An aerogel fiber wet spinning device and a method for preparing aerogel fibers

By designing a wet spinning equipment for aerogel fibers and using pneumatic drive and multi-stage coagulation bath treatment, continuous production of aerogel fibers throughout the entire process was achieved. This solved the problem of achieving a porous skin structure and a dense core orientation in existing technologies, and produced aerogel fibers with high strength and low thermal conductivity.

CN123108752APending Publication Date: 2026-11-17SHANGHAI SAZHUOKEFANG INSTRUMENT EQUIPMENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611593293.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-14
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing aerogel fiber preparation processes cannot achieve continuous production throughout the entire process, and it is difficult to simultaneously achieve the formation of porous skin structure and densification orientation of core layer during continuous fiber forming, which limits the continuous and large-scale preparation of high-strength aerogel fibers.

Method used

Design a wet spinning equipment for aerogel fibers, including a gas control device, a liquid storage spinning device, a multi-stage coagulation device, a drying device, and a winding and collecting device. Employ pneumatic drive, coaxial spinning, multi-stage coagulation bath, and high and low temperature gradient temperature treatment to achieve continuous production of cross-scale aerogel fibers with porous skin and dense core.

Benefits of technology

It has achieved continuous production of aerogel fibers throughout the entire process, with tensile strength reaching 80~160 MPa and thermal conductivity of 0.018~0.098 W/(m·K). It possesses excellent mechanical properties and thermal insulation properties, and is suitable for high-performance aerogel fibers and composite functional fiber materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108752A_ABST
    Figure CN123108752A_ABST
Patent Text Reader

Abstract

The application belongs to the technical field of polymer fiber preparation and aerogel fiber forming, and particularly relates to an aerogel fiber wet spinning equipment and a method for preparing aerogel fibers. The aerogel fiber wet spinning equipment comprises a gas control device, a liquid storage spinning device, a coagulation device, a drying device and a winding and collecting device arranged in sequence along a spinning direction. The equipment can realize the synergistic effect of high-low temperature gradient temperature coagulation and high-temperature bath drawing, and form a cross-scale multi-level structure with a porous skin layer and a dense core layer. The skin layer has a loose porous structure and meets the heat insulation performance and functionalization requirements. The core layer is a dense network and bears the main mechanical load, and the tensile strength reaches 80-160 MPa, and the thermal conductivity is as low as 0.018-0.098 W / (m.K). The application realizes the large-scale continuous and stable production of high-strength aerogel fibers, and can be widely applied to the preparation of high-performance aerogel fibers, composite functional fibers and advanced thermal insulation materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of polymer fiber preparation and aerogel fiber molding technology, specifically relating to a wet spinning equipment for aerogel fibers and a method for preparing aerogel fibers. Background Technology

[0002] Aerogel fibers possess the dual properties of both flexible fiber materials and aerogel materials, showing significant application potential in flexible thermal insulation, aerospace thermal protection, and high-end textiles. Currently, aerogel fibers are mainly prepared through wet spinning combined with post-processing techniques such as freeze-drying and supercritical drying. However, existing preparation processes largely rely on intermittent post-processing steps, making it difficult to achieve continuous production throughout the entire process. For example, the team of Zhuang Xupin and Yang Guang at Tianjin University of Technology used a two-step coagulation method of "rapid gelation in formic acid → slow gelation in water" to prepare aramid aerogel fibers (Adv. Funct. Mater. 2025), forming a "dense skin-porous core" structure, but this requires intermittent treatment such as supercritical drying. Similarly, the team of Liu Tianxi and Fan Wei at Jiangnan University used coaxial wet spinning combined with thermal imidization to prepare polyimide aerogel fibers (Adv. Fiber Mater. 2025). After fiber solidification, it requires roller collection, step-by-step drying, and thermal imidization, also involving intermittent freeze-drying steps, making continuous production throughout the entire process impossible. Moreover, current wet spinning equipment and aerogel fiber preparation processes cannot simultaneously achieve the formation of a porous skin structure and the densification and orientation of the core layer during the continuous fiber forming process, which further restricts the continuous and large-scale preparation of high-strength aerogel fibers. Summary of the Invention

[0003] In view of this, the purpose of this invention is to provide a wet spinning apparatus for aerogel fibers and a method for preparing aerogel fibers. This invention provides a wet spinning apparatus for aerogel fibers that can achieve the formation of a porous skin structure and the densification and orientation of the core layer, producing aerogel fibers with a "porous skin and dense core" structure, and enabling continuous production of high-strength aerogel fibers throughout the entire process.

