A Pt-Ni bimetallic hydrogen evolution electrocatalyst and its preparation method

By constructing a Pt-Ni heterointerface using a modified fullerene support and air annealing in-situ hydroxylation technology, the problems of slow hydrolysis of Pt catalysts and insufficient contact with Ni(OH)2 under alkaline conditions were solved. This resulted in highly efficient hydrogen evolution over a wide pH range with low Pt dosage. The catalyst exhibited excellent performance under both acidic and alkaline conditions, and the cost was reduced.

CN123108635APending Publication Date: 2026-11-17SHAANXI UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611535677.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-30
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing technologies, Pt catalysts have high energy barriers for water dissociation under alkaline conditions and slow kinetics; Ni exists in alloy form in Pt-Ni alloy catalysts, which fails to effectively promote water dissociation; Ni(OH)2 and Pt have insufficient contact and limited interfacial area; fullerene-based catalysts have small specific surface area and insufficient metal anchoring sites; and there is a lack of simple and controllable methods to induce Ni surface hydroxylation in situ at the Pt-Ni heterointerface.

Method used

Fullerene supports were modified using a mesoporous silica template method. A Pt-Ni heterostructure was constructed by wet chemical reduction and in-situ hydroxylation of the Ni surface was induced under air annealing to form a Ni(OH)2-rich co-catalytic layer. The performance of the catalyst under acidic and alkaline conditions was controlled by combining one-step co-reduction and stepwise reduction methods.

Benefits of technology

It achieves high-efficiency hydrogen evolution performance over a wide pH range with low Pt dosage. The catalyst exhibits excellent HER performance under both acidic and alkaline conditions. It uses less precious metal, reduces costs, and significantly improves stability and activity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108635A_ABST
    Figure CN123108635A_ABST
Patent Text Reader

Abstract

This invention discloses a Pt-Ni bimetallic hydrogen evolution electrocatalyst and its preparation method, belonging to the field of electrocatalytic hydrogen evolution technology. The catalyst uses fullerene modified by mesoporous silica template method as a support, and employs a wet chemical reduction method to support platinum and nickel to form a platinum-nickel heterointerface. Then, air annealing induces in-situ hydroxylation of the nickel surface, forming a surface hydroxylation layer rich in nickel hydroxide. Hydroxylated nickel promotes the dissociation of water molecules, while platinum promotes the recombination and desorption of hydrogen intermediates; the two functions synergistically. The Pt-Ni bimetallic hydrogen evolution electrocatalyst exhibits a conductivity of 10 mA / cm² in 0.5 mol / L H₂SO₄. 2 The overpotential is only 37mV, and the mass activity is 3.4 times that of commercial Pt / C; the overpotential in 1mol / L KOH is 56mV; the Faraday efficiency is over 98.8%, and it can operate stably for more than 120 hours.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of electrocatalytic hydrogen evolution technology, specifically relating to a Pt-Ni bimetallic hydrogen evolution electrocatalyst and its preparation method, which can be applied to fields such as water electrolysis for hydrogen production, renewable energy conversion and storage. Background Technology

[0002] Hydrogen energy, with its zero carbon emissions, high energy density (146 kJ / g), and wide availability, is considered the most promising clean energy source for achieving global carbon neutrality. Water electrolysis for hydrogen production uses electricity to split water into hydrogen and oxygen, producing no carbon-containing byproducts. Furthermore, the electricity can be converted from renewable energy sources such as wind and solar power, making it a green and sustainable hydrogen production method. In water electrolysis hydrogen production devices, the hydrogen evolution reaction (HER) occurring at the cathode is a two-electron reduction process. In acidic media, it follows the Volmer-Heyrovsky or Volmer-Tafel mechanism. In alkaline media, because the protons originate from water molecules, additional energy is required to break the H-OH bond, resulting in alkaline HER kinetics being 2 to 3 orders of magnitude slower than acidic HER. Therefore, developing highly efficient HER catalysts with suitable hydrogen adsorption free energy and low water dissociation energy barriers is crucial for the large-scale industrial application of water electrolysis for hydrogen production.

[0003] Platinum (Pt)-based materials, with their near-ideal hydrogen adsorption free energy, are currently recognized as the most active HER electrocatalysts. However, the scarcity of Pt in the Earth's crust, its high price, and its slow water dissociation kinetics under alkaline conditions severely limit its large-scale application. To reduce Pt usage and improve catalytic performance, researchers have developed various strategies, including alloying, interface engineering, support regulation, and co-catalyst modification. Regarding alloying strategies, Pt can form alloys with transition metals (such as Ni, Co, and Cu) to regulate the electronic structure of Pt through ligand and strain effects, thereby optimizing the hydrogen adsorption energy. Zhejiang University prepared a PtNi / C alloy catalyst using a polyol method. By adjusting the pH value with NaOH to control the alloy particle size, they found that as the particle size decreased, the electrocatalytic activity for methanol oxidation increased, and the PtNi alloy exhibited a certain degree of resistance to CO poisoning. Beijing University of Chemical Technology prepared high-entropy nanoalloys such as PtAg, PtCuRu, and PtRuCoNiCu using liquid-phase reduction, centrifugal, and solvothermal methods. Among them, the high-entropy nanodendritic PtRuCoNiCu exhibited a performance of 10 mA / cm² in alkaline HER. 2 The overpotential is only 10 mV. However, in alloying strategies, the uniform mixing of metal atoms makes it difficult to achieve spatial separation of functional sites; and alloying usually requires high-temperature treatment, which leads to particle growth and reduced atom utilization.

