A method for spinning PAN-based carbon fiber precursor
By combining a five-stage gradient coagulation bath and an in-situ plasticizing bath, the problems of uneven solvent diffusion and high energy consumption in the spinning process of PAN-based carbon fiber precursor were solved, and high-performance, low-energy carbon fiber precursor production was achieved.
Patent Information
- Application Number
- CN202611529033.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-30
- Publication Date
- 2026-11-17
AI Technical Summary
Existing PAN-based carbon fiber precursor spinning processes suffer from problems such as an imbalance between solvent diffusion and non-solvent penetration rates, differences in core-sheath structure, high energy consumption, and high production costs, making it difficult to achieve high-performance, low-cost mass production.
A spinning method employing a five-stage gradient coagulation bath combined with an in-situ plasticizing bath reduces production energy consumption and minimizes internal structural defects in the raw yarn by progressively adjusting solvent concentration and temperature and combining multi-stage thermal stretching.
It significantly improves the tensile strength and modulus of the precursor, reduces production energy consumption, simplifies the process, and is suitable for the large-scale production of high-performance PAN-based carbon fiber precursor.
Smart Images

Figure CN123108751A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the technical field of carbon fiber preparation, and in particular to a method for spinning PAN-based carbon fiber precursor. Background Technology
[0002] Polyacrylonitrile (PAN)-based carbon fibers have been widely used in aerospace, new energy wind power, and high-end equipment manufacturing due to their excellent properties such as high specific strength, high specific modulus, and corrosion resistance. As the precursor of carbon fibers, the uniformity of the internal structure, the content of defects, and the degree of molecular orientation directly determine the mechanical properties and product quality of the final carbon fibers, and the spinning process is the key link in controlling the structure of the precursor fibers.
[0003] Currently, the mainstream industrial spinning processes for PAN-based precursor fibers are wet spinning and dry-jet wet spinning. These traditional processes generally use a single-concentration coagulation bath for coagulation and forming, which has many technical drawbacks: First, the large difference between solvent and non-solvent concentrations in the single coagulation bath causes an imbalance between solvent diffusion and non-solvent penetration rates during the coagulation process of the PAN spinning solution, easily leading to the formation of a large number of irregular micropores inside the precursor fiber, resulting in significant differences in the core-sheath structure and numerous fiber defects and large strength dispersion after subsequent carbonization. Second, to improve molecular orientation, traditional processes require a separate high-temperature steam drawing or hot water bath drawing process, which results in high energy consumption, easy fiber breakage during drawing, and uneven precursor fiber fineness. Third, the high solvent residue in the precursor fiber leads to large water consumption and long processing time in the subsequent washing process, further increasing production costs and making it difficult to meet the demand for low-cost, high-quality, large-scale production of high-performance carbon fiber precursor fibers.
[0004] While existing technologies include some research on coagulation bath optimization and spinning plasticization to address the aforementioned issues, none have achieved the synergistic coupling of gradient solvent replacement and in-situ plasticization. This fails to fundamentally solve industry pain points such as numerous defects in the raw fiber forming process, high energy consumption in post-processing, and poor performance stability. Therefore, there is an urgent need to develop a novel spinning method to overcome the bottlenecks of current technologies. Summary of the Invention
[0005] The technical problem to be solved by the present invention is to provide a spinning preparation method for PAN-based carbon fiber precursor in order to overcome the shortcomings of the prior art. The method achieves a smooth diffusion exchange between solvent and non-solvent through a five-level gradient coagulation bath and combines it with multi-level thermal stretching in an in-situ plasticizing bath. This method can reduce internal structural defects of the precursor while reducing production energy consumption and is suitable for large-scale continuous production of high-performance, low-energy-consumption PAN-based carbon fiber precursor.
[0006] The technical solution adopted by this invention to solve its technical problem is: a method for preparing PAN-based carbon fiber precursor by spinning, comprising the following steps:
[0007] S1: PAN polymer is dissolved in dimethyl sulfoxide to prepare a spinning solution; wherein, the acrylonitrile content of the PAN raw material is 29% and the itaconic acid content is 8%. The molecular weight distribution index (PDI) of PAN is ≤2.0.