[0004] The present invention provides a wet spinning equipment for aerogel fibers, including a gas control device, a liquid storage spinning device 3, and a multi-stage coagulation device, a drying device 14 and a winding and collecting device 15 arranged sequentially along the spinning direction; The gas control device includes a gas supply unit 1 and a gas pressure control unit 2; The spinning device 3 includes a spinning solution storage tank, a coaxial spinneret 312, and a first temperature control unit 4 connected to the spinning solution storage tank; the spinning solution storage tank includes a core layer spinning solution storage tank 33 and a skin layer spinning solution storage tank 34, which are respectively connected to the core layer channel and the skin layer channel of the coaxial spinneret; both the core layer spinning solution storage tank and the skin layer spinning solution storage tank are provided with air inlets at the top, which are connected to the gas output pipeline of the air pressure control unit 2; The multi-stage coagulation device includes a first coagulation bath 5, a first drafting roller 7, a second coagulation bath 10, a second drafting roller 11, and a third coagulation bath 13 arranged sequentially along the spinning direction, as well as a second temperature control unit 6, a third temperature control unit 9, and a fourth temperature control unit 12 respectively connected to the first coagulation bath 5, the second coagulation bath 10, and the third coagulation bath 13.

[0005] Preferably, the first coagulation bath 5, the second coagulation bath 10 and the third coagulation bath 13 are all hollow double-walled structures, and each end is provided with a liquid inlet 51 and a liquid outlet 52.

[0006] Preferably, detachable alumina ceramic wire pressing guide rollers 8 are provided at the right end of the first coagulation bath, both ends of the second coagulation bath, and both ends of the third coagulation bath.

[0007] Preferably, the first drafting roller 7 and the second drafting roller 11 each include three drafting rollers arranged in an inverted triangle; the drying device 14 is an atmospheric pressure hot air drying device.

[0008] The present invention also provides a method for preparing aerogel fibers using the aerogel fiber wet spinning equipment described above, comprising the following steps: The sheath spinning solution and the core spinning solution are placed in the sheath spinning solution storage tank 34 and the core spinning solution storage tank 33, respectively. The temperature of the sheath-core spinning solution storage tank is controlled at 35~75℃ by the first temperature control unit 4. Under the action of air pressure, the solution is extruded through the coaxial spinneret 312 to form a spinning fine stream with a sheath-core structure. After the spun yarn is subjected to multi-stage coagulation bath treatment by a multi-stage coagulation device, it is dried by a drying device 14 and wound and collected by a winding and collecting device 15 in sequence to obtain aerogel fibers; the temperature of the first coagulation bath treatment in the multi-stage coagulation bath treatment is 30~80℃, the temperature of the second coagulation bath treatment is 90~98℃, and the temperature of the third coagulation bath treatment is 10~25℃.

[0009] Preferably, the solute in the sheath spinning solution includes polyimide, aromatic polyamide, polysulfone, cellulose, or polyacrylonitrile; the solute in the core spinning solution includes polyvinyl alcohol, polylactic acid, polyoxyethylene, chitosan, or sodium alginate.

[0010] Preferably, the mass fraction of the sheath spinning solution and the core spinning solution is independently 10~30wt%.

[0011] Preferably, the pressure applied by the air pressure is 0.05~0.8MPa.

[0012] Preferably, during the second coagulation bath treatment, wet heat stretching and fiber structure orientation treatment are performed, wherein the draw ratio of the orientation treatment is 1.2 to 5.0 times.

[0013] Preferably, the aerogel fiber has a core-sheath structure, a tensile strength of 80~160MPa, and a thermal conductivity of 0.018~0.098W / (m·K).

[0014] Compared with the prior art, the present invention has the following beneficial effects: This invention provides a wet spinning apparatus for aerogel fibers, comprising a gas control device, a liquid-spinning device 3, and a multi-stage coagulation device, a drying device 14, and a winding and collecting device 15 arranged sequentially along the spinning direction; the gas control device includes a gas supply unit 1 and a gas pressure control unit 2; the liquid-spinning device includes a spinning solution storage tank, a coaxial spinneret 312, and a first temperature control unit 4 connected to the spinning solution storage tank; the spinning solution storage tank includes a core layer spinning solution storage tank 33 and a sheath layer spinning solution storage tank 34, respectively connected to... The coaxial spinneret has a core layer channel and a sheath layer channel; both the core layer spinning solution tank and the sheath layer spinning solution tank are provided with air inlets at the top, which are connected to the gas output pipeline of the air pressure control unit 2; the multi-stage coagulation device includes a first coagulation bath 5, a first drafting roller 7, a second coagulation bath 10, a second drafting roller 11 and a third coagulation bath 13 arranged sequentially along the spinning direction, and a second temperature control unit 6, a third temperature control unit 9 and a fourth temperature control unit 12 respectively connected to the first coagulation bath, the second coagulation bath and the third coagulation bath.