[0004] In the field of Pt-Ni oxide composite catalysts, nickel oxide (NiO) and nickel hydroxide (Ni(OH)2) are used as co-catalysts in combination with Pt due to their excellent adsorption and activation capabilities for water molecules. Xuchang University prepared NiO microspheres (3-4 μm in diameter) with a secondary lamellar structure at 85 °C using a hydrothermal method. Then, Pt nanoparticles were deposited on NiO / carbon rod electrodes via electrodeposition for the electrocatalytic oxidation of ethanol. The study found that NiO exhibits catalytic activity for CO and synergistically interacts with Pt, improving its resistance to poisoning. However, in this study, the NiO was pre-prepared as bulk nickel oxide microspheres with a small specific surface area and limited active sites; the electrodeposition method is complex and difficult to scale up. Jiangxi University of Science and Technology prepared a PtNi / CeO2 / NC catalyst using an equal-volume impregnation method and an electrodisplacement method for methanol oxidation, where CeO2 was used as a rare earth oxide modifier and Ni as an alloy component. However, in this study, Ni existed in alloy form without surface hydroxylation treatment, and the application was limited to methanol oxidation. Regarding the mechanism by which Ni(OH)2 cocatalysts promote water dissociation, previous studies have shown that Ni(OH)2 can serve as an active site for water molecule dissociation, synergistically enhancing the hydrogen recombination function of Pt to improve the performance of basic HER. However, in existing technologies, Ni(OH)2 is usually pre-prepared and then physically mixed or electrodeposited with Pt, which suffers from problems such as insufficient contact between Ni(OH)2 and Pt, limited interfacial area, and complex preparation processes. How to construct a Ni(OH)2 cocatalytic layer in situ on the Pt-Ni heterointerface using a simple and controllable method to achieve spatial proximity synergy between water dissociation sites and hydrogen recombination sites remains an unsolved technical challenge.

[0005] Regarding catalyst supports, the interaction between traditional carbon supports (carbon black, carbon nanotubes, graphene, etc.) and metal nanoparticles is weak, and the metal particles are prone to aggregation, detachment, and dissolution during long-term electrolysis. Fullerene C 60 It is a carbon material with a unique spherical curved surface structure and strong electron-withdrawing properties, capable of modulating the electronic structure of metal atoms and providing anchoring points. Huazhong University of Science and Technology uses C... 60 Ru-based HER catalysts were prepared using fullerenes as supports, demonstrating the strong electronic interactions between the fullerene support and the metal. Donghua University used functionalized fullerene self-assembled structures as supports and electrochemically deposited Pt / Pd for methanol oxidation, finding that the introduction of fullerenes significantly improved catalytic activity. However, most existing fullerene-based catalysts use unmodified C2000. 60Alternatively, simply hydroxylated fullerols have limited specific surface areas and insufficient metal anchoring sites. Furthermore, existing Pt-Ni bimetallic catalysts are mostly prepared using a co-reduction method, where the simultaneous reduction of both metals easily forms a homogeneous alloy, making it difficult to achieve spatial optimization of Ni(OH)₂ surface enrichment and Pt active site exposure. In addition, existing technologies lack precise methods for controlling the degree of hydroxylation on the Ni species surface, making it difficult to optimize the catalyst surface structure according to the application scenario (acidic or alkaline electrolyte).

[0006] In summary, the existing technology has the following technical defects: First, single-metal Pt catalysts have high energy barriers for water dissociation under alkaline conditions and slow kinetics; in Pt-Ni alloy catalysts, Ni exists in alloy form and does not have the water dissociation co-catalytic function of Ni(OH)2, so it cannot effectively solve the bottleneck of alkaline water dissociation.

[0007] Second, in existing Pt-NiO or Pt-Ni(OH)2 composite catalysts, NiO / Ni(OH)2 is mostly a pre-prepared bulk material (micron-scale), with a small specific surface area, limited active sites, and a limited contact interface area with Pt, so the synergistic effect cannot be fully utilized; the preparation methods are mostly electrodeposition or physical mixing, which are complex processes and difficult to scale up.

[0008] Third, existing technologies lack a method to induce Ni surface hydroxylation in situ at the Pt-Ni heterointerface through a simple and controllable air annealing process, which makes it impossible to achieve spatial proximity and precise control of Ni(OH)2 water dissociation sites and Pt hydrogen recombination sites.

[0009] Fourth, most existing fullerene-based catalysts use unmodified C464. 60 It has a limited specific surface area and insufficient metal anchor points.

[0010] Therefore, developing a catalyst and its preparation method that uses modified fullerene as a support, induces in-situ hydroxylation of Ni surface through air annealing, constructs a Pt-Ni(OH)2 heterointerface, and achieves high-efficiency hydrogen evolution over a wide pH range with low Pt content is of great theoretical and practical significance. Summary of the Invention

[0011] The purpose of this invention is to overcome the aforementioned problems in the prior art and provide a Pt-Ni bimetallic hydrogen evolution electrocatalyst and its preparation method. This method enhances the metal-support interaction by modifying the fullerene support using a mesoporous silica template method, constructs a Pt-Ni heterostructure using a wet chemical reduction method, and then induces in-situ hydroxylation of the Ni surface through air annealing to form a Ni(OH)2-rich co-catalytic layer. This achieves the synergistic function of Ni(OH)2 promoting water dissociation and Pt promoting hydrogen recombination. Furthermore, the acid / base performance is responsively regulated through both one-step co-reduction and stepwise reduction pathways.

[0012] To address the aforementioned technical problems, this invention provides a Pt-Ni bimetallic hydrogen evolution electrocatalyst, comprising a modified fullerene support and nickel and platinum components supported on the surface of the modified fullerene support. The nickel and platinum components form a platinum-nickel bimetallic heterointerface on the surface of the modified fullerene support. The surface of the nickel component is hydroxylated to form a surface hydroxylation layer containing nickel hydroxide. The modified fullerene support is a fullerene modified by a mesoporous silica template method.

