A coaxial nested spinneret device and a method for preparing an in-situ modified functional fiber membrane.
In-situ modification of functional fiber membranes is achieved by using a coaxial nested spinneret device, which solves the problem of simultaneous functionalization in existing technologies, improves the structural stability and functional durability of fiber membranes, and is suitable for the industrial production of high-end functional nonwoven membrane materials.
Patent Information
- Application Number
- CN202611603374.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-16
- Publication Date
- 2026-11-17
AI Technical Summary
Existing instantaneous pressure-relief spinning technology lacks dedicated molding equipment that can simultaneously complete fiber formation and functionalization. Traditional modification processes suffer from structural damage, low utilization rate of functional raw materials, poor stability, complex processes, and high costs, failing to meet the demand for efficient, integrated, and high-quality preparation of high-end functional nonwoven membrane materials.
A coaxial nested spinneret device is used to drive the functional side chains and/or functional monomers in the homogeneous precursor solution to rapidly surface segregate within a millisecond-level setting period through the coupling of the inner liquid channel and the outer ring fluid medium channel. This achieves an in-situ surface activation reaction, resulting in an in-situ modified functional fiber membrane with a highly uniform porous skeleton, high tensile strength, long-lasting resistance to physical washing, and responsive function.
It simplifies the production process, improves the efficiency of functional modification, ensures the stability of the porous fiber skeleton structure and the washability of the functional layer, reduces production costs, and is suitable for the industrial application of high-end functional nonwoven membrane materials.
Smart Images

Figure CN123108748A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of polymer nonwoven material molding and processing equipment and non-equilibrium multiphase flow reaction engineering technology, specifically involving a coaxial nested spinneret device and a method for preparing an in-situ modified functional fiber membrane. Background Technology
[0002] Instantaneous pressure-relief spinning is a special fiber-forming process based on the non-equilibrium phase transition of a homogeneous polymer solution under high temperature and pressure. Its core principle utilizes the extremely rapid pressure difference instantly generated as the polymer solution flows through the spinneret structure, simultaneously triggering multiple physical effects such as instantaneous solvent evaporation, polymer phase separation, and strain-induced crystallization of macromolecules. This allows the polymer matrix to be constructed into a three-dimensional network of micro / nano porous fibrils with multi-level fractal characteristics within milliseconds. Leveraging its unique advantages of rapid fiber formation, controllable porous structure, and good matrix integrity, the nonwoven fiber membrane materials prepared by this process possess irreplaceable application value in high-tech industries such as specialized medical protection, industrial superfiltration, and high-end specialty packaging.
[0003] With the rapid development of the modern functional materials industry, the market's performance requirements for functional polymer nonwoven membrane materials continue to upgrade. The application scenarios of high-end functional fiber membranes such as moisture-absorbing and heat-humidity management membranes, heavy metal chelate adsorption membranes, charged electret air deep filtration membranes, and decontamination and antiviral biobarrier membranes are constantly expanding, which puts forward stringent requirements on the functional activity, structural stability, long-term use and high efficiency of preparation of materials.
[0004] Currently, the industry mainly uses two methods for functional modification of instantaneous pressure-relieving spun fiber membranes: post-finishing modification and in-reactor pre-addition of functional phases. However, both mainstream processes have inherent technical defects, which seriously restrict the industrial application and performance upgrade of functional fiber membranes. Among them, the post-finishing modification process mainly uses methods such as impregnation, spraying, and grafting modification to functionalize the formed fiber membrane. This process is not only cumbersome, with a long production cycle and high cost, but also easily generates wastewater and waste liquid, causing environmental pollution. It also erodes and damages the original three-dimensional porous skeleton structure of the fiber membrane, resulting in a significant decrease in the material's mechanical properties and air permeability filtration performance. At the same time, the functional modification layer only adheres to the fiber surface, with low bonding strength, poor washability and functional durability, and is prone to functional detachment and failure after long-term use.
[0005] The in-spinning functional phase modification process involves directly incorporating functional auxiliaries, monomers, or fillers during the preparation of the precursor solution to achieve blending of functional components with the polymer matrix. However, in actual spinning, the functional phase dispersed in the polymer solution is easily and tightly embedded by the rapidly solidifying polymer matrix. Only a very small number of functional active sites are exposed on the fiber membrane surface, while most functional components are locked inside the matrix and cannot participate in interfacial interactions. This significantly reduces the efficiency of functional modification, resulting in the fiber membrane's core functions such as adsorption, filtration, antibacterial properties, and humidity and heat regulation not being fully realized. Consequently, the actual performance of the product falls far short of design expectations.
[0006] In summary, existing instantaneous pressure-relief spinning technology lacks dedicated molding equipment that can simultaneously complete fiber formation and functionalization. Traditional modification processes have many shortcomings, such as structural damage, low utilization rate of functional raw materials, poor stability, complex processes, and high costs, which cannot meet the needs of efficient, integrated, and high-quality preparation of high-end functional nonwoven membrane materials. Summary of the Invention
[0007] The purpose of this invention is to provide a coaxial nested spinneret device and a method for preparing in-situ modified functional fiber membranes. The coaxial nested spinneret device provided by this invention drives the functional side chains and / or functional monomers in the homogeneous precursor solution to rapidly segregate on the surface within a millisecond-level setting period, and completes the in-situ surface activation reaction in one step, thereby obtaining an in-situ modified functional fiber membrane with highly uniform porous skeleton, high tensile strength, long-lasting resistance to physical washing, and responsive function. This invention has high utilization rate of functional raw materials, good product stability, simple process flow, and low cost, making it suitable for industrial applications.