[0015] The aerogel fiber wet spinning equipment of the present invention has each device arranged sequentially along the spinning direction, forming a fully continuous wet spinning production line from extrusion of spinning solution to winding and collection of finished products. The multi-bath treatment does not involve intermittent processes such as freeze-drying or supercritical drying, enabling continuous production throughout the entire process. This solves the technical problem of existing aerogel fiber preparation processes, which rely on intermittent post-processing steps, making continuous and efficient production difficult. Furthermore, the present invention features a three-stage coagulation bath, with drawing rollers on both sides of the second coagulation bath. This allows for stepped temperature treatment in the three-stage coagulation bath while simultaneously performing stretching and orientation treatment in the second coagulation bath, effectively controlling the internal pore structure and uniformity of the fiber, achieving the formation of a porous skin structure and the densification and orientation of the core layer.

[0016] Furthermore, the aerogel fiber wet spinning equipment of the present invention also has the following advantages: (1) Using pneumatic drive instead of traditional mechanical pump to transport spinning solution: The structure is simpler, which can effectively reduce the complexity of equipment and maintenance costs, while reducing fluid pulsation and improving the stability and continuity of the spinning process. The pneumatic pressure adjustment range is 0.05~0.8MPa, and the pressure value is displayed in real time in digital form, which can realize precise control of the extrusion pressure of spinning solution.

[0017] (2) The hollow double-wall temperature control structure can be adopted to precisely control the temperature of the spinning solution and the coagulation bath, thereby improving the rheological properties of the spinning solution and the uniformity of fiber forming. Four independent temperature control devices control the temperature of the spinning solution storage tank, the first coagulation bath, the second coagulation bath and the third coagulation bath respectively, forming a precise, independent and graded temperature control system.

[0018] (3) Inverted triangular arrangement of drafting rollers is set on both sides of the second bath: each drafting roller is arranged in an inverted triangle, with the two rollers at the base of the triangle rotating clockwise in the same direction, and the roller opposite to the base rotating counterclockwise in the opposite direction, with all three rollers rotating at the same speed. The adjustable drafting ratio (1.2~5.0 times) is formed by the speed difference between the front and rear drafting rollers. The drafting rollers can switch between forward and reverse rotation synchronously, applying uniform and stable longitudinal tensile stress to the fiber in the high-temperature bath, avoiding slippage, displacement or damage of the fiber during the drafting process, and ensuring the uniform formation of a dense core network. This adjustable wet heat drafting method can improve the molecular chain orientation, thereby significantly improving the mechanical properties of the fiber.

[0019] (4) The use of a lifting liquid storage tank structure can effectively prevent the backflow of solidified liquid during shutdown, which can cause the spinneret to be blocked, thus improving the stability and reusability of the equipment; the use of detachable alumina ceramic pressing guide rollers can improve the stability of fiber operation and reduce friction damage.

[0020] (5) The two independent storage tank structure can not only realize continuous feeding, but also be used to prepare coaxial structure, core-sheath structure and composite structure fibers, which are suitable for the continuous preparation of high performance fibers, functional fibers and aerogel fiber materials.

[0021] This invention also provides a method for preparing aerogel fibers using the aerogel fiber wet spinning equipment described above, which has at least the following beneficial effects: (1) The first use of high and low temperature gradient temperature coagulation and high temperature bath stretching synergistic control technology: The present invention adopts the high and low temperature gradient temperature treatment process of "first coagulation bath - medium and high temperature coagulation (30~80℃) + second coagulation bath - high temperature bath stretching above 90℃ + room temperature water washing", which realizes the full-process continuous wet spinning production of aerogel fiber with "porous skin and dense core". In existing technologies, the two-step solidification technology of Professor Zhuang Xupin and Professor Yang Guang's team at Tianjin University of Technology forms a "dense skin-porous core" structure (dense skin, porous core), which is the opposite of the "porous skin, dense core" structure of this invention in terms of pore distribution. The coaxial wet spinning technology of Professor Liu Tianxi and Professor Fan Wei's team at Jiangnan University requires step-by-step post-processing after fiber solidification, including collection by rollers, drying, and thermal imidization, and is not a fully continuous production line. The wet freeze-spinning technology uses freeze-solidification in a low-temperature solidification bath (-196℃ liquid nitrogen), which is fundamentally different from the high-low temperature gradient solidification system of this invention. This invention separates solidification kinetics control and stretching orientation in two baths with different temperature conditions, allowing for independent optimization of the temperature and stretching conditions of both steps, achieving better structural and performance control.