[0013] Furthermore, the surface hydroxylation layer contains nickel hydroxide, and the molar percentage of nickel hydroxide in the nickel component is 30% to 80%. The surface hydroxylation layer retains the conductivity of the metallic Ni core and provides abundant water dissociation active sites.

[0014] Further, the platinum component is loaded at 3 wt% to 10 wt%, the nickel component is loaded at 1 wt% to 8 wt%, and the molar ratio of platinum to nickel is 1:1 to 1:5. Preferably, the platinum loading is 4 wt% to 7 wt%, the nickel loading is 3 wt% to 6 wt%, and the molar ratio of platinum to nickel is 1:2 to 1:3. The introduction of the non-noble metal Ni significantly reduces the amount of noble metal Pt used and the overall cost of the catalyst.

[0015] Furthermore, the modified fullerene support has a specific surface area of ​​80 m². 2 / g to 200m 2 / g, with pore size distribution concentrated in the range of 2nm to 10nm.

[0016] Furthermore, the platinum component Pt 4f 7 / 2 The characteristic peak binding energy shifts by 0.2 eV to 0.8 eV relative to the single metal platinum / fullerene catalyst towards a higher binding energy direction, with electrons transferring from Pt to Ni or the surface hydroxylation layer, and the electronic structure of Pt is effectively modulated.

[0017] Furthermore, the catalyst achieves 10 mA / cm² in a 0.5 mol / L H₂SO₄ electrolyte. 2 The overpotential of the current density is no greater than 50 mV, reaching 10 mA / cm² in 1 mol / L KOH electrolyte. 2 The overpotential of the current density is not greater than 70mV.

[0018] To achieve the above objectives, the present invention also provides a method for preparing the Pt-Ni bimetallic hydrogen evolution electrocatalyst, comprising the following steps: (1) Preparation of modified fullerene support: Fullerene C 60The fullerene carrier with a mesoporous silica template was mixed with the fullerene carrier and then removed after high-temperature treatment to obtain a mesoporous modified fullerene carrier. After high-temperature treatment, the surface defects of the fullerene increased, providing more anchoring points for the metal particles.

[0019] (2) Metal component loading: The modified fullerene support is dispersed in a solvent, and nickel and platinum precursors are added. Nickel and platinum nanoparticles are deposited under the action of a reducing agent to form a platinum-nickel heterostructure interface. (3) Air annealing and hydroxylation: The product obtained in step (2) is subjected to thermal annealing in an air atmosphere to cause oxidation and hydroxylation of the nickel species surface, forming a surface hydroxylation layer containing nickel hydroxide, thus obtaining the Pt-Ni bimetallic hydrogen evolution electrocatalyst. The air annealing treatment causes oxidation and hydroxylation of the Ni species surface, forming a thin layer rich in Ni(OH)2 on the surface of Ni nanoparticles.

[0020] Further, step (2) employs a one-step co-reduction method: the nickel precursor and platinum precursor are simultaneously added to the dispersion, and co-reduction is performed under the action of a reducing agent to form a platinum-nickel heterostructure. Specifically, the nickel precursor solution and the platinum precursor solution are simultaneously added to the modified fullerene dispersion, stirred and adsorbed, and then sodium borohydride is added for co-reduction to obtain PtNi / C. 60 The precursor, after air annealing, yields a one-step co-reduced prototype PtNiO / C. 60 Catalyst. In the catalyst prepared by this method, Ni and Pt nucleate and grow simultaneously, resulting in a more uniform mixing of Pt and Ni at the heterogeneous interface. After surface hydroxylation, Ni(OH)2 sites and Pt sites are highly interleaved, exhibiting superior HER performance under acidic conditions.

[0021] Further, step (2) adopts a stepwise reduction method: first, a nickel precursor is added to reduce and deposit nickel nanoparticles, and then a platinum precursor is added to reduce and deposit platinum nanoparticles to form a platinum-nickel heterostructure. Specifically, a nickel precursor solution is added first, stirred and adsorbed, and then sodium borohydride is added to reduce and obtain a nickel-supported fullerene intermediate. After washing and drying, it is dispersed in water, a platinum precursor solution is added, stirred and adsorbed, and then sodium borohydride is added to reduce and deposit Pt on or near its surface. The resulting heterostructure has a clearer Ni core-Pt shell or Ni-Pt adjacent structure, resulting in Pt-Ni / C. 60 The precursor, after air annealing, yields a stepwise reduced Pt-NiO / C precursor. 60 Catalyst. The catalyst prepared by this method exhibits a more hierarchical spatial distribution of Pt and Ni, more complete hydroxylation of the Ni surface, and superior water dissociation ability and HER performance under alkaline conditions.

[0022] Further, in step (2), the nickel precursor is nickel chloride, the platinum precursor is chloroplatinic acid, the reducing agent is sodium borohydride, and the nickel and platinum precursors are prepared by dissolving them in ethanol respectively; in step (3), the air annealing temperature is 250°C to 350°C, the annealing time is 1 h to 3 h, and the air flow rate is 50 mL / min to 200 mL / min. If the annealing temperature is too low (<250°C), the hydroxylation of the Ni surface is insufficient; if the annealing temperature is too high (>350°C), Ni is over-oxidized to NiO and the metal particles agglomerate. Preferably, the annealing temperature is 280°C to 320°C.

[0023] The present invention also provides the application of the above-mentioned Pt-Ni bimetallic hydrogen evolution electrocatalyst in water electrolysis for hydrogen production, including hydrogen evolution reaction catalysis in alkaline electrolytes (such as 1M KOH) and acidic electrolytes (such as 0.5M H2SO4).