[0008] To achieve the above objectives, the present invention provides the following technical solution: This invention provides a coaxial nested spinneret device, comprising a housing, wherein an axially penetrating liquid channel is provided within the housing. The liquid channel includes a liquid inlet, a pressure-reducing channel, a first channel, a spinneret hole, and a spinneret hole connected in sequence. The first channel is a tapered channel, with its larger end connected to the pressure-reducing channel and its smaller end connected to the spinneret hole. The spinneret hole is a frustum-shaped spinneret hole, with its smaller end connected to the spinneret hole, forming an expanding cavity from the smaller end to the larger end. The housing also includes a fluid medium channel, which comprises a fluid medium delivery channel and a fluid medium annular nozzle. The fluid medium delivery channel and the fluid medium annular nozzle are connected through a second channel. The fluid medium annular nozzle is coaxially arranged around the outside of the wire exit hole. The second channel and the fluid medium annular nozzle are inclined towards the central axis of the wire exit hole in the direction of fluid medium flow. The second channel is a tapered channel, with its large end connected to the fluid medium delivery channel and its small end connected to the fluid medium annular nozzle.
[0009] Preferably, the cone angle A1 of the first channel satisfies: 120°>A1>100°; the diameter and length of the spinneret are D1 and L1 respectively, satisfying: 0.5 mm≤D1≤2 mm, 1:1≤L1 / D1≤4:1; the small port diameter of the wire exiting hole is D2, the large port diameter is D3, the length is L2, and the cone angle is A2, satisfying: 3 mm≤D2≤6 mm, 9 mm≤D3≤12 mm, L2 / D3<L2 / D2≤2, 20° <A2≤45°。
[0010] Preferably, the diameter and length of the liquid inlet are D1' and L1', respectively, satisfying: 1 mm ≤ D1' ≤ 3 mm, 1:1 ≤ L1' / D1' ≤ 3:1.
[0011] Preferably, the fluid medium conveying channel is provided in multiple ways, and each fluid medium conveying channel is evenly distributed on the shell along the circumference; the inclination angle of the second channel relative to the central axis is A4, and the inclination angle of the fluid medium annular nozzle relative to the central axis is A3, satisfying: 30°>A4>A3>3°; the cone angle A5 of the second channel satisfies: 60°>A5>30°; the diameter of the fluid medium conveying channel is D4, and the slit width of the fluid medium annular nozzle is D5, satisfying: 5 mm≤D4≤10 mm, 0.5 mm≤D5≤1.5 mm.
[0012] Preferably, the inner wall surface of the spinneret is perpendicular to the small end face of the wire exiting hole; a micro-rounded corner is provided at the junction of the small end face of the wire exiting hole and its inner wall surface, and the radius R of the micro-rounded corner satisfies: 0.01 mm ≤ R ≤ 0.05 mm.
[0013] Preferably, the inlet end of the fluid medium delivery channel is connected to the fluid medium generation system; the fluid medium generation system includes a microchannel heat exchange unit, the microchannel heat exchange unit is provided with a heating jacket, and a metering pump is provided on the feed inlet pipe of the microchannel heat exchange unit.
[0014] This invention provides a method for preparing in-situ modified functional fiber membranes, using the coaxial nested spinneret device described in the above technical solution, and includes the following steps: A fluid medium is introduced into the fluid medium channel, and after flowing through the fluid medium delivery channel, it is ejected through the fluid medium annular nozzle. A homogeneous precursor solution, containing functional side chains and / or functional monomers, is introduced into the liquid channel through the inlet hole. After flowing through the depressurization channel, it is ejected into the expansion cavity of the spinneret hole through the spinneret hole. After the fluid medium ejected from the fluid medium annular nozzle and the homogeneous precursor solution ejected from the spinneret hole meet, the fluid medium modifies the homogeneous precursor solution in situ. Then, it is deposited on the receiving grid with the flow field to obtain the in-situ modified functional fiber membrane.
[0015] Preferably, the fluid medium ejected from the annular nozzle includes superheated active chemical fluid, superheated steam, or reactive monomer aerosol fluid.
[0016] Preferably, the pressure of the fluid medium input into the fluid medium channel is 2~4MPa and the temperature is 150~180℃.
[0017] Preferably, the in-situ modification includes surface segregation and / or in-situ surface activation reactions of functional side chains and / or functional monomers in a homogeneous precursor solution, wherein the in-situ surface activation reactions include one or more of in-situ surface graft polymerization, in-situ surface ring-opening hydrolysis, and in-situ surface acid-base neutralization reactions.
[0018] This invention provides a coaxial nested spinneret device. The coaxial nested spinneret device utilizes a first channel with a contracting cone angle in the inner liquid channel and a secondary cavitation expansion effect of the exit hole with an inverted frustum structure. Combined with the coupling of the outer ring-shaped annular nozzle of the fluid medium, it leverages the ultra-strong polarity / charge / chemical reaction field formed by the focusing of the fluid medium in situ. When this field interacts with the homogeneous precursor solution, it triggers an active polar capture effect at the phase interface, driving the functional side chains and / or functional monomers in the homogeneous precursor solution to rapidly segregate on the surface within a millisecond-level settling period. This allows for a one-step in-situ surface activation reaction (including graft polymerization, ring-opening hydrolysis, or neutralization anchoring), resulting in an in-situ modified functional fiber membrane with a highly uniform porous skeleton, high tensile strength, long-lasting resistance to physical washing, and responsive functionality. Therefore, the coaxial nested spinneret device provided by this invention, through the coupling effect of the external centripetal counteracting reaction flow field formed by the liquid channel and the fluid medium channel, can still maintain excellent fiber-forming performance under the extreme non-equilibrium flow field environment of high temperature, high pressure and instantaneous pressure release. It is suitable for the whole spectrum of near-critical soluble polymer systems including polymers such as polyolefins, thermoplastic polyesters and polyacrylonitrile-based polymers, and meets the manufacturing scenarios of micro and nanofiber membranes with instantaneous pressure release fiber formation and in-situ chemical reaction modification at the interface, and has important engineering application value.