[0022] (2) Coaxial spinning allows for simultaneous extrusion molding of the sheath and core spinning solutions, thereby constructing aerogel fibers with a sheath-core structure. The sheath can be composed of rigid-chain polymer components (such as polyimide, aromatic polyamide, etc.), which facilitates the formation of a porous aerogel structure and improves the high-temperature resistance of the fiber; the core can be composed of flexible-chain polymer components (such as polyvinyl alcohol, etc.), which promotes the orientation and densification of the core molecular chains during the high-temperature bath stretching process, thereby achieving a synergistic improvement in the fiber's high strength and thermal insulation performance.

[0023] (3) The coaxial spinneret can be replaced with a single filament spinneret or a flat filament spinneret, and can be flexibly replaced according to different product requirements to meet the preparation requirements of different morphological materials such as single filament, multifilament and ribbon fiber, thereby improving the flexibility and applicability of the device.

[0024] (4) Setting up high and low temperature gradient coagulation bath treatment: The first coagulation bath uses medium-high temperature coagulation of 30~80℃ to quickly form a porous structure in the cortex of the spun yarn; the second bath uses high temperature bath above 90℃ for drawing to promote the densification of molecular chain orientation in the core layer; and the residual solvent is removed by washing with room temperature water. This high and low temperature gradient temperature treatment process effectively controls the internal pore structure and structural uniformity of the fiber, and realizes cross-scale independent control of the cortex and core layer.

[0025] (5) Excellent mechanical properties and thermal insulation properties are achieved: the dense network of the core layer provides reliable mechanical support, with a tensile strength of 80~160 MPa, which can meet the needs of industrial textile processing; the porous structure of the skin layer has controllable porosity and pore size, and a thermal conductivity as low as 0.018~0.098 W / (m·K). The prepared aerogel fiber can be widely used in high-performance aerogel fiber, composite functional fiber and advanced thermal insulation materials, and has the advantages of stable extrusion, precise temperature control, compact structure and wide applicability. Attached Figure Description

[0026] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0027] Figure 1 This is a schematic diagram of the structure of the wet spinning equipment for aerogel fibers of the present invention; Figure 2 This is a schematic diagram of the liquid storage spinning device of the present invention; Figure 3 This is a top view of the hollow double-walled coagulation bath of the present invention. Figure 4 This is a schematic diagram of the drawing device of the present invention; Figure 5 This is a schematic diagram of the winding and collecting device of the present invention; Figure 6 This is a photograph of the high-strength aerogel fiber prepared in Example 1. Figure 7 The images shown are scanning electron microscope (SEM) images of the high-strength aerogel fibers obtained in Example 1, where a is a surface SEM image of the fiber, b is a cross-sectional SEM image of the fiber sheath, c is a 500x SEM image of the cross-section of the fiber sheath, d is a 2000x SEM image of the cross-section of the fiber sheath, e is a cross-sectional SEM image of the PVA core layer, and f is a 5000x SEM image of the cross-section of the PVA core layer. Reference numerals: 1. Gas supply unit; 2. Gas pressure control unit; 3. Liquid storage spinning device; 4. First temperature control unit; 5. First coagulation bath; 6. Second temperature control unit; 7. First drafting roller; 8. Alumina ceramic pressing guide roller; 9. Third temperature control unit; 10. Second coagulation bath; 11. Second drafting roller; 12. Fourth temperature control unit; 13. Third coagulation bath; 14. Drying device; 15. Winding and collecting device; 31. First air inlet; 32. Second air inlet; 33. Core layer spinning solution storage tank; 34. Sheet layer spinning solution storage tank; 35. Heating liquid outlet; 36. Clamp; 37. Liquid storage tank rack; 38. Heating liquid inlet; 39. Ball valve; 310. Liquid delivery pipeline; 311. Hollow double-walled liquid delivery pipeline; 312. 313. Coaxial spinneret assembly; 314. Storage tank rack base; 51. Hand-cranked rotary lifting platform; 52. Coagulation bath inlet; 73. Coagulation bath outlet; 74. Forward / reverse adjustment switch; 75. Drafting roller 1; 76. Drafting roller 2; 77. Drafting roller 3; 78. Drafting roller speed adjustment knob; 79. Drafting roller handle; 100. Drafting roller base; 111. Winding and collecting device LCD display panel; 122. Reciprocating oscillating shaft speed adjustment knob; 133. Collecting roller speed adjustment knob; 14. Winding and collecting device switch button; 155. Winding and collecting device base; 156. Alumina ceramic guide hook; 157. Alumina ceramic guide wheel; 158. Collecting roller; 159. Winding and collecting device handle. Detailed Implementation