[0024] Compared with the prior art, the present invention has the following beneficial effects: First, this invention induces in-situ hydroxylation of Ni species on the surface through air annealing, forming a surface hydroxylation layer rich in Ni(OH)2 at the Pt-Ni heterostructure interface. Ni(OH)2 acts as an active center for water molecule dissociation, efficiently breaking H-OH bonds to generate H intermediates; Pt acts as an active center for hydrogen intermediate desorption, promoting H binding to generate H2. The two are spatially adjacent and functionally synergistic at the nanoscale, simultaneously solving the problems of slow dissociation of single-metal Pt in alkaline water and poor conductivity of Ni(OH)2, achieving highly efficient HER over a wide pH range. Compared with existing methods that pre-fabricate NiO / Ni(OH)2 and then recombine it with Pt, the Ni(OH)2 layer formed by in-situ hydroxylation has a closer contact with the Pt and Ni cores, a larger interface area, and more active sites.

[0025] Secondly, the air annealing hydroxylation method of the present invention is simple, controllable, and scalable. By adjusting the annealing temperature (250-350℃) and time (1-3h), the degree of hydroxylation on the Ni surface (Ni(OH)2 molar ratio 30%-80%) can be precisely controlled, avoiding the complex processes such as electrodeposition and hydrothermal treatment in the prior art.

[0026] Third, this invention employs a mesoporous silica template method to modify the structure of fullerenes, resulting in a surface area that remains unchanged. 60 Approximately 40m 2 / g increased to 120m 2 The addition of a layer of saturated carbon (C) at a density of over / g introduces abundant mesoporous structures and surface defects, providing more anchoring sites for metal nanoparticles, enhancing metal-support interactions, and effectively suppressing the aggregation and detachment of metal particles. This contrasts with existing unmodified C… 60 Or simply hydroxylated C 60In comparison, modified fullerene supports significantly improve the activity and stability of catalysts.

[0027] Fourth, this invention provides two synthetic routes: one-step co-reduction and stepwise reduction. By controlling the deposition sequence and interfacial structure of Pt and Ni, the responsiveness of acid / base performance is optimized. The catalyst prepared by the one-step co-reduction method exhibits better performance under acidic conditions, while the catalyst prepared by the stepwise reduction method exhibits better performance under alkaline conditions.

[0028] Fifth, the catalyst of this invention has a low amount of precious metal (approximately 5 wt% Pt), far lower than that of commercial Pt / C (20 wt% Pt), but its mass activity under acidic conditions is 3.4 times that of commercial Pt / C, with a TOF value of 3.62 s. -1 The Faraday efficiency is over 98.8%, and it operates stably for over 120 hours. This achieves efficient utilization of precious metals, which helps reduce catalyst costs. Attached Figure Description

[0029] Figure 1 The Pt-Ni bimetallic hydrogen evolution electrocatalyst PtNiO / MFC prepared by the two methods of this invention 60 Pt-NiO / MFC 60 Structural diagram; Figure 2 Transmission electron microscope image of a Pt-Ni bimetallic hydrogen evolution electrocatalyst; Figure 3 High-resolution transmission electron microscope image and electron diffraction pattern of Pt-Ni bimetallic hydrogen evolution electrocatalyst; Figure 4 X-ray diffraction pattern of Pt-Ni bimetallic hydrogen evolution electrocatalyst; Figure 5 X-ray photoelectron spectroscopy of Pt-Ni bimetallic hydrogen evolution electrocatalyst; Figure 6 Polarization curves of Pt-Ni bimetallic hydrogen evolution electrocatalysts prepared by one-step co-reduction and stepwise reduction methods in 0.5 mol / L H2SO4; Figure 7 Polarization curves of Pt-Ni bimetallic hydrogen evolution electrocatalysts prepared by one-step co-reduction and stepwise reduction methods in 1 mol / L KOH; Figure 8 The stability test curves and Faraday efficiency plots for the catalyst are shown. Detailed Implementation

[0030] The technical solution of the present invention will be clearly and completely described below with reference to the embodiments. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0031] It will be understood by those skilled in the art that, unless otherwise defined, all terms used herein (including technical and scientific terms) have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. It should also be understood that terms such as those defined in general dictionaries should be understood to have the meaning consistent with their meaning in the context of the prior art, and should not be interpreted in an idealized or overly formal sense unless specifically defined as herein. The reagents used herein may be commercially available related products, and performance testing standards refer to industry or national standards.

[0032] Those skilled in the art will understand that, unless specifically stated otherwise, the singular forms “a,” “an,” “the,” and “the” used herein may also include the plural forms. It should be further understood that the term “comprising” as used in this specification means the presence of the stated features, integers, steps, operations, elements, and / or components, but does not exclude the presence or addition of one or more other features, integers, steps, operations, elements, components, and / or groups thereof. The term “and / or” as used herein includes all or any units and all combinations of one or more associated listed items.

[0033] Example 1

[0034] In this embodiment, the modified fullerene carrier MFC was prepared using the mesoporous silica template method. 60 The specific steps are as follows: (1) Weigh 100mg of fullerene C 60 Mix 500 mg of mesoporous silica template SBA-15 in an agate mortar and grind thoroughly for 30 minutes to achieve C 60 It is uniformly filled into the mesoporous channels of SBA-15.

[0035] (2) The mixture was transferred into a ceramic boat and placed in a tube furnace. Under an argon atmosphere, the temperature was increased to 600°C at 5°C / min and held for 2 hours. Then, it was allowed to cool naturally to room temperature. This high-temperature treatment caused C... 60 Under the mesoporous confinement of SBA-15, structural rearrangement occurs, forming a defect-enriched carbon structure.