[0008] S2: The spinning solution is extruded through a spinneret and then passed through a five-stage gradient coagulation bath for solidification and shaping. The solvent concentration in the five-stage gradient coagulation bath decreases step by step to obtain the nascent filament.
[0009] S3: The nascent raw yarn is introduced into the in-situ plasticizing bath located at the outlet of the final coagulation bath. The in-situ plasticizing bath contains polyethylene glycol and propylene glycol. During plasticizing, multi-stage thermal stretching is performed, with a total stretching ratio of 2 to 3 times.
[0010] S4: The drawn precursor yarn is sequentially washed, dried, oiled, dried and densified, and then coiled to obtain PAN-based carbon fiber precursor yarn.
[0011] Furthermore, in S2, the five-stage gradient coagulation bath is a dimethyl sulfoxide aqueous solution, and the solvent concentrations of the first to fifth stages are 50%~60%, 30%~40%, 20%~30%, 15%~20%, and 10%~15%, respectively.
[0012] Furthermore, in S2, the temperatures of the five-stage gradient coagulation baths are 70~80℃, 60~70℃, 70~80℃, 75~85℃, and 80~90℃ respectively, and the residence time of each coagulation bath is 8~12 seconds.
[0013] Furthermore, in S3, the mass concentration of polyethylene glycol in the in-situ plasticizing bath is 5%~10%, the mass concentration of propylene glycol is 2%~5%, and the temperature of the plasticizing bath is 40~45℃.
[0014] Furthermore, in S3, the stretching rate of the multi-stage thermal stretching is 17~22 m / min.
[0015] Furthermore, in S3, the multi-stage thermal drawing is a two-stage thermal drawing, with the first stage drawing ratio being 1.4 to 1.7 times and the second stage drawing ratio being 1.4 to 1.7 times, and the product of the first stage drawing ratio and the second stage drawing ratio being 2 to 3 times.
[0016] Furthermore, in S1, the viscosity-average molecular weight of the PAN polymer is 17.25 × 10⁻⁶. 4 ~24.75×10 4 The solid content of the spinning solution is 16%~22%, the desizing and defoaming temperature is 45~55℃, and the time is 60~90 minutes.
[0017] Furthermore, in S4, the water washing is a three-stage countercurrent water washing, with water washing temperatures of 55℃, 45℃, and 35℃ respectively, and a total water washing time of 20~25 minutes; the drying is hot air drying, with a temperature of 60~70℃ and a time of 10~15 minutes.
[0018] Furthermore, in S4, the drying and densification process is carried out in five temperature zones, with temperatures of 80~90℃, 90~100℃, 100~120℃, 110~120℃, and 120~130℃ respectively, and a total processing time of 8~10 minutes; the winding tension for curling is 0.9~1.2cN / dtex.
[0019] Furthermore, in S4, a special nonionic spinning oil for carbon fiber is used for oiling. The concentration of the oil bath is 1%~2%, the temperature of the oil bath is 30~40℃, the oiling time is 5~7 seconds, and the oiling rate of the raw yarn is controlled at 1%~1.5%.
[0020] The present invention also provides a PAN-based carbon fiber precursor, which is prepared by a spinning method for PAN-based carbon fiber precursor, and the moisture content of the PAN-based carbon fiber precursor is ≤1.5%.