[0028] The present invention provides a wet spinning equipment for aerogel fibers, including a gas control device, a liquid storage spinning device 3, and a multi-stage coagulation device, a drying device 14 and a winding and collecting device 15 arranged sequentially along the spinning direction; The gas control device includes a gas supply unit 1 and a gas pressure control unit 2; The spinning device 3 includes a spinning solution storage tank, a coaxial spinneret 312, and a first temperature control unit 4 connected to the spinning solution storage tank. The spinning solution storage tank includes a core layer spinning solution storage tank 33 and a skin layer spinning solution storage tank 34, which are respectively connected to the core layer channel and the skin layer channel of the coaxial spinneret. The top of both the core layer spinning solution storage tank and the skin layer spinning solution storage tank is provided with an air inlet, which is connected to the gas output pipeline of the air pressure control unit 2. The multi-stage coagulation device includes a first coagulation bath 5, a first drafting roller 7, a second coagulation bath 10, a second drafting roller 11, and a third coagulation bath 13 arranged sequentially along the spinning direction, as well as a second temperature control unit 6, a third temperature control unit 9, and a fourth temperature control unit 12 respectively connected to the first coagulation bath 5, the second coagulation bath 10, and the third coagulation bath 13.

[0029] like Figure 1As shown, the aerogel fiber wet spinning equipment of the present invention includes a gas control device, which includes a gas supply unit 1 and a gas pressure control unit 2.

[0030] In this invention, the gas supply unit of the gas control device is connected to a pressure control unit to provide stable air pressure to the spinning device. The gas supply unit is preferably an air compressor, and the pressure control unit is a precision pressure controller with a pressure adjustment range of 0~0.81 MPa and a spinning pressure adjustment range of 0.05~0.8 MPa. The pressure values ​​are displayed in real-time digitally. Using a pneumatic drive method to replace the traditional mechanical pump for conveying the spinning solution results in a simpler structure, effectively reducing equipment complexity and maintenance costs, while also reducing fluid pulsation and improving the stability and continuity of the spinning process.

[0031] like Figure 1 As shown, the aerogel fiber wet spinning equipment of the present invention includes a liquid-spinning device 3, which includes a spinning solution storage tank, a coaxial spinneret 312, and a first temperature control unit 4 connected to the spinning solution storage tank. The spinning solution storage tank includes a core layer spinning solution storage tank 33 and a sheath layer spinning solution storage tank 34, which are respectively connected to the core layer channel and the sheath layer channel of the coaxial spinneret. The top of both the core layer spinning solution storage tank and the sheath layer spinning solution storage tank is provided with an air inlet, which is connected to the gas output pipeline of the air pressure control unit 2.

[0032] In this invention, the coaxial spinneret is located at the outlet of the spinning solution storage tank and is used to extrude the spinning solution to form a spinning stream.

[0033] In this invention, the core spinning solution storage tank 33 and the sheath spinning solution storage tank 34 are two independently configured spinning solution storage tanks, respectively connected to the core channel and sheath channel of the coaxial spinneret, for conveying core spinning solution and sheath spinning solution of different components respectively. The spinning solution storage tanks adopt a hollow double-wall structure and are connected to an independent temperature control unit (shown as the first temperature control unit 4), which can adjust the temperature of the spinning solution to control its viscosity and rheological properties, thereby improving its spinnability and extrusion stability.

[0034] In this invention, such as Figure 2As shown, the spinning solution storage tank is equipped with a detachable storage tank cover on top. The top of the storage tank cover has air inlets (first air inlet 31 and second air inlet 32). The storage tank cover is fixed to the storage tank using stainless steel clamps 36. A flexible material sealing ring is provided between the storage tank cover and the storage tank to ensure the airtightness of the storage tank. The lower end of the spinning solution storage tank is sequentially connected to a ball valve 39, a liquid delivery pipe 310 (or a hollow double-walled liquid delivery pipe 311, which can be connected to a temperature control unit for heating), and a coaxial spinneret assembly 312. The ball valve is used to adjust the spinning solution flow rate and control the spinning solution extrusion speed. The spinning solution storage tank is externally equipped with a heating liquid inlet 38 and a heating liquid outlet 35 for heating the spinning solution inside the tank. The heating liquid is water. The liquid storage spinning device also includes a tank lifting structure, which includes a liquid storage tank frame 37, a liquid storage tank frame base 313, and a hand-cranked rotary lifting platform 314. The tank lifting structure can adjust the height of the tank and the spinneret assembly: during spinning, the tank position can be lowered so that the spinneret assembly is immersed below the coagulation bath liquid surface for spinning; when spinning is paused or ended, the tank position can be raised so that the spinneret assembly is above the coagulation bath liquid surface, thereby preventing the coagulation bath liquid from flowing back into the spinneret assembly and causing blockage.