[0036] (3) The product was immersed in 50 mL of 10 wt% HF solution and stirred for 24 h to completely remove the silica template. Then, it was washed with deionized water by centrifugation until the pH of the supernatant was neutral. The product was then vacuum dried at 60 °C for 12 h to obtain the modified fullerene carrier MFC. 60 MFC was tested using nitrogen adsorption-desorption. 60 Specific surface area is 128 m² 2 / g, average pore size 4.2nm, pore volume 0.35cm³ 3 / g; and unmodified C 60 Its specific surface area is only 38m² 2 / g, almost no mesoporous structure. Raman spectroscopy shows MFC 60 The intensity ratio (ID / IG) of the D-band to G-band is 0.86, which is higher than that of the unmodified C. 60 The value of 0.52 indicates that the mesoporous template method introduces abundant surface defects. Transmission electron microscopy observation shows that MFC 60 It retains the spherical particle characteristics of fullerenes, while there are obvious mesoporous channels between the particles.

[0037] Example 2

[0038] This embodiment employs a one-step co-reduction method combined with air annealing to prepare a fullerene-based Pt-Ni bimetallic hydrogen evolution electrocatalyst, PtNiO / MFC, at a surface-hydroxylated platinum-nickel heterointerface. 60 A schematic diagram of the overall structure of the catalyst is shown below. Figure 1 As shown, combined with Figure 2 The TEM image shows that Ni / Ni(OH)₂ nanoparticles and Pt nanoparticles are loaded on the surface of the modified fullerene support in the catalyst, forming a Pt-Ni heterostructure. The Ni particles are covered with a surface hydroxylation layer. The specific steps are as follows: (1) Weigh 50 mg of the MFC prepared in Example 1 60 The carrier was dispersed in 40 mL of ethylene glycol and sonicated for 30 min to form a uniform dispersion. A nickel precursor solution with a concentration of 20 mg / mL was prepared by dissolving nickel chloride (NiCl2·6H2O) in ethanol, and a platinum precursor solution with a concentration of 19.3 mmol / L was prepared by dissolving chloroplatinic acid (H2PtCl6·6H2O) in ethanol. 0.42 mL of the nickel precursor solution and 0.73 mL of the platinum precursor solution were simultaneously added to the above MFC. 60 In the dispersion, stir for 30 minutes to allow the metal ions to be fully adsorbed onto the carrier surface.

[0039] (2) Under ice-water bath (0℃) conditions, add 5 mL of fresh NaBH4 solution with a concentration of 0.1 mol / L dropwise, and continue stirring for 2 h to allow Ni to react. 2+ and Pt 4+Co-reduction yields metallic nanoparticles, forming a platinum-nickel heterostructure. After three alternating centrifugal washes with deionized water and ethanol, and vacuum drying at 60°C, PtNi / MFC is obtained. 60 Precursor.

[0040] (3) The precursor was placed in a tube furnace and heated to 300°C at 5°C / min under an air atmosphere (flow rate 100 mL / min), held for 2 h, and then naturally cooled to obtain the one-step co-reduced PtNiO / MFC. 60 The catalyst is denoted as sample A.

[0041] Inductively coupled plasma atomic emission spectrometry (ICP-AES) analysis revealed that sample A contained 5 wt% Pt and 3.6 wt% Ni, with a Pt / Ni molar ratio of approximately 1:2.5. High-resolution transmission electron microscopy (HTEM) was used to determine the composition of sample A. Figure 3 As shown, from Figure 3 The high-resolution transmission electron microscopy (HTEM) image shows that the heterostructure nanoparticles formed by the Pt and Ni are uniformly dispersed on the surface of the fullerene MFC60 matrix, with an average particle size of 3.1 nm. The heterostructure formed by the direct contact between the Pt (111) and Ni (111) crystal planes can be observed (the 0.226 nm interplanar spacing corresponds to the Pt (111) crystal plane, and the 0.203 nm interplanar spacing corresponds to the Ni (111) crystal plane). Electron diffraction (SAED) patterns were selected to demonstrate the diffraction spots of the MFC60 (002) and (110) crystal planes, the Pt (111) crystal plane, and the Ni (111) crystal plane. The X-ray diffraction pattern is shown below. Figure 4 As shown, the diffraction peaks at 34.7°, 46.3°, and 67.7° correspond to the (111), (200), and (220) crystal planes of the cubic Pt (JCPDS No. 87-0646), respectively. The diffraction peaks at 10.8°, 17.7°, and 20.8° correspond to the (111), (220), and (311) crystal planes of the face-centered cubic C60 (JCPDS No. 44-0558), respectively, indicating that the fullerene structure was not completely destroyed by high-temperature oxidation. As for the lack of detection of the Ni metal peak, it may be due to the low Ni loading and fine grain size leading to broadening of the diffraction peak, thus not being clearly displayed in the XRD pattern. At the same time, no obvious alloy phase shift peaks were observed, proving that it is a heterostructure rather than an alloy. X-ray photoelectron spectroscopy is as follows. Figure 5As shown in the full spectrum, Pt, Ni, C, and O were detected in PtNiO / MFC60, Pt-NiO / MFC60, PtNi / MFC60, and Pt-Ni / MFC60. The O1s XPS spectra of all four samples can be fitted with three distinct peaks, corresponding to lattice oxygen (MO), hydroxyl groups (OH), and adsorbed oxygen species (Oad), respectively. Compared to PtNi / MFC60 and Pt-Ni / MFC60, the OH peaks of PtNiO / MFC60 and Pt-NiO / MFC60 are more shifted towards higher binding energy directions and have a higher proportion, indicating the formation of a large number of hydroxyl groups on their surface, which may affect their HER performance. The high-resolution fine spectrum of Pt 4f can be divided into two orbitals, Pt4f5 / 2 and Pt4f7 / 2, which are convolved with metallic platinum (Pt0) and platinum oxide (Pt2+), respectively. The Ni 2p orbital can be divided into two orbitals, Ni 2p3 / 2 and Ni 2p1 / 2, which can be divided into two peaks, corresponding to the Ni2+ species and its satellite peak, respectively. After calcination, the Pt and Ni peaks of the two samples, PtNiO / MFC60 and Pt-NiO / MFC60, shift towards higher binding energies, indicating an increase in valence state. High-valence metals provide numerous catalytically active sites on the catalyst surface. Simultaneously, the heterojunction between Pt and Ni further enhances the synergistic effect between different components, accelerating the kinetic process. In the Ni 2p spectrum, Ni0 and Ni2+ coexist, and peak fitting calculations show that the molar proportion of Ni(OH)2 is approximately 55%. The Pt 4f7 / 2 binding energy is 71.18 eV, shifting by 0.38 eV towards higher binding energies compared to single-metal Pt / MFC60 (70.80 eV), indicating electron transfer from Pt to Ni or the surface hydroxylation layer at the heterojunction. In-situ Raman spectroscopy revealed that the intensity of the tetrahedral coordinated water peak at 3200 cm⁻¹ and the hydrogen-bonded water peak at 3400 cm⁻¹ varies with potential, demonstrating that the surface hydroxylation layer promotes the activation of interfacial water and the dynamic reorganization of the hydrogen bond network.