[0021] The beneficial effects of this invention are as follows: This invention employs a five-stage gradient coagulation bath, achieving smooth coagulation through a gradual decrease in solvent concentration, effectively reducing micropores and core-sheath structural defects within the raw yarn, resulting in a significant improvement in both tensile strength and tensile modulus. An in-situ plasticizing bath is set at the outlet of the final coagulation bath, utilizing the synergistic plasticizing effect of polyethylene glycol and propylene glycol to achieve high-ratio drawing at a lower temperature, eliminating the need for traditional high-temperature steam drawing, significantly reducing production energy consumption, and simplifying the process flow. Both polyethylene glycol and propylene glycol are water-soluble, allowing for thorough removal through subsequent washing without interfering with subsequent processes such as pre-oxidation and carbonization. The invention has a wide range of process parameters and moderate equipment requirements, enabling technological upgrades by adding an in-situ plasticizing bath to existing wet or dry-jet wet spinning production lines, and possesses excellent prospects for industrial application. Attached Figure Description
[0022] Figure 1 This is a flowchart of a spinning preparation method for PAN-based carbon fiber precursor according to the present invention. Detailed Implementation
[0023] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0024] See Figure 1 The present invention discloses a method for spinning PAN-based carbon fiber precursor, comprising the following steps:
[0025] S1: The PAN polymer was dissolved in dimethyl sulfoxide to prepare a spinning solution. The viscosity-average molecular weight of the PAN polymer was 17.25 × 10⁻⁶. 4 ~24.75×10 4 The solid content of the spinning solution is 16%~22%, preferably 18%~20%. The degassing temperature is 45~55℃, and the time is 60~90 minutes to remove air bubbles and impurities from the solution, ensuring its uniformity and stability. If the solid content is below 16%, the viscosity of the spinning solution is too low, making it difficult for the fine stream to solidify and form, resulting in insufficient fiber strength; if the solid content is above 22%, the viscosity is too high, making degassing difficult and increasing spinneret resistance. Degassing efficiency is low below 45℃, and temperatures above 55℃ may cause thermal degradation of the PAN polymer.
[0026] S2: The spinning solution is extruded through a spinneret and then coagulated in a five-stage gradient coagulation bath. The solvent concentration in each stage of the coagulation bath decreases progressively, resulting in nascent precursor fibers. The five-stage gradient coagulation bath is an aqueous solution of dimethyl sulfoxide (DMSO), with solvent concentrations of 50%–60%, 30%–40%, 20%–30%, 15%–20%, and 10%–15% for the first to fifth stages, respectively. The use of a five-stage gradient instead of two or three stages is based on the inventors' research finding that fewer than five stages result in a large concentration gradient span, leading to premature solidification of the skin layer; more than five stages significantly increase equipment costs while performance improvement tends to saturate, resulting in decreased economic efficiency. The residence time in each coagulation bath is 8–12 seconds. If the residence time is less than 8 seconds, double diffusion is insufficient, leaving a large amount of solvent residue inside the precursor fiber; if it exceeds 12 seconds, over-coagulation increases the brittleness of the nascent precursor fiber, making it prone to breakage during subsequent drawing. The temperatures of the five-stage coagulation bath are 70–80℃, 60–70℃, 70–80℃, 75–85℃, and 80–90℃, respectively. The coordinated matching of temperature and concentration at each stage is crucial. High temperatures help suppress excessive penetration of non-solvents during coagulation, working in conjunction with the gradient concentration to achieve smooth coagulation. If the coagulation bath temperature exceeds the above range, the solvent diffusion rate and non-solvent penetration rate will become unbalanced, still resulting in differences in the core-skin structure.
[0027] S3: The nascent precursor fiber is introduced into an in-situ plasticizing bath located at the outlet of the final coagulation bath. This bath contains polyethylene glycol (PEG) and propylene glycol, and multi-stage hot stretching is performed simultaneously with plasticizing, with a total stretching ratio of 2-3 times. The PEG concentration in the in-situ plasticizing bath is 5%-10%, and the propylene glycol concentration is 2%-5%. The bath temperature is 40-45°C. The PEG to propylene glycol ratio has been optimized. If the bath temperature is below 40°C, the plasticizing effect is insufficient, resulting in inadequate flexibility of the nascent precursor fiber, making it prone to breakage during high stretching. If the temperature is above 45°C, the plasticizer penetrates too quickly, potentially leading to over-plasticization of the fiber surface and insufficient plasticization of the core, while also increasing energy consumption. If the PEG concentration is below 5%, core plasticization is insufficient, and the movement of macromolecular chain segments is restricted; if it is above 10%, the viscosity of the plasticizing bath is too high, which is not conducive to uniform wetting of the precursor fiber. If the propylene glycol concentration is below 2%, the surface plasticizing effect is insufficient; if it is above 5%, over-plasticization may occur, leading to a sticky surface on the precursor fiber and affecting the drawing stability. The total draw ratio is 2-3 times, and the drawing rate is 17-22 m / min. Multi-stage hot drawing consists of two stages: the first stage draw ratio is 1.4-1.7 times, and the second stage draw ratio is also 1.4-1.7 times. The distribution of the two draw ratios is determined based on the specific total draw ratio, with the principle of relatively balanced drawing deformation at each stage. If the total draw ratio is below 2 times, the molecular orientation is insufficient, resulting in low precursor fiber strength and modulus; if it is above 3 times, the drawing stress is too high, and the precursor fiber is prone to breakage.