[0019] This invention provides a method for preparing in-situ modified functional fiber membranes, using the coaxial nested spinneret device described in the above technical solution. Compared with the prior art, this invention has the following significant advantages: This invention abandons the traditional two-step modification model of post-treatment and in-reactor pre-addition. It relies on a ring-shaped fluid medium channel to precisely focus a high-temperature, high-enthalpy fluid medium, constructing a high-intensity polarity, charge, and chemical reaction field at the fiber strand forming front. Utilizing the active capture effect of the gas-liquid non-equilibrium phase interface, it drives the rapid surface segregation of functional side chains and / or functional monomers in the homogeneous precursor solution within the millisecond-level fiber shaping window, simultaneously completing the in-situ surface activation reaction. The entire process eliminates the need for subsequent secondary functionalization processes such as wet impregnation, spraying, and high-temperature curing, significantly simplifying the production process, shortening the production cycle, reducing equipment investment and energy consumption, while completely avoiding the corrosion, damage, and environmental pollution problems caused by traditional post-treatment processes to the fiber's porous skeleton.
[0020] This invention simultaneously couples functional modification with the fiber film-forming and shaping process. Functional segments and active groups in the homogeneous precursor solution achieve interfacial anchoring and co-crystallization lock during the polymer macromolecule solidification stage, resulting in an integrated structure between the functional modification layer and the fiber matrix, rather than the surface-attached structure of traditional processes. This fundamentally solves the problems of easy functional layer detachment and poor washability. Furthermore, no secondary processing such as subsequent wet heat soaking or chemical treatment is required; the fiber's original three-dimensional porous network structure remains undamaged, and the air permeability network retention rate can reach over 96%. The prepared in-situ modified functional fiber membrane possesses excellent structural stability, physical wash resistance, and long-lasting functional response characteristics.
[0021] Furthermore, this invention precisely limits the parameters of the cone angle of the first channel of the liquid channel, the aspect ratio of the spinneret, and the expansion angle and aspect ratio of the expansion cavity formed by the downstream frustum-shaped fiber exit hole. By utilizing the sudden expansion structure of the expansion cavity, a rapid drop in the chemical potential of the homogeneous precursor solution is achieved, inducing the rapid and instantaneous evaporation of volatile solvents. This causes the polymer melt to tear and stretch uniformly, forming a three-dimensional network of clustered fibers. The structural design of this invention can precisely control the non-equilibrium phase separation and crystallization behavior of macromolecules, eliminating the problems of uneven fiber thickness, disordered pores, and numerous local defects in traditional spinning processes. Ultimately, a high-performance fiber membrane product with a highly uniform porous skeleton, excellent structural density, and significantly improved tensile strength is obtained.
[0022] In summary, the coaxial nested spinneret device provided by this invention adopts a coaxial nested integrated structural design, integrating multiple functions such as fluid decompression stretching, instantaneous solvent evaporation, interface focusing reaction, and rapid fiber shaping into one device. The device has a compact structure, is easy to assemble, and has high operational stability. Furthermore, the geometric parameters and operating conditions of the fluid medium channel arranged in the outer ring of the liquid channel in this invention can be independently adjusted, making it adaptable to various polymer spinning systems. It can switch between reaction gas flow and aerosol systems according to different functional requirements, realizing the preparation of different types of functional fiber membranes such as adsorption, filtration, antibacterial, and humidity and heat control. The coaxial nested spinneret device provided by this invention has wide adaptability and strong process adjustability, and can be directly adapted to existing instantaneous pressure-relief spinning production lines, making it easy to scale up and industrialize, and possessing extremely high industrial transformation value. Attached Figure Description
[0023] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0024] Figure 1 A schematic diagram of the coaxial nested spinneret device provided by the present invention; Figure 2 for Figure 1 A magnified structural diagram of part A in the middle; Figure 3 This is a schematic diagram of the cross-section of the device of the present invention; Figure 4 Electron micrographs of the quaternary ammonium salt antibacterial fiber membranes prepared for Example 1 (left) and Comparative Example 1 (right); Figure 5 Electron micrographs of the antibacterial nanoparticle fiber membranes prepared for Example 2 (left) and Comparative Example 2 (right); In the diagram: 10-Liquid channel; 11-Liquid inlet; 12-Pressure reducing channel; 13-Spinneret orifice; 14-Spinneret outlet; 20-Fluid medium channel; 21-Fluid medium transport channel; 22-Fluid medium annular nozzle; 23-First channel; 24-Second channel. Detailed Implementation
[0025] This invention provides a coaxial nested spinneret device, comprising a housing, wherein an axially penetrating liquid channel is provided within the housing. The liquid channel includes a liquid inlet, a pressure-reducing channel, a first channel, a spinneret hole, and a spinneret hole connected in sequence. The first channel is a tapered channel, with its larger end connected to the pressure-reducing channel and its smaller end connected to the spinneret hole. The spinneret hole is a frustum-shaped spinneret hole, with its smaller end connected to the spinneret hole, forming an expanding cavity from the smaller end to the larger end. The housing also includes a fluid medium channel, which comprises a fluid medium delivery channel and a fluid medium annular nozzle. The fluid medium delivery channel and the fluid medium annular nozzle are connected through a second channel. The fluid medium annular nozzle is coaxially arranged around the outside of the wire exit hole. The second channel and the fluid medium annular nozzle are inclined towards the central axis of the wire exit hole in the direction of fluid medium flow. The second channel is a tapered channel, with its large end connected to the fluid medium delivery channel and its small end connected to the fluid medium annular nozzle.
[0026] like Figures 1-3 As shown, the coaxial nested spinneret device provided by the present invention adopts a coaxial double-layer nested shell structure, with an axially penetrating liquid channel at its center and a fluid medium channel on the outside of the liquid channel. In the present invention, the second channel and the annular nozzle of the fluid medium are inclined towards the central axis of the wire outlet hole in the direction of fluid medium flow, i.e., the second channel and the annular nozzle of the fluid medium are generally inclined in the same direction as the direction of fluid medium flow.