[0042] Example 3

[0043] This embodiment uses a stepwise reduction method combined with air annealing to prepare the catalyst Pt-NiO / MFC. 60 A schematic diagram of the overall structure of the catalyst is shown below. Figure 1 As shown, Ni / Ni(OH)₂ nanoparticles and Pt nanoparticles are loaded onto the surface of the modified fullerene support, forming a Pt-Ni heterointerface. The Ni particles are covered with a surface hydroxylation layer. The specific steps are as follows: (1) Weigh 50 mg of the MFC prepared in Example 1 60The carrier was dispersed in 40 mL of ethylene glycol and sonicated for 30 min to form a uniform dispersion. A nickel precursor solution with a concentration of 20 mg / mL was prepared by dissolving nickel chloride (NiCl2·6H2O) in ethanol, and a platinum precursor solution with a concentration of 19.3 mmol / L was prepared by dissolving chloroplatinic acid (H2PtCl6·6H2O) in ethanol. 0.42 mL of the nickel precursor solution was added to the above MFC. 60 Stir the dispersion for 30 minutes.

[0044] (2) Under ice-water bath (0℃) conditions, add 5 mL of fresh NaBH4 solution with a concentration of 0.1 mol / L dropwise, and continue stirring for 2 h to allow Ni to react. 2+ Reduced to metal nanoparticles, the mixture was washed three times alternately by centrifugation with deionized water and ethanol, and then vacuum dried at 60°C to obtain Ni / MFC. 60 Precursor.

[0045] (3) Ni / MFC 60 The precursor was redispersed in 40 mL of ethylene glycol and sonicated for 30 min. 0.73 mL of the prepared platinum precursor solution was added, and the mixture was stirred for 30 min. Then, 5 mL of fresh 0.1 mol / L NaBH4 solution was added dropwise under an ice-water bath, and stirring was continued for 2 h to allow the Pt precursor to react. 4+ Reduced to metal nanoparticles deposited on or near the surface of Ni particles to form a platinum-nickel heterointerface, the Pt-Ni / MFC was obtained by alternating centrifugation and washing three times with deionized water and ethanol, followed by vacuum drying at 60°C. 60 Precursor.

[0046] (4) Air annealing is performed in the same manner as step (3) in Example 2 (300℃, 2h, air flow rate 100mL / min) to obtain the stepwise reduction Pt-NiO / MFC. 60 The catalyst is denoted as sample B.

[0047] ICP-AES analysis showed that sample B contained 5.0 wt% Pt and 3.6 wt% Ni, with a Pt / Ni molar ratio of approximately 1:2.5. HRTEM revealed more uniform Pt and Ni dispersion, a clearer heterogeneous interface structure, and a more continuous and complete Ni(OH)₂ layer on the surface of the Ni particles. XPS analysis showed that the molar percentage of Ni(OH)₂ was approximately 62%, higher than the 55% of the one-step co-reduction method. The Pt 4f₇ / ₂ binding energy was 71.25 eV, a shift of 0.45 eV compared to the single-metal Pt / MFC₆0 method.

[0048] Example 4

[0049] This example tests the HER performance of the catalyst in 0.5 mol / L H2SO4. A three-electrode system was used, with a catalyst loading of 0.283 mg / cm³ on the working electrode. 2The counter electrode is a graphite rod, the reference electrode is RHE, and the scan rate is 5mV / s.

[0050] The results are as follows Figure 6 As shown, sample A obtained by the one-step co-reduction method has a strength of 10 mA / cm under acidic conditions. 2 Overpotential (η) at current density 10 The overpotential is 37 mV, the Tafel slope is 20.24 mV / dec; the mass activity at an overpotential of 100 mV is 2.28 A / mgPt, and the transition frequency (TOF) is 3.62 s. -1 Sample B, acidic η, obtained by stepwise reduction method 10 The value is 45 mV, and the mass activity is 1.65 A / mg Pt. The η of commercially available 20% Pt / C... 10 The activity was 48 mV and 0.67 A / mg Pt. Sample A's activity was 3.4 times that of commercial Pt / C. This demonstrates that the one-step co-reduction method is superior under acidic conditions, attributed to the highly staggered distribution of Pt and Ni providing more exposed Pt active sites.

[0051] Example 5

[0052] This embodiment tests the HER performance of the catalyst in 1 mol / L KOH.

[0053] The results are as follows Figure 7 As shown, sample B in the stepwise reduction method under alkaline conditions η 10 =56mV, Tafel slope 42mV / dec, double-layer capacitance Cdl=12.12mF / cm 2 One-step co-reduction method for sample A under alkaline conditions η 10 =68mV. η for commercial use of 20% Pt / C 10 The value is 62 mV. It can be seen that the stepwise reduction method is better under alkaline conditions. This is attributed to the fact that the more continuous and complete Ni(OH)2 layer provides more water dissociation sites, which effectively reduces the energy barrier of the alkaline Volmer step.