[0028] S4: The drawn precursor yarn is sequentially washed, dried, oiled, dried and densified, and then coiled to obtain PAN-based carbon fiber precursor yarn. The washing process is a three-stage counter-current washing, with washing temperatures of 55℃, 45℃, and 35℃ respectively, for a total washing time of 20-25 minutes. The gradient design of the washing temperature allows the precursor yarn to cool gradually, avoiding thermal stress defects caused by excessive temperature differences. A washing time of less than 20 minutes results in insufficient removal of plasticizers and solvents, and the residues will interfere with subsequent pre-oxidation and carbonization processes; a washing time of more than 25 minutes reduces production efficiency, increases energy consumption, and prolonged immersion may cause swelling and damage to the internal structure of the precursor yarn. Drying is done with hot air at 60-70℃ for 10-15 minutes, controlling the moisture content of the precursor yarn to below 1.5%. Drying temperatures below 60℃ result in low drying efficiency and difficulty in achieving the required moisture content; temperatures above 70℃ may cause the raw yarn surface to lose water too quickly, forming a hard skin layer and affecting subsequent densification. The oiling process uses a special non-ionic spinning oil for carbon fiber, with an oil bath concentration of 1%~2%, an oil bath temperature of 30~40℃, and an oiling time of 5~7 seconds, controlling the oiling rate of the raw yarn at 1%~1.5%. An oiling rate below 1% results in insufficient yarn bundle cohesion, easily leading to fuzz formation in subsequent processing; a rate above 1.5% results in excessive oil residue, potentially affecting the performance of the carbonized fiber. The drying and densification process involves five temperature zones: 80~90℃, 90~100℃, 100~120℃, 110~120℃, and 120~130℃, with a total processing time of 8~10 minutes. This gradient heating across the five zones gradually evaporates residual solvent and moisture from the raw yarn, simultaneously achieving fiber densification. If the temperature gradient is too steep or the temperature in a certain zone exceeds the above range, the rapid evaporation rate of moisture and solvent may cause pore defects to form inside the raw yarn. The winding tension for crimping is 0.9~1.2 cN / dtex. If the winding tension is lower than 0.9 cN / dtex, the raw yarn will be loosely wound and poorly formed; if it is higher than 1.2 cN / dtex, it may cause additional tensile stress in the raw yarn during the winding process, affecting the uniformity of fineness.
[0029] Example 1:
[0030] A viscosity-average molecular weight of 17.25 × 10⁻⁶ was selected. 4 ~24.75×10 4PAN polymer was used as a solvent to prepare a spinning solution with a solid content of 20%, and degassing was carried out at 50℃ for 75 min. Five-stage gradient coagulation baths were used with concentrations of 55%, 35%, 25%, 15%, and 12%, and temperatures of 75℃, 65℃, 75℃, 80℃, and 85℃, respectively, with each stage lasting 10 s to obtain nascent precursor fibers. A plasticizing bath containing 8% polyethylene glycol and 4% propylene glycol was used at 43℃, with a total draw ratio of 2.55 times and a draw rate of 20 m / min, where the first stage draw ratio was 1.5 times and the second stage draw ratio was 1.7 times. Three-stage washing was performed at temperatures of 55℃, 45℃, and 35℃, with a total washing time of 25 min. Hot air drying was carried out at 65℃ for 15 min. The oiling process used an oil concentration of 1.5%, an oiling temperature of 35℃, and an oiling time of 6 s. The drying and densification processes were carried out at five temperature zones: 85℃, 95℃, 110℃, 115℃, and 125℃, with a total processing time of 9 minutes. The winding tension was 1 cN / dtex, and the PAN-based precursor fibers were collected.