[0035] In this invention, the coaxial spinneret is a coaxial core-sheath structure spinneret, and it is a replaceable structure. It can be replaced with a two-component single-hole spinneret (core layer 0.2~0.3mm, sheath layer 0.2~0.4mm); a single-component multi-hole spinneret (1~100 holes, hole diameter 0.07~0.25mm); a single-component single-needle spinneret (hole diameter 0.4~2.5mm); or a single-component flat ribbon spinneret, used to realize the continuous forming of multi-strand fibers, monofilament fibers or ribbon fibers.

[0036] like Figure 1 As shown, the aerogel fiber wet spinning equipment of the present invention includes a multi-stage coagulation device. The multi-stage coagulation device includes a first coagulation bath 5, a first drafting roller 7, a second coagulation bath 10, a second drafting roller 11 and a third coagulation bath 13 arranged sequentially along the spinning direction, and a second temperature control unit 6, a third temperature control unit 9 and a fourth temperature control unit 12 respectively connected to the first coagulation bath, the second coagulation bath and the third coagulation bath.

[0037] In this invention, the spinning direction is the direction in which the spinning stream travels.

[0038] In this invention, the first coagulation bath 5, the second coagulation bath 10, and the third coagulation bath 13 are all hollow double-walled structures, including a coagulation bath inlet 51 and a coagulation bath outlet 52 (e.g., Figure 3(As shown). The second temperature control unit is a medium-high temperature control device, and the temperature can be set to 30~80℃; the third temperature control unit is a high temperature control device, and the temperature can be set to above 90℃; the temperature of the fourth temperature control unit can be set to 10~25℃ (room temperature).

[0039] In this invention, an adjustable drafting ratio is formed between the first and second drafting rollers through a speed difference, with the adjustable range being 1.2 to 5.0 times. This invention employs a high-low temperature gradient coagulation process. After the fiber is drawn from the first coagulation bath, it enters the second coagulation bath, where it undergoes stretching and orientation treatment in a high-temperature medium above 90°C, and then enters a room-temperature water bath. By setting drafting rollers on both sides of the second bath and performing stretching and orientation treatment in the high-temperature bath, the orderly arrangement and densification of the core layer molecular chains are effectively promoted, forming a dense core layer network. The temperature control devices of the first coagulation bath, the second coagulation bath, and the room-temperature water bath, together with the temperature control device of the storage tank, form an independently configured temperature control system, creating a high-low temperature gradient treatment condition from medium-high temperature coagulation to high-temperature stretching and then to room-temperature washing. Each bath is equipped with a circulating medium inlet and outlet, and temperature regulation is achieved through the circulation of temperature-controlled liquid within the double-walled interlayer.

[0040] In this invention, detachable alumina ceramic pressing guide wheels 8 are provided at the right end of the first coagulation bath, both ends of the second coagulation bath, and both ends of the third coagulation bath (room temperature water bath) to guide the fibers into and out of each bath and keep the fibers running.

[0041] In this invention, each drafting roller (first drafting roller and second drafting roller 11) includes three drafting rollers (drafting roller 1, drafting roller 2, and drafting roller 3) arranged in an inverted triangle: the two rollers at the base of the triangle rotate in the same direction, while the roller opposite to the base rotates in the opposite direction, and all three rollers move at the same speed; the adjustable drafting ratio is formed by the speed difference of the drafting rollers. The drafting rollers can be switched synchronously in both directions; that is, before switching, the two rollers at the base of the triangle rotate clockwise, and the roller opposite to the base rotates counterclockwise; after synchronous switching, the two rollers at the base of the triangle rotate counterclockwise, and the roller opposite to the base rotates clockwise. This inverted triangle arrangement of the drafting rollers can apply uniform and stable longitudinal tensile stress to the fiber in a high-temperature bath, preventing the fiber from slipping, shifting, or being damaged during the drafting process, and ensuring the uniform formation of a dense core network. Figure 4 The diagram shows the structure of the drafting device of the present invention, including a front view, a rear view, and a side view. 71 is a forward / reverse adjustment switch; 72 is a drafting roller 1; 73 is a drafting roller 2; 74 is a drafting roller 3; 75 is a drafting roller speed adjustment knob; 76 is a drafting roller handle; and 77 is a drafting roller base.

[0042] like Figure 1 As shown, the aerogel fiber wet spinning equipment of the present invention includes a drying device 14 and a winding and collecting device 15.

[0043] In this invention, the drying device is positioned after the coagulation device and is used to dry the fibers. The drying device is preferably an atmospheric pressure hot air drying device, specifically a hot air dryer. It can select an atmospheric pressure drying mode according to the target pore structure requirements of the cortex (adjusting the temperature and fiber travel speed parameters of atmospheric pressure drying to control the evaporation rate of moisture and solvent, thereby matching and obtaining preset pore structure indicators such as cortex pore size and porosity), and does not rely on freeze-drying or supercritical drying. In an embodiment of this invention, the drying device is positioned after a room temperature water bath and is used to dry the washed fibers.