[0054] Example 6

[0055] This example investigates the effect of air annealing temperature on the degree of hydroxylation and catalytic performance. A series of prepared catalysts were air-annealed at 200℃, 250℃, 300℃, 350℃, and 400℃ for 2 hours, and their acidic HER performance was tested.

[0056] The results show that the performance is optimal when annealed at 300℃ (η 10 =37mV), at 200℃, the molar percentage of Ni(OH)2 is only 22%, indicating insufficient hydroxylation, η 10 The value is 58mV; at 250℃, Ni(OH)₂ accounts for 40%, and η 10The value is 45mV; at 300℃, Ni(OH)₂ accounts for 55%, and η 10 The value is 37mV; at 350℃, Ni(OH)₂ accounts for 72%, but the metal particles begin to slightly agglomerate (average particle size 4.2nm), η 10 The value is 48mV; at 400℃, Ni is excessively oxidized to NiO and the particles grow significantly (average particle size 6.5nm), η 10 The value was increased to 72 mV. This result demonstrates that effective surface hydroxylation and particle dispersion can be achieved within the annealing temperature range of 250 °C to 350 °C.

[0057] Example 7

[0058] This embodiment investigates the effect of the Pt / Ni molar ratio on performance. While keeping the Pt loading at approximately 5 wt%, the Ni feed amount was varied, and catalysts with Pt / Ni molar ratios of 1:1, 1:2, 1:3, and 1:5 were prepared by one-step co-reduction method and annealing at 300°C for 2 hours.

[0059] The results are shown in Table 1. The acidity performance was optimal when the Pt / Ni molar ratio was 1:3. When the Ni ratio was too low (1:1), there were insufficient hydrolysis sites, and η... 10 The value is 50mV; when the Ni ratio is too high (1:5), the Pt active sites are covered by Ni(OH)2, η 10 The value was 49 mV. This result demonstrates that a Pt / Ni molar ratio in the range of 1:1 to 1:5 can achieve a balance between water dissociation sites and hydrogen recombination sites.

[0060] Table 1. Catalyst test data for different Pt / Ni molar ratios. Pt / Ni molar ratio Pt loading (wt%) Ni loading (wt%) <![CDATA[η 10 (mV)]]> Mass activity (A / mgPt) 1:1 5.1 1.5 50 1.12 1:2 5.0 3.0 40 1.85 1:3 5.2 4.7 37 2.28 1:5 5.1 7.7 49 1.05 Example 8

[0061] This example tests the long-term stability and Faraday efficiency of the catalyst. The catalyst was tested in 0.5 mol / L H₂SO₄ at a rate of 10 mA / cm⁻¹. 2 The Faraday efficiency was calculated by collecting the generated hydrogen gas using the water displacement method after 120 hours of constant current electrolysis.

[0062] Test results are as follows Figure 8 As shown, after 120 hours of continuous electrolysis, the overpotential increased by only 10 mV (from 37 mV to 47 mV), demonstrating the excellent long-term stability of the catalyst. The Faraday efficiency ranged from 98.8% to 99.7%, close to the theoretical value of 100%, indicating that the HER reaction was dominant and the side reactions were negligible. HRTEM observation after electrolysis showed no significant agglomeration of the metal particles, with the particle size increasing from 3.1 nm to 3.6 nm, proving that the strong interaction between the modified fullerene support and the metal effectively suppressed particle agglomeration and shedding.

[0063] Comparative Example 1 This comparative preparation of PtNi / MFC without air annealing and hydroxylation 60 The catalyst was prepared by a one-step co-reduction method (same as steps 1-3 in Example 2), except that step (3) was changed to annealing at 300°C for 2 hours in an argon atmosphere. The other conditions were the same as in Example 2, and it was recorded as control sample 1.

[0064] XPS displays Ni as almost entirely Ni. 0 (Ni) 2+ (Percentage <5%), with no obvious hydroxylation layer on the surface. Acidic HER test η 10 68mV, alkaline η 10 The value was 95 mV, significantly lower than that of sample A (37 mV for acidic samples and 68 mV for basic samples). This result demonstrates that the surface hydroxylation layer induced by air annealing is crucial for improving HER performance, and the hydrolysis co-catalytic function of Ni(OH)2 is a key factor in performance enhancement.

[0065] Comparative Example 2 This comparative example prepares single-metal Pt / MFC 60 The catalyst, loaded with only Pt (5.2 wt%) and not Ni, was subjected to the same wet chemical reduction method and air annealing (300 °C, 2 h), and is designated as control sample 2.

[0066] Acidic HER test η 10 The value is 55 mV, and the mass activity is 0.82 A / mg Pt; the alkalinity η is... 10 The value was 88 mV, significantly worse than that of sample A. This result demonstrates that the introduction of Ni and the surface hydroxylation layer significantly improves the catalytic performance, especially under alkaline conditions, where the hydrolysis-promoting effect of Ni(OH)2 significantly enhances the alkaline performance.

[0067] Comparative Example 3 This comparative example uses commercial Ni(OH)2 powder and Pt / MFC. 60 Physical mixing. First, prepare Pt / MFC. 60 (Pt loading 5.2wt%), then add commercial Ni(OH)2 powder at a Pt / Ni molar ratio of 1:3, ultrasonically mix for 30 min, do not air annealing, and record as control sample 3.

[0068] Acidic HER test η 10 72mV, alkaline η 10 The activity was 85 mV and 0.58 A / mg Pt. This performance was significantly worse than sample A, demonstrating that the physical mixing of pre-prepared Ni(OH)₂ and Pt suffers from poor interfacial contact and low utilization of active sites. The Ni(OH)₂ layer formed in situ through air annealing in this invention has a closer contact with Pt and the Ni core, resulting in a larger interfacial area and significant advantages.