[0027] The coaxial nested spinneret die device provided by the present invention comprises an axially penetrating liquid passage. The liquid inlet hole, the pressure relief flow channel, the first duct, the spinneret orifice and the filament outlet hole are arranged coaxially. In the present invention, the diameter and length of the liquid inlet hole are respectively D1' and L1', which preferably satisfy: 1 mm≤D1'≤3 mm, 1:1≤L1' / D1'≤3:1. In the present invention, the pressure relief flow channel has a diameter D0 and a length L0. The diameter D0 of the pressure relief flow channel preferably satisfies: 6 mm≤D0≤15 mm, more preferably 8 mm≤D0≤12 mm, and in the embodiment, D0=10 mm. The length L0 of the preferred pressure relief flow channel preferably satisfies: 50 mm≤L0≤200 mm, more preferably 80 mm≤L0≤120 mm, and in the embodiment, L0=100 mm. The length-diameter ratio L0 / D0 of the pressure relief flow channel preferably satisfies: 5:1≤L0 / D0≤15:1, more preferably 8:1≤L0 / D0≤12:1, and in the embodiment, L0 / D0=10:1. In the present invention, the cone angle A1 of the first duct preferably satisfies: 120°>A1>100°, and in the embodiment, A1=110°. The diameter and length of the spinneret orifice are respectively D1 and L1, which preferably satisfy: 0.5 mm≤D1≤2 mm, and in the embodiment, D1=1.0 mm; 1:1≤L1 / D1≤4:1, more preferably 2:1≤L1 / D1≤3:1, and in the embodiment, L1 / D1=2.5:1. The small port diameter of the filament outlet hole is D2, the large port diameter is D3, the length is L2, and the cone angle is A2, which preferably satisfy: 3 mm≤D2≤6 mm, more preferably 4 mm≤D2≤5 mm; 9 mm≤D3≤12 mm, more preferably 10 mm≤D3≤11 mm; L2 / D3<L2 / D2≤2, L2 is preferably 6~8 mm; 20°<A2≤45°, preferably A2=30°.
[0028] In the present invention, the inner wall surface of the spinneret orifice is preferably perpendicular to the small end face of the filament outlet hole, that is, the junction of the spinneret orifice and the filament outlet hole is precisely machined into a completely right-angled non-fillet sharp edge end face without any chamfering and polishing. In the present invention, a micro fillet is provided at the junction of the small end face of the filament outlet hole and its inner wall surface, and the radius R of the micro fillet preferably satisfies: 0.01 mm ≤ R ≤ 0.05 mm. In the present invention, by making the inner wall surface of the spinneret orifice perpendicular to the small end face of the filament outlet hole and optimizing the radius R of the micro fillet to satisfy: 0.01 mm ≤ R ≤ 0.05 mm, the interfacial capillary wall-attached continuity of the non-Newtonian polymer melt fluid is cut off under an extreme pressure relief flow field.
[0029] In the coaxial nested spinneret device provided by the present invention, multiple fluid medium delivery channels are provided, and each fluid medium delivery channel is evenly distributed circumferentially on the housing. In the present invention, the number of fluid medium delivery channels is preferably ≥2, specifically 2, 3, 4 or 6.
[0030] In this invention, the diameter of the fluid medium conveying channel is D4, and the length is L4. The diameter D4 of the fluid medium conveying channel preferably satisfies: 5mm ≤ D4 ≤ 10mm, more preferably 6mm ≤ D4 ≤ 9mm, and in this embodiment, D4 = 8.0mm. The length L4 of the fluid medium conveying channel preferably satisfies: 10mm ≤ L4 ≤ 30mm, more preferably 12mm ≤ L4 ≤ 20mm, and in this embodiment, L4 = 15mm. In this invention, the inclination angle (centripetal angle) of the second channel relative to the central axis is A4, and the inclination angle (centripetal angle) of the fluid medium annular nozzle relative to the central axis is A3, preferably satisfying: 30° > A4 > A3 > 3°, more preferably 25° > A4 > A3 > 8°, even more preferably 15° > A3 > 8°, and 25° > A4 > 18°. The cone angle A5 of the second channel preferably satisfies: 60°>A5>30°, more preferably: 50°>A5>35°, and in this embodiment, A5=45°. The slit width D5 of the annular nozzle of the fluid medium preferably satisfies: 0.5 mm≤D5≤1.5 mm, more preferably 0.6 mm≤D5≤1.0 mm, and in this embodiment, D5=0.8 mm.
[0031] The coaxial nested spinneret device provided by the present invention includes a fluid medium generation system, wherein the inlet end of the fluid medium delivery channel is connected to the fluid medium generation system. The fluid medium generation system preferably includes a microchannel heat exchange unit, which is equipped with a heating jacket, and a metering pump is preferably installed on the feed inlet pipe of the microchannel heat exchange unit.
[0032] This invention provides a method for preparing in-situ modified functional fiber membranes, using the coaxial nested spinneret device described in the above technical solution, and includes the following steps: A fluid medium is introduced into the fluid medium channel, and after flowing through the fluid medium delivery channel, it is ejected through the fluid medium annular nozzle. A homogeneous precursor solution, containing functional side chains and / or functional monomers, is introduced into the liquid channel through the inlet hole. After flowing through the depressurization channel, it is ejected into the expansion cavity of the exit hole through the spinneret hole. After the fluid medium ejected from the fluid medium annular nozzle and the homogeneous precursor solution ejected from the spinneret hole meet, the fluid medium modifies the homogeneous precursor solution in situ, and then it is deposited on the receiving grid with the flow field to obtain the in-situ modified functional fiber membrane.
[0033] In this invention, unless otherwise specified, all raw materials / components used in the preparation are commercially available products well known to those skilled in the art.
[0034] In this invention, the homogeneous precursor solution is preferably a supercritical solution. The homogeneous precursor solution can be a high-pressure near-critical polymer solution.
