6 It can be seen that the introduction of high-valence metal Re promotes electron transfer.

[0048] The above research results of this invention demonstrate that the introduction of high-valence metals Re or Mo can not only regulate the morphology of Ni2P, but also accelerate the electron transfer in the electrocatalytic process, thereby enhancing the activity of furfural oxidation and synergistic hydrogen evolution.

Claims

1. An electrocatalyst M-Ni2P / NF, characterized in that: The catalyst is based on NF, on which Ni2P regulated by metal M is grown in situ. The metal M is a high-valence metal.

2. The electrocatalyst M-Ni2P / NF as described in claim 1, characterized in that: The metal M is Re or Mo.

3. A method for preparing the electrocatalyst M-Ni2P / NF as described in claim 1, characterized in that, The preparation steps are as follows: (1) After cutting the nickel foam, pickle and dry it for later use; (2) Mix M source, nickel salt, ammonium fluoride, urea and water together to obtain a mixed solution; (3) Transfer the nickel foam and the mixed solution to the hydrothermal reaction apparatus and immerse the nickel foam in the mixed solution. Seal the hydrothermal reaction apparatus and perform a hydrothermal reaction at 80~200℃ for 200~900 min. After the reaction is completed, allow it to cool naturally to room temperature, remove the nickel foam, wash it, and dry it to obtain a solid precursor. (4) Calcine the phosphating material and solid precursor at 200-800℃ for 30-200 min under an inert or protective atmosphere to obtain the target catalyst; In step (2), the M source is calculated based on the M element it provides, and the nickel salt is calculated based on the nickel element it provides. The ratio of raw materials used is M source: nickel salt: ammonium fluoride: urea: water = (0.1~1) mmol: (0.5~5) mmol: (2~10) mmol: (2~10) mmol: (15~35) mL; Based on the amount of nickel provided, for every 3 mmol of nickel salt described in step (2), the area of ​​the nickel foam used in step (3) is 2-7 cm². 2 ; Every 2cm 2 The amount of nickel foam described in step (3) corresponds to the amount of phosphating material used in step (4) of 150~250mg.

4. The preparation method of the electrocatalyst M-Ni2P / NF as described in claim 3, characterized in that: The M source is perrhenate or ammonium molybdate.

5. The method for preparing the electrocatalyst M-Ni2P / NF as described in claim 4, characterized in that: The perrhenate is ammonium perrhenate, sodium perrhenate, or potassium perrhenate.

6. The method for preparing the electrocatalyst M-Ni2P / NF as described in claim 3, characterized in that: The nickel salt is nickel nitrate, nickel sulfate, or nickel acetate.

7. The method for preparing the electrocatalyst M-Ni2P / NF as described in claim 3, characterized in that: In step (4), the phosphating material and the solid precursor are placed upstream and downstream of the tube furnace, respectively, and then calcined at 200~800℃ for 30~200min under an inert atmosphere or protective atmosphere.

8. The method for preparing the electrocatalyst M-Ni2P / NF as described in claim 3 or 7, characterized in that: The phosphating material is sodium hypophosphite.

9. The method for preparing the electrocatalyst M-Ni2P / NF as described in claim 3, characterized in that: In step (4), the temperature is increased to the calcination temperature at a heating rate of 1~25℃ / min.

10. The application of the electrocatalyst M-Ni2P / NF as described in claim 1 or 2 in the synergistic hydrogen evolution of furfural oxidation.