[0031] Example 2:
[0032] A viscosity-average molecular weight of 17.25 × 10⁻⁶ was selected. 4 ~24.75×10 4 PAN polymer was used as a solvent to prepare a spinning solution with a solid content of 18%, and degassing was carried out at 50℃ for 75 min. Five-stage gradient coagulation baths were used, with concentrations of 52%, 32%, 22%, 12%, and 10%, and temperatures of 70℃, 60℃, 70℃, 75℃, and 80℃, respectively. Each coagulation bath was held for 10 s to obtain nascent precursor fibers. The plasticizing bath contained 7% polyethylene glycol and 3% propylene glycol, at a temperature of 43℃, a total draw ratio of 2.55, and a draw rate of 20 m / min, with the first stage draw ratio at 1.5 and the second stage at 1.7. Three-stage washing was performed at temperatures of 55℃, 45℃, and 35℃, with a total washing time of 25 min. Hot air drying was carried out at 65℃ for 15 min. The oiling process involved an oil concentration of 1.2%, an oiling temperature of 35℃, and an oiling time of 6 s. The drying and densification processes were carried out at five temperature zones: 85℃, 95℃, 110℃, 115℃, and 125℃, with a total processing time of 9 minutes. The winding tension was 1 cN / dtex, and the PAN-based precursor fibers were collected.
[0033] Example 3:
[0034] A viscosity-average molecular weight of 17.25 × 10⁻⁶ was selected. 4 ~24.75×10 4PAN polymer was used as a solvent to prepare a spinning solution with a solid content of 25%, and degassing was carried out at 50℃ for 75 min. Five-stage gradient coagulation baths were used, with concentrations of 60%, 40%, 30%, 20%, and 15%, and temperatures of 80℃, 70℃, 80℃, 85℃, and 90℃, respectively. Each coagulation bath was held for 10 s to obtain nascent precursor fibers. A plasticizing bath containing 10% polyethylene glycol and 5% propylene glycol was used at 43℃, with a total draw ratio of 2.55 and a draw rate of 20 m / min, where the first stage draw ratio was 1.5 times and the second stage draw ratio was 1.7 times. Three-stage washing was performed at temperatures of 55℃, 45℃, and 35℃, with a total washing time of 25 min. Hot air drying was carried out at 65℃ for 15 min. The oiling process involved an oil concentration of 1.8%, an oiling temperature of 35℃, and an oiling time of 6 s. The drying and densification processes were carried out at five temperature zones: 85℃, 95℃, 110℃, 115℃, and 125℃, with a total processing time of 9 minutes. The winding tension was 1 cN / dtex, and the PAN-based precursor fibers were collected.
[0035] Comparative Example 1:
[0036] A viscosity-average molecular weight of 17.25 × 10⁻⁶ was selected. 4 ~24.75×10 4 PAN polymer was used as a solvent to prepare a spinning solution with a solid content of 25%, and degassing was carried out at 50℃ for 75 min. Five-stage gradient coagulation baths were used with concentrations of 60%, 40%, 30%, 20%, and 15%, and temperatures of 80℃, 70℃, 80℃, 85℃, and 90℃, with each stage lasting 10 s, to obtain nascent precursor fibers. The nascent precursor fibers underwent three stages of water washing at temperatures of 55℃, 45℃, and 35℃, for a total time of 25 min; hot air drying at 65℃ for 15 min; oiling agent with a concentration of 1.8% at 35℃ for 6 s; and drying and densification at five temperature zones of 85℃, 95℃, 110℃, 115℃, and 125℃ for a total treatment time of 9 min; steam drawing pressure was 0.26 MPa, steam drawing ratio was 2.2; and the winding tension was 1 cN / dtex to collect the PAN-based precursor fibers. The only difference between Comparative Example 1 and Example 3 is the stretching method. Comparative Example 1 uses steam stretching, while Example 3 uses in-situ plasticizing stretching. All other process parameters are exactly the same.