[0035] In this invention, the homogeneous precursor solution preferably comprises a matrix polymer raw material, an amphiphilic functionally modified monomer, and a solvent. The homogeneous precursor solution preferably also includes an amphiphilic functionally modified oligomer. The solvent is preferably a low-boiling-point, volatile solvent. The homogeneous precursor solution is a macromolecular-level entangled homogeneous high-pressure solution. In a specific embodiment of this invention, the matrix polymer raw material can be high-density polyethylene (HDPE). The amphiphilic functionally modified oligomer can be a quaternary ammonium salt graft copolymer. The pressure of the homogeneous precursor solution is preferably 5-10 MPa, and the temperature is preferably 200-220°C.
[0036] In this invention, the homogeneous precursor solution passes through a first channel, the cone angle of which is preferably A1 satisfying 120°>A1>100°, and is then vertically injected into the expansion cavity of the exit hole through a spinneret orifice with a diameter of D1 and a length-to-diameter ratio of L1 / D1. This invention utilizes the abrupt expansion of space and pressure cliff to induce the homogeneous precursor solution to instantaneously cross the phase diagram boundary of the spinoline, resulting in instantaneous decompression and sudden phase separation.
[0037] In this invention, the fluid medium ejected from the annular nozzle preferably comprises a superheated active chemical fluid, superheated steam, or a reactive monomeric aerosol fluid. In this invention, the fluid medium is heated by the microchannel heat exchange unit, and the pressure of the fluid medium input into the fluid medium channel is preferably 2-4 MPa, and the temperature is preferably 150-180°C. In this invention, when the fluid medium is water, the pressure of the water input into the fluid medium channel is preferably 2-4 MPa, and the temperature is preferably 150-180°C. The water ejected from the annular nozzle then forms superheated steam. The superheated steam can form fine water mist upon cooling.
[0038] In this invention, the confluence of the fluid medium ejected from the annular nozzle and the homogeneous precursor solution ejected from the spinneret at the outer side of the spinneret outlet controls the cone angle A5 of the second channel to satisfy: 60°>A5>30°. The second channel and the annular nozzle of the fluid medium form a multi-stage focusing tilt structure satisfying the angle constraint 30°>A4>A3>3°. This allows the high-speed superheated reactive fluid (which can be a gas flow) ejected from the fluid medium nozzle to bombard the three-dimensional clustered stream ejected from the center, generating a centripetal strong shear flow field. Utilizing the thermodynamic polarity / charge gradient difference between the gas-liquid non-equilibrium phase interface and the surrounding gas flow, an active polarity capture effect is triggered at the interface, strongly pulling the amphiphilic functional components within the bulk phase to rapidly migrate and enrich towards the outermost layer of the fibril. Simultaneously, millisecond-level in-situ grafting, ring-opening hydrolysis, or acid-base neutralization activation reactions are carried out under the high-temperature fluid and high-enthalpy reaction field. The in-situ modified functional fiber membrane is deposited on an atmospheric pressure receiving grid along with the flow field, obtaining the membrane in situ continuously in one step.
[0039] In this invention, the in-situ modification preferably includes surface segregation and / or in-situ surface activation reactions of functional side chains and / or functional monomers in a homogeneous precursor solution. The in-situ surface activation reaction preferably includes one or more of the following: in-situ surface graft polymerization, in-situ surface ring-opening hydrolysis, and in-situ surface acid-base neutralization reactions.
[0040] In this invention, the in-situ modified functional fiber membrane is a porous membrane. The in-situ modified functional fiber membrane is constructed from functional fibers. The functional fibers include fibrils and a functionally active modification layer coating the surface of the fibrils. The internal structure of the fibrils consists of matrix macromolecules arranged axially to form a strong and tough three-dimensional fractal cluster network framework. The functionally active modification layer is seamlessly coated on the fibril surface. The roots of the functionally active modification layer are deeply embedded in the eutectic lock within the crystalline region of the matrix macromolecules. The functionally active modification layer is obtained through in-situ modification.
[0041] To further illustrate the present invention, the technical solutions provided by the present invention will be described in detail below with reference to the embodiments, but they should not be construed as limiting the scope of protection of the present invention.
[0042] Example 1 This embodiment provides a method for preparing a quaternary ammonium salt antibacterial fiber membrane, specifically including the following steps: (1) Maleic anhydride-grafted polyethylene (HDPE-g-MAH, grafting rate 1.2 wt%~1.5 wt%) was dissolved in xylene and heated to 130 °C to completely dissolve it. N,N-dimethylhexanediamine was slowly added dropwise according to the molar ratio of anhydride group to tertiary amine group of 1:1.05. The mixture was refluxed at 140 °C for 5 hours to form an imide side chain tertiary amine structure through ring-opening amidation and dehydration ring-closing reaction. Then, 1.2 molar amounts of hexadecane chloroform and sodium carbonate catalyst (the amount of sodium carbonate catalyst was 1.0 molar amount of tertiary amine group) were added to the system and the quaternization reaction was maintained at 135 °C for 10 hours. After the reaction was completed, the mixture was poured into ethanol while hot to precipitate. After washing with ethanol 3 times, the mixture was vacuum dried at 80 °C for 24 hours to obtain the quaternary ammonium salt graft copolymer (HDPE-g-QAS).
[0043] (2) High-density polyethylene (HDPE) and HDPE-g-QAS were mixed and dissolved in dichloromethane solvent at a weight ratio of 97.5:2.5 to prepare a homogeneous precursor solution with a total solid content of 12 wt%. The temperature inside the high-pressure dissolution vessel was maintained at 220 ℃ and the pressure at 10 MPa.