[0069] Comparative Example 4 This comparative example uses unmodified C. 60 PtNiO / C was prepared using a one-step co-reduction method and air annealing (300℃, 2h) as a carrier. 60 The catalyst, with Pt and Ni loadings comparable to that of sample A, is designated as control sample 4.

[0070] Acidic HER test η 10 The overpotential was 55 mV, with a mass activity of 1.18 A / mgPt; after 50 h of stability testing, the overpotential increased by 28 mV. Both performance and stability were inferior to sample A, demonstrating that the fullerene support modified by the mesoporous silica template method significantly improved catalytic activity and stability by increasing specific surface area and defect sites, and enhancing metal-support interactions.

[0071] Comparative Example 5 This comparative example uses a commercially available 20% Pt / C catalyst (Johnson Matthey) as a reference to test HER performance under the same conditions.

[0072] Acidic HER: η 10 =48mV, mass activity 0.67A / mgPt, TOF=1.05s -1 ; Alkaline HER: η 10 =62mV. Sample A, with a Pt loading of only one-quarter that of commercially available Pt / C, exhibits an acidic η. 10 The catalyst exhibits lower efficiency, with a mass activity 3.4 times that of commercial Pt / C and a TOF 3.4 times higher, demonstrating that the catalyst of this invention achieves efficient utilization of precious metals.

[0073] The above examples and comparative examples fully demonstrate that the surface-hydroxylated platinum-nickel heterointerface fullerene-based hydrogen evolution electrocatalyst of the present invention has excellent wide pH HER activity, high stability, high Faradaic efficiency and low noble metal content. The air annealing in-situ hydroxylation method is simple and controllable, and has good application prospects.

[0074] The preferred embodiments of the present invention have been described in detail above, and are only used to illustrate the technical solutions of the present invention, and are not intended to limit it. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features therein; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A Pt-Ni bimetallic hydrogen evolution electrocatalyst, comprising a modified fullerene support and nickel and platinum components supported on the surface of the modified fullerene support, characterized in that, The nickel component and the platinum component form a platinum-nickel bimetallic heterostructure on the surface of the modified fullerene support. The surface of the nickel component is hydroxylated to form a surface hydroxylation layer containing nickel hydroxide. The modified fullerene support is a fullerene modified by a mesoporous silica template method.

2. The Pt-Ni bimetallic hydrogen evolution electrocatalyst according to claim 1, characterized in that, The surface hydroxylation layer contains nickel hydroxide, wherein the molar percentage of nickel hydroxide is 30% to 80%.

3. The Pt-Ni bimetallic hydrogen evolution electrocatalyst according to claim 1, characterized in that, The platinum component has a loading of 3 wt% to 10 wt%, the nickel component has a loading of 1 wt% to 8 wt%, and the molar ratio of platinum to nickel is 1:1 to 1:

5.

4. The Pt-Ni bimetallic hydrogen evolution electrocatalyst according to claim 1, characterized in that, The modified fullerene carrier has a specific surface area of ​​80 m². 2 / g to 200m 2 / g, with pore size distribution concentrated in the range of 2nm to 10nm.

5. The Pt-Ni bimetallic hydrogen evolution electrocatalyst according to claim 1, characterized in that, The platinum component Pt4f 7 / 2 The characteristic peak binding energy shifts by 0.2 eV to 0.8 eV relative to the single-metal platinum / fullerene catalyst towards higher binding energy.

6. The Pt-Ni bimetallic hydrogen evolution electrocatalyst according to claim 1, characterized in that, The catalyst achieves 10 mA / cm² in a 0.5 mol / L H₂SO₄ electrolyte. 2 The overpotential of the current density is no greater than 50 mV, reaching 10 mA / cm² in 1 mol / L KOH electrolyte. 2 The overpotential of the current density is not greater than 70mV.

7. A method for preparing the Pt-Ni bimetallic hydrogen evolution electrocatalyst according to any one of claims 1 to 6, characterized in that, Includes the following steps: (1) Preparation of modified fullerene support: Fullerene C 60 The mixture was mixed with a mesoporous silica template, and the template was removed after high-temperature treatment to obtain a mesoporous modified fullerene carrier. (2) Metal component loading: The modified fullerene support is dispersed in a solvent, and nickel and platinum precursors are added. Nickel and platinum nanoparticles are deposited under the action of a reducing agent to form a platinum-nickel heterostructure interface. (3) Air annealing hydroxylation: The product obtained in step (2) is subjected to thermal annealing in an air atmosphere to cause oxidation and hydroxylation of the nickel species surface, forming a surface hydroxylation layer containing nickel hydroxide, and the Pt-Ni bimetallic hydrogen evolution electrocatalyst is obtained.

8. The preparation method according to claim 7, characterized in that, Step (2) adopts a one-step co-reduction method: the nickel precursor and the platinum precursor are added to the dispersion at the same time, and co-reduction is carried out under the action of the reducing agent to form a platinum-nickel heterostructure. The resulting catalyst has better performance under acidic conditions.

9. The preparation method according to claim 7, characterized in that, Step (2) adopts a stepwise reduction method: first, nickel precursor is added to reduce and deposit nickel nanoparticles, and then platinum precursor is added to reduce and deposit platinum nanoparticles to form a platinum-nickel heterostructure. The resulting catalyst has better performance under alkaline conditions.

10. The preparation method according to claim 7, characterized in that, In step (2), the nickel precursor is nickel chloride, the platinum precursor is chloroplatinic acid, the reducing agent is sodium borohydride, and the nickel and platinum precursors are prepared by dissolving them in ethanol respectively; in step (3), the air annealing temperature is 250°C to 350°C, the annealing time is 1h to 3h, and the air flow rate is 50mL / min to 200mL / min.