[0044] In this invention, the winding and collecting device is located after the drying device and is used for continuous winding and collecting of fibers. The winding and collecting device is a continuous winding device with a yarn-spinning function, which works in conjunction with the drawing roller and the multi-bath treatment unit to realize continuous production from spinning solution extrusion to finished fiber winding. Figure 5 The diagram shows the structure of the winding and collecting device in this invention, including a front view, a side view, and a rear view. 151 is the LCD display panel of the winding and collecting device; 152 is the reciprocating oscillating wire shaft speed adjustment knob; 153 is the collecting roller speed adjustment knob; 154 is the winding and collecting device switch button; 155 is the winding and collecting device base; 156 is the alumina ceramic wire guide hook; 157 is the alumina ceramic guide wheel; 158 is the collecting roller; and 159 is the winding and collecting device handle.

[0045] The various devices of this invention are arranged sequentially along the spinning direction to form a fully continuous wet spinning production line.

[0046] The present invention also provides a method for preparing aerogel fibers using the aerogel fiber wet spinning equipment described above, comprising the following steps: The sheath spinning solution and the core spinning solution are placed in the sheath spinning solution storage tank 34 and the core spinning solution storage tank 33, respectively. The temperature of the spinning solution storage tank is controlled at 35~75℃ by the first temperature control unit 4, and the solution is extruded through the coaxial spinneret 312 under air pressure to form a spinning fine stream with a sheath-core structure. After the spun yarn is subjected to multi-stage coagulation bath treatment by a multi-stage coagulation device, it is dried by a drying device 14 and wound and collected by a winding and collecting device 15 in sequence to obtain aerogel fibers; the temperature of the first coagulation bath treatment in the multi-stage coagulation bath treatment is 30~80℃, the temperature of the second coagulation bath treatment is 90~98℃, and the temperature of the third coagulation bath treatment is 10~25℃.

[0047] Unless otherwise specified, all materials and equipment used in this invention are commercially available products in the field.

[0048] In this invention, the sheath spinning solution and the core spinning solution are placed in the sheath spinning solution storage tank 34 and the core spinning solution storage tank 33, respectively, and extruded through the coaxial spinneret 312 under air pressure to form a spinning fine stream with a sheath-core structure.

[0049] In this invention, the sheath spinning solution and the core spinning solution are prepared independently and transported separately in two independent spinning solution storage tanks.

[0050] In this invention, the solute of the skin spinning solution is preferably a rigid-chain component, specifically one of polyimide, aromatic polyamide, polyarylsulfone, cellulose, and polyacrylonitrile, and the solvent is preferably dimethyl sulfoxide. The solute of the core spinning solution is preferably a flexible-chain component, specifically one of polyvinyl alcohol, polylactic acid, polyoxyethylene, chitosan, and sodium alginate, and the solvent is preferably dimethyl sulfoxide.

[0051] In this invention, the solid content of the sheath spinning solution and the core spinning solution is preferably 10-30 wt%, the solid content of the sheath spinning solution can be 15 wt%, 20 wt%, 25 wt%, or 30 wt%, and the solid content of the core spinning solution can be 10 wt%, 12.5 wt%, or 15 wt%. The temperature of the sheath spinning solution and the core spinning solution is preferably 35-75°C, specifically 35°C, 45°C, 55°C, or 75°C.

[0052] In this invention, the pressure of the air pressure is preferably 0.05~0.8MPa, specifically 0.2MPa, 0.5MPa or 0.7MPa.

[0053] After forming a spun yarn with a skin-core structure, the present invention uses a multi-stage coagulation device for multi-stage coagulation bath treatment, followed by drying using a drying device 14 and winding and collecting using a winding and collecting device 15 to obtain aerogel fibers; in the multi-stage coagulation bath treatment, the temperature of the first coagulation bath treatment is 30~80℃, the temperature of the second coagulation bath treatment is 90~98℃, and the temperature of the third coagulation bath treatment is 10~25℃.

[0054] In this invention, the bath solutions for the first, second, and third coagulation baths are all water; the preferred temperature for the first coagulation bath is 50-80°C, the preferred temperature for the second coagulation bath is 95-98°C, and the preferred temperature for the third coagulation bath is 15-25°C. The first coagulation bath uses medium-high temperature coagulation to initially solidify and shape the spun fibers, forming a porous skin structure; the second coagulation bath involves stretching and orienting the fibers in a high-temperature bath with a draw ratio of 1.2-5.0 times, promoting the orderly arrangement and densification of the core layer molecular chains, forming a dense core layer network; the third coagulation bath (room temperature water washing) washes the stretched fibers to remove residual solvent and coagulation medium.