[0044] (3) This embodiment adopts the following Figures 1-3 The coaxial nested spinneret device shown is fabricated using a coaxial double-layer nested shell structure. Its interior center has an axially penetrating liquid channel, and a fluid medium channel is provided on the outer side of the liquid channel. The shell contains an axially penetrating liquid channel, which includes, in sequence, an inlet, a pressure-reducing channel, a first channel, a spinneret hole, and an outlet hole. The first channel is a tapered channel, with its larger end connected to the pressure-reducing channel and its smaller end connected to the spinneret hole. The outlet hole is a frustum-shaped outlet hole, with its smaller end connected to the spinneret hole, forming an expanding cavity from the smaller end to the larger end. The diameter and length of the inlet hole are D1' and L1', respectively, with D1' being 1.0 mm. The length-to-diameter ratio (L1' / D1') of the inlet hole is controlled to be 3:1. The length L0 of the pressure-reducing channel is 100 mm, and the diameter D0 is 10 mm. The cone angle A1 of the first channel is set to 110°. The spinneret orifice has a diameter D1 = 1.0 mm and a length-to-diameter ratio L1 / D1 = 2.5:1. The exit orifice dimensions are precisely controlled as follows: D2 = 4.0 mm, D3 = 10 mm, length L2 = 8.0 mm, and cone angle A2 = 30°. The inner wall of the spinneret orifice is perpendicular to the small end face of the exit orifice. A micro-rounded corner is provided at the junction of the small end face of the exit orifice and its inner wall, with the radius R of the micro-rounded corner satisfying: 0.01 mm ≤ R ≤ 0.05 mm. The homogeneous precursor solution is stably input into the liquid channel of the coaxial nested spinneret device, and the homogeneous precursor solution suddenly expands into the expansion cavity of the exit orifice.
[0045] (4) The coaxial nested spinneret device used in this embodiment also has a fluid medium channel inside its housing. The fluid medium channel includes a fluid medium conveying channel and a fluid medium annular nozzle. The fluid medium conveying channel and the fluid medium annular nozzle are connected through a second channel. The fluid medium annular nozzle is coaxially arranged around the outside of the wire exit hole. The second channel and the fluid medium annular nozzle are inclined towards the central axis of the wire exit hole in the direction of fluid medium flow. The second channel is a tapered channel, with its large end connected to the fluid medium conveying channel and its small end connected to the fluid medium annular nozzle. In this embodiment, the diameter D4 of the fluid medium conveying channel is controlled to be 8.0 mm and the length L4 is 15 mm. The cone angle A5 of the second channel is 45°, the slit width D5 of the fluid medium annular nozzle is 0.8 mm, and the centripetal inclination angle of the second channel and the fluid medium annular nozzle is precisely controlled to be A3=10° and A4=22°. Water at a temperature of 165 ℃ and a pressure of 3.5 MPa is introduced into the fluid medium delivery channel and ejected from the fluid medium annular nozzle to obtain superheated steam, which is used to construct an external high-enthalpy polarity strong charge induction.
[0046] (5) At the expansion cavity and outside the outlet, due to the cliff-like thermodynamic polarity gradient between the peripheral superheated steam and the non-polar HDPE matrix, the in-situ triggered interfacial polarity active capture effect, which strongly pulled the HDPE-g-QAS that was originally entangled in the reactor to rapidly undergo surface flipping and kinetic segregation outward within the millisecond window period at the fiber curing front. Its strongly polar quaternary ammonium salt groups are oriented to be exposed on the outermost layer of the fiber, while the non-polar HDPE root is directly embedded in the stacked lamellar region of HDPE for co-crystallization deadlock, resulting in a quaternary ammonium salt antibacterial fiber membrane.
[0047] Example 2 This embodiment provides a method for preparing a nanoparticle antibacterial fiber membrane, specifically including the following steps: (1) Rigid nano-zinc oxide (ZnO) with an average particle size of 20 nm was vacuum dried at 120 °C for 12 hours; the activated nano-ZnO was mixed with anhydrous xylene at a mass ratio of 10 wt%: 90 wt%, and ultrasonically dispersed for 45 minutes to obtain a uniform nano-ZnO suspension; in another reactor, maleic anhydride-grafted polyethylene (HDPE-g-MAH, in which the mass percentage of maleic anhydride is 1.2 wt%~1.5 wt%) and xylene were mixed at a mass ratio of 16.7 wt%: 83.3 wt%, heated to 130 °C and stirred to dissolve to obtain an HDPE-g-MAH solution; under nitrogen protection, the prepared nano-ZnO suspension and HDPE-g-MAH solution were mixed at a mass ratio of 1:1.8. Specifically, the nano-ZnO suspension was slowly pumped into the HDPE-g-MAH solution, and a high-shear emulsifier (speed 8000 rpm) was turned on and maintained at 130 °C. The reaction was carried out at ℃ for 6 hours, and covalent bond anchoring and coating were achieved by the ring-opening esterification reaction between the hydroxyl groups on the ZnO surface and the macromolecular anhydride ring. After the reaction, the mixture was separated by centrifugation while hot, and the free polymer was removed by repeated ultrasonic washing / centrifugation with hot xylene 3 times. The residue of xylene solvent was removed by washing with anhydrous ethanol 3 times. Finally, the mixture was vacuum dried at 80 ℃ for 24 hours and ground to obtain the surface-modified nano-ZnO composite antibacterial particles (ZnO@HDPE-g-MAH).
[0048] (2) High-density polyethylene (HDPE) and ZnO@HDPE-g-MAH were mixed and dispersed in dichloromethane solvent at a weight ratio of 97.5:2.5. The total solid content was controlled at 11 wt% in a high-pressure dissolution vessel, the temperature was raised to 220 ℃, nitrogen was added and the pressure was stabilized at 10 MPa, and the mixture was stirred at 400 rpm to maintain the high homogeneity of the nanoparticles in the near-critical fluid, thus obtaining a homogeneous precursor solution.