[0037] Comparative Example 2:
[0038] A viscosity-average molecular weight of 17.25 × 10⁻⁶ was selected. 4 ~24.75×10 4PAN polymer was used as a solvent to prepare a spinning solution with a solid content of 25%, and degassing was carried out at 50°C for 75 min. A single-stage coagulation bath was used with a concentration of 30%, a temperature of 80°C, and a residence time of 50 s to obtain nascent precursor fibers. The plasticizing bath contained 10% polyethylene glycol and 5% propylene glycol, with a temperature of 43°C, a total draw ratio of 2.55, and a draw rate of 20 m / min, of which the first stage draw was 1.5 times and the second stage draw was 1.7 times. The three-stage washing temperatures were 55℃, 45℃, and 35℃, with a total washing time of 25 minutes; the hot air drying temperature was 65℃, and the time was 15 minutes; the oiling process had an oil concentration of 1.8%, an oiling temperature of 35℃, and an oiling time of 6 seconds; the drying and densification processes had five temperature zones of 85℃, 95℃, 110℃, 115℃, and 125℃, with a total processing time of 9 minutes; the winding tension was 1 cN / dtex, and PAN-based raw yarn was collected. Comparative Example 2 and Example 3 differed only in the number of coagulation bath stages. Comparative Example 2 used a single-stage coagulation bath, while Example 3 used a five-stage gradient coagulation bath; all other process parameters were identical. In Comparative Example 2, the residence time in the single-stage coagulation bath was 50 seconds, while in the five-stage gradient coagulation bath, each stage had a residence time of 10 seconds, with a total time of 50 seconds. This demonstrates a comparison of the performance differences between the two coagulation methods under the premise of the same total coagulation time.
[0039] The tensile strength and tensile modulus were tested in accordance with GB / T 1446-2005 "General Rules for Test Methods of Fiber Reinforced Plastics"; the linear density was tested in accordance with GB / T 3362-2017 "Test Method for Tensile Properties of Carbon Fiber Multifilament"; and the boiling water shrinkage rate was tested in accordance with GB / T 6505-2017 "Test Method for Heat Shrinkage Rate of Chemical Fiber Filaments" (after treatment).
[0040] Table 1 Summary of performance data for each embodiment and comparative example
[0041] Sample / Performance Tensile strength tensile modulus Linear density Boiling water shrinkage rate Example 1 6.9 cN / dtex 144 cN / dtex 0.4881 g / m 5.72% Example 2 7.2 cN / dtex 177 cN / dtex 0.4842 g / m 5.60% Example 3 7.7 cN / dtex 210 cN / dtex 0.4887 g / m 5.42% Comparative Example 1 6.6 cN / dtex 144 cN / dtex 0.4852 g / m 5.66% Comparative Example 2 5.9 cN / dtex 157 cN / dtex 0.4861 g / m 5.51%
[0042] As shown in Table 1, the only difference between Comparative Example 1 and Example 3 is the drawing method; Comparative Example 1 uses traditional steam drawing, while Example 3 uses in-situ plasticizing bath drawing. The tensile strength of Example 3 is 7.7 cN / dtex, and the tensile modulus is 210 cN / dtex, both significantly better than the tensile strength of Comparative Example 1 (6.6 cN / dtex) and the tensile modulus (144 cN / dtex). The linear density and boiling water shrinkage rate show little change, indicating that using in-situ plasticizing bath drawing instead of steam drawing can improve the performance of the raw yarn while reducing production energy consumption.
[0043] The only difference between Comparative Example 2 and Example 3 is the number of coagulation bath stages. Comparative Example 2 uses a single-stage coagulation bath with a residence time of 50 seconds, while Example 3 uses a five-stage gradient coagulation bath with a residence time of 10 seconds per stage, for a total residence time of 50 seconds. Under the premise of the same total coagulation time, the tensile strength of Example 3 is 7.7 cN / dtex, significantly better than the 5.9 cN / dtex of Comparative Example 2. This demonstrates that the five-stage gradient coagulation bath of this application effectively reduces internal structural defects in the precursor fiber and improves its mechanical properties through a smooth solvent-non-solvent exchange process.