[0049] (3) This embodiment adopts the following Figures 1-3The coaxial nested spinneret device shown is fabricated using a coaxial double-layer nested shell structure. Its interior center has an axially penetrating liquid channel, and a fluid medium channel is provided on the outer side of the liquid channel. The shell contains an axially penetrating liquid channel, which includes, in sequence, an inlet, a pressure-reducing channel, a first channel, a spinneret hole, and an outlet hole. The first channel is a tapered channel, with its larger end connected to the pressure-reducing channel and its smaller end connected to the spinneret hole. The outlet hole is a frustum-shaped outlet hole, with its smaller end connected to the spinneret hole, forming an expanding cavity from the smaller end to the larger end. The diameter and length of the inlet hole are D1' and L1', respectively, with D1' being 1.0 mm. The length-to-diameter ratio (L1' / D1') of the inlet hole is controlled to be 3:1. The length L0 of the pressure-reducing channel is 100 mm, and the diameter D0 is 10 mm. The cone angle A1 of the first channel is set to 110°. The spinneret orifice has a diameter D1 = 1.0 mm and a length-to-diameter ratio L1 / D1 = 2.5:1. The exit orifice dimensions are precisely controlled as follows: D2 = 4.0 mm, D3 = 10 mm, length L2 = 8.0 mm, and cone angle A2 = 30°. The inner wall of the spinneret orifice is perpendicular to the small end face of the exit orifice. A micro-rounded corner is provided at the junction of the small end face of the exit orifice and its inner wall, with the radius R of the micro-rounded corner satisfying: 0.01 mm ≤ R ≤ 0.05 mm. The homogeneous precursor solution is stably input into the liquid channel of the coaxial nested spinneret device, and the homogeneous precursor solution suddenly expands into the expansion cavity of the exit orifice.
[0050] (4) The coaxial nested spinneret device used in this embodiment also has a fluid medium channel inside its housing. The fluid medium channel includes a fluid medium conveying channel and a fluid medium annular nozzle. The fluid medium conveying channel and the fluid medium annular nozzle are connected through a second channel. The fluid medium annular nozzle is coaxially arranged around the outside of the wire exit hole. The second channel and the fluid medium annular nozzle are inclined towards the central axis of the wire exit hole in the direction of fluid medium flow. The second channel is a tapered channel, with its large end connected to the fluid medium conveying channel and its small end connected to the fluid medium annular nozzle. In this embodiment, the diameter D4 of the fluid medium conveying channel is controlled to be 8.0 mm and the length L4 is 15 mm. The cone angle A5 of the second channel is 45°, the slit width D5 of the fluid medium annular nozzle is 0.8 mm, and the centripetal inclination angle of the second channel and the fluid medium annular nozzle is precisely controlled to be A3=10° and A4=22°. Water at a pressure of 3.0 MPa and a temperature of 160 °C is introduced into the fluid medium delivery channel and ejected from the fluid medium annular nozzle to obtain superheated steam, which is used to construct an external high-enthalpy polarity strong charge induction.
[0051] (5) At the expansion cavity and outside the outlet, due to the cliff-like thermodynamic polarity gradient between the peripheral superheated steam and the non-polar HDPE matrix, the in-situ triggered interfacial polarity active capture effect, which strongly pulled the ZnO@HDPE-g-MAH that was originally entangled in the reactor to rapidly undergo surface flipping and kinetic segregation outward within the millisecond window period at the fiber curing front. The ZnO groups were oriented to be exposed on the outermost layer of the fiber, while the non-polar HDPE roots were directly embedded in the stacked lamellar regions of HDPE for co-crystallization deadlock, resulting in a nanoparticle antibacterial fiber membrane.
[0052] Comparative Example 1 This comparative example serves as a control for Example 1, with the fluid medium delivery channel completely shut off. During the dissolving reactor preparation, high-density polyethylene (HDPE) and HDPE-g-QAS were mixed and dissolved in dichloromethane solvent at a weight ratio of 97.5:2.5 to prepare a homogeneous precursor solution with a total solid content of 12 wt%. The temperature inside the high-pressure dissolving reactor was maintained at 220 ℃ and the pressure at 10 MPa. Then, under the condition of completely shutting off the fluid medium delivery channel, the solution was spun into quaternary ammonium salt antibacterial fiber membrane.
[0053] Comparative Example 2 This comparative example serves as a control for Example 2, with the fluid medium delivery channel completely shut off. During the dissolving reactor preparation, high-density polyethylene (HDPE) and ZnO@HDPE-g-MAH were mixed and dispersed in dichloromethane solvent at a weight ratio of 97.5:2.5. In a high-pressure dissolving reactor, the total solid content was controlled at 11 wt%, the temperature was raised to 220 °C, nitrogen was added and the pressure stabilized at 10 MPa, and stirring was maintained at 400 rpm to ensure highly uniform deagglomeration of the nanoparticles in the near-critical fluid, resulting in a homogeneous precursor solution. Then, under conditions of completely shutting off the fluid medium delivery channel, the solution was spun into nanoparticle antibacterial fiber membranes.
[0054] Figure 4 The left image in the image is an electron microscope image of the quaternary ammonium salt antibacterial fiber membrane prepared in Example 1. Figure 4 The right image in the figure is an electron microscope image of the quaternary ammonium salt antibacterial fiber membrane prepared in Comparative Example 1. Figure 5 The left image in the image is an electron microscope image of the nanoparticle antibacterial fiber membrane prepared in Example 2. Figure 5 The right image in the table is an electron microscope image of the nanoparticle antibacterial fiber membrane prepared in Comparative Example 2. Table 1 is a summary of the performance comparison between the functional fiber membranes prepared in Examples 1-2 and Comparative Examples 1-2.
[0055] Table 1. Performance comparison results of functional fiber membranes prepared in Examples 1-2 and Comparative Examples 1-2
[0056] Depend on Figure 4 , Figure 5As shown in Table 1, the mechanical properties and antibacterial properties of the in-situ modified functional fiber membranes prepared by the coaxial nested spinneret device provided by the present invention in Examples 1 and 2 are significantly improved compared with those of Comparative Examples 1 and 2.
[0057] As can be seen from the above embodiments, the coaxial nested spinneret device provided by the present invention can complete functional modification in situ in one step. Utilizing the polar active capture effect generated at the gas-liquid non-equilibrium interface by the high-enthalpy reactive gas flow focused in the fluid medium channel, it induces rapid surface segregation of functional segments within a millisecond-level setting period and completes chemical grafting or activation in situ, eliminating the need for subsequent wet processing steps, simplifying the process flow, and avoiding the damage to the porous framework caused by two-step methods. Because functionalization and film formation are completed simultaneously, the present invention avoids the disordered pulverization of the three-dimensional porous structure caused by subsequent wet-heat soaking. The air-permeable porous network retention rate is ≥96%, and the functional modification layer and the substrate are firmly bonded through co-crystallization, possessing long-lasting resistance to physical washing and responsiveness. The device provided by the present invention achieves a cliff-like drop in the chemical potential of the high-pressure fluid through the sudden expansion of the outlet cavity and strict geometric dimensional constraints, inducing instantaneous solvent evaporation, allowing the fiber strands to form a highly uniform three-dimensional porous cluster network in a very short time, which is beneficial for obtaining fiber membrane products with high tensile strength. The coaxial nested spinneret device provided by this invention integrates multiple functions such as fluid stretching, instantaneous solvent evaporation, interfacial reaction and focusing acceleration. The device has a compact structure, wide applicability, and the geometric parameters of each channel can be adjusted independently. It is suitable for various polymer systems and different reaction gas flow conditions, and is easy to scale up and promote industrially.
[0058] Although the above embodiments have provided a detailed description of the present invention, they are only some embodiments of the present invention, and not all embodiments. Other embodiments can be obtained based on these embodiments without creative effort, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A coaxial nested spinneret device, characterized in that, The device includes a housing, within which an axially penetrating liquid channel is provided. The liquid channel includes, in sequence, an inlet hole, a pressure-reducing channel, a first channel, a spinneret hole, and an outlet hole. The first channel is a tapered channel, with its larger end connected to the pressure-reducing channel and its smaller end connected to the spinneret hole. The outlet hole is a frustum-shaped outlet hole, with its smaller end connected to the spinneret hole, forming an expanding cavity from the smaller end to the larger end. The housing also includes a fluid medium channel, which comprises a fluid medium delivery channel and a fluid medium annular nozzle. The fluid medium delivery channel and the fluid medium annular nozzle are connected through a second channel. The fluid medium annular nozzle is coaxially arranged around the outside of the wire exit hole. The second channel and the fluid medium annular nozzle are inclined towards the central axis of the wire exit hole in the direction of fluid medium flow. The second channel is a tapered channel, with its large end connected to the fluid medium delivery channel and its small end connected to the fluid medium annular nozzle.
2. The coaxial nested spinneret device according to claim 1, characterized in that, The cone angle A1 of the first channel satisfies: 120°>A1>100°; the diameter and length of the spinneret are D1 and L1 respectively, satisfying: 0.5 mm≤D1≤2 mm, 1:1≤L1 / D1≤4:1; the small port diameter of the wire exiting hole is D2, the large port diameter is D3, the length is L2, and the cone angle is A2, satisfying: 3 mm≤D2≤6 mm, 9 mm≤D3≤12 mm, L2 / D3<L2 / D2≤2, 20° <A2≤45°。 3. The coaxial nested spinneret device according to claim 1, characterized in that, The diameter and length of the liquid inlet are D1' and L1', respectively, satisfying: 1 mm ≤ D1' ≤ 3 mm, 1:1 ≤ L1' / D1' ≤ 3:
1.
4. The coaxial nested spinneret device according to claim 1 or 2, characterized in that, The fluid medium conveying channel is provided in multiple ways, and each fluid medium conveying channel is evenly distributed circumferentially on the housing; the inclination angle of the second channel relative to the central axis is A4, and the inclination angle of the fluid medium annular nozzle relative to the central axis is A3, satisfying: 30°>A4>A3>3°; the cone angle A5 of the second channel satisfies: 60°>A5>30°; the diameter of the fluid medium conveying channel is D4, and the slit width of the fluid medium annular nozzle is D5, satisfying: 5 mm≤D4≤10 mm, 0.5 mm≤D5≤1.5 mm.
5. The coaxial nested spinneret device according to claim 1 or 2, characterized in that, The inner wall of the spinneret is perpendicular to the small end face of the wire exiting hole; a micro-rounded corner is provided at the junction of the small end face of the wire exiting hole and its inner wall, and the radius R of the micro-rounded corner satisfies: 0.01 mm ≤ R ≤ 0.05 mm.
6. The coaxial nested spinneret device according to claim 1, characterized in that, The inlet end of the fluid medium delivery channel is connected to the fluid medium generation system; the fluid medium generation system includes a microchannel heat exchange unit, the microchannel heat exchange unit is equipped with a heating jacket, and a metering pump is installed on the feed inlet pipe of the microchannel heat exchange unit.
7. A method for preparing an in-situ modified functional fiber membrane, characterized in that, The process, performed using the coaxial nested spinneret device according to any one of claims 1 to 6, includes the following steps: A fluid medium is introduced into the fluid medium channel, and after flowing through the fluid medium delivery channel, it is ejected through the fluid medium annular nozzle. A homogeneous precursor solution, containing functional side chains and / or functional monomers, is introduced into the liquid channel through the inlet hole. After flowing through the depressurization channel, it is ejected into the expansion cavity of the spinneret hole through the spinneret hole. After the fluid medium ejected from the fluid medium annular nozzle and the homogeneous precursor solution ejected from the spinneret hole meet, the fluid medium modifies the homogeneous precursor solution in situ. Then, it is deposited on the receiving grid with the flow field to obtain the in-situ modified functional fiber membrane.
8. The preparation method according to claim 7, characterized in that, The fluid medium ejected from the annular nozzle can be in the form of superheated active chemical fluid, superheated steam, or reactive monomer aerosol fluid.
9. The preparation method according to claim 7 or 8, characterized in that, The pressure of the fluid medium input into the fluid medium channel is 2~4MPa, and the temperature is 150~180℃.
10. The preparation method according to claim 7, characterized in that, The in-situ modification includes surface segregation and / or in-situ activation reactions of functional side chains and / or functional monomers in a homogeneous precursor solution. The in-situ activation reactions include one or more of the following: in-situ graft polymerization, in-situ ring-opening hydrolysis, and in-situ acid-base neutralization reactions.