[0044] Based on actual production statistics, the energy consumption per unit product for the two drawing methods is compared as follows:
[0045] Stretch type Energy consumption (kWh / t of primary fiber) In-situ plasticizing stretching (this application) 72 Steam drawing (traditional process) 142
[0046] The unit product energy consumption of in-situ plasticizing stretching is about 50% of that of traditional steam stretching, which has a significant energy-saving effect and fully verifies the technical effect of reducing production energy consumption in this application.
[0047] The above are merely preferred embodiments of the present invention, but the scope of protection of the present invention is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the scope of the technology disclosed in the present invention, based on the technical solution and inventive concept of the present invention, should be covered within the scope of protection of the present invention.
Claims
1. A method for spinning PAN-based carbon fiber precursor, characterized in that, Includes the following steps: S1: Dissolve PAN polymer in dimethyl sulfoxide to prepare a spinning solution; S2: The spinning solution is extruded through a spinneret and then passed through a five-stage gradient coagulation bath for solidification and shaping. The solvent concentration of the five-stage gradient coagulation bath decreases step by step to obtain nascent raw yarn. S3: The nascent filament is introduced into an in-situ plasticizing bath located at the outlet of the final stage coagulation bath. The in-situ plasticizing bath contains polyethylene glycol and propylene glycol. During plasticizing, multi-stage thermal stretching is performed, with a total stretching ratio of 2 to 3 times. S4: The drawn precursor yarn is sequentially washed, dried, oiled, dried and densified, and then coiled to obtain PAN-based carbon fiber precursor yarn.
2. The method for preparing PAN-based carbon fiber precursor by spinning according to claim 1, characterized in that, In S2, the five-stage gradient coagulation bath is a dimethyl sulfoxide aqueous solution, and the solvent concentrations of the first to fifth stages are 50%~60%, 30%~40%, 20%~30%, 15%~20%, and 10%~15%, respectively.
3. The method for preparing PAN-based carbon fiber precursor by spinning according to claim 1 or 2, characterized in that, In S2, the temperatures of the five-stage gradient coagulation baths are 70~80℃, 60~70℃, 70~80℃, 75~85℃, and 80~90℃ respectively, and the residence time of each coagulation bath is 8~12 seconds.
4. The method for preparing PAN-based carbon fiber precursor by spinning according to claim 1, characterized in that, In S3, the mass concentration of polyethylene glycol in the in-situ plasticizing bath is 5%~10%, the mass concentration of propylene glycol is 2%~5%, and the temperature of the plasticizing bath is 40~45℃.
5. The method for preparing PAN-based carbon fiber precursor by spinning according to claim 1, characterized in that, In S3, the stretching rate of the multi-stage thermal stretching is 17~22 m / min.
6. The method for preparing PAN-based carbon fiber precursor by spinning according to claim 1, characterized in that, In S3, the multi-stage thermal stretching is a two-stage thermal stretching, with the first stage stretching ratio being 1.4 to 1.7 times and the second stage stretching ratio being 1.4 to 1.7 times, and the product of the first stage stretching ratio and the second stage stretching ratio being 2 to 3 times.
7. The method for preparing PAN-based carbon fiber precursor by spinning according to claim 1, characterized in that, In S1, the viscosity-average molecular weight of the PAN polymer is 17.25 × 10⁻⁶. 4 ~24.75×10 4 The solid content of the spinning solution is 16%~22%, the desizing and defoaming temperature is 45~55℃, and the time is 60~90 minutes.
8. The method for preparing PAN-based carbon fiber precursor by spinning according to claim 1, characterized in that, In S4, the water washing is a three-stage countercurrent water washing, with water washing temperatures of 55℃, 45℃, and 35℃ respectively, and a total water washing time of 20~25 minutes; the drying is hot air drying, with a temperature of 60~70℃ and a time of 10~15 minutes.
9. The method for preparing PAN-based carbon fiber precursor by spinning according to claim 1, characterized in that, In S4, the drying and densification is carried out in five temperature zones, with temperatures of 80~90℃, 90~100℃, 100~120℃, 110~120℃, and 120~130℃ respectively, and a total processing time of 8~10 minutes; the winding tension of the curling forming is 0.9~1.2cN / dtex.
10. A PAN-based carbon fiber precursor, characterized in that, It is prepared by the spinning method of any one of claims 1 to 9.