[0055] During the second coagulation bath treatment (in the second coagulation bath tank), stretching and orientation treatment is performed. Drafting rollers are set on both sides of the second coagulation bath tank, and the stretching ratio is formed by the speed difference between the drafting rollers. After the fiber is drawn out from the first coagulation bath, it directly enters the second bath tank and completes the stretching and orientation in a high-temperature medium above 90°C. Then it enters the room temperature water bath.

[0056] This invention involves online drying of fibers after a third coagulation bath treatment (washing). In this invention, the drying process is carried out using atmospheric pressure hot air drying, without relying on freeze-drying or supercritical drying post-treatment.

[0057] The present invention continuously winds and collects the obtained fibers to obtain high-strength aerogel fibers with a cross-scale structure of "porous skin and dense core".

[0058] The multi-bath treatment described in this invention does not involve intermittent processing techniques such as freeze-drying or supercritical drying, nor does it involve separate fiber collection followed by intermittent processing. Each step is carried out sequentially and continuously along the spinning direction, achieving continuous production of wet spinning throughout the entire process.

[0059] The aerogel fiber prepared by this invention has a multi-scale, multi-level structure of "porous skin and dense core": the skin is a loose porous structure with a porosity of 85-98% and an average pore size of 50-500 nm; the core is a dense structure; the tensile strength of the fiber is 80-160 MPa and the thermal conductivity is 0.018-0.098 W / (m·K).

[0060] Currently prepared aerogel fibers suffer from a trade-off between mechanical strength and thermal insulation performance. While the porous structure of aerogel fibers imparts excellent thermal insulation, it also leads to high fiber brittleness and low strength. Although composite reinforcement can improve strength, it is difficult to simultaneously control the fine-grained pore structure. Currently, the tensile strength of wet-spun aerogel fibers is mostly in the range of several MPa to tens of MPa, and there is an inherent contradiction between strength and porosity. This invention constructs a multi-scale, multi-level structure with a porous outer layer and a dense core layer. The loose, porous outer layer ensures the high porosity required for thermal insulation, while the dense core layer acts as a mechanical load-bearing skeleton, breaking the inherent trade-off between strength and porosity. Existing wet spinning equipment cannot meet the requirements for continuous and precise preparation of multi-scale structural fibers. Traditional equipment often uses mechanical metering pumps to deliver the spinning solution, resulting in problems such as large fluid pulsation and unstable micro-volume delivery. This invention achieves stable spinning solution delivery through air pressure control. Existing equipment has limited temperature control precision for the spinning solution and coagulation bath, making it difficult to accurately regulate coagulation kinetics. This invention achieves precise temperature control by connecting a hollow spinning solution tank and a coagulation bath via a temperature control system. Existing equipment has a simple spinneret structure, poor adaptability to coaxial core-sheath structures, and cannot produce coaxial fibers. This invention, with its two spinning solution tanks and coaxial spinning assembly, can produce coaxial fibers.

[0061] This invention addresses the technical bottlenecks of existing aerogel fiber manufacturing processes, such as the difficulty in achieving a balance between strength and thermal insulation performance, the reliance on intermittent post-processing steps that hinder continuous production, and the problems of poor extrusion stability, insufficient temperature control precision, poor fiber structure uniformity, and inadequate continuous production capabilities in existing wet spinning equipment. Currently, these systems lack multi-bath staged processing and online drawing capabilities, making it impossible to simultaneously achieve porous skin structure formation and core densification and orientation during fiber forming. This invention provides a continuous forming scheme and supporting equipment for preparing high-strength aerogel fibers based on a synergistic control technology of high-low temperature gradient solidification and high-temperature bath drawing. The pneumatic wet spinning equipment features stable gas pressure extrusion, high-low temperature gradient solidification, and high-temperature bath drawing capabilities, and can be used for continuous wet spinning of high-strength aerogel fibers.

[0062] To further illustrate the present invention, the wet spinning equipment for aerogel fibers and the method for preparing aerogel fibers provided by the present invention will be described in detail below with reference to the accompanying drawings and embodiments, but these should not be construed as limiting the scope of protection of the present invention.

[0063] Example 1 use Figure 1 The equipment shown is used for a continuous wet spinning process of high-strength aerogel fibers.

[0064] 1. Preparation of spinning solution: The skin spinning solution uses polyarylsulfone (PES) dissolved in dimethyl sulfoxide (DMSO), with a PES mass fraction of 15 wt% (a lower concentration, resulting in a thinner skin layer with larger pore size).

[0065] The core spinning solution uses polyvinyl alcohol (PVA) dissolved in DMSO, with a PVA mass fraction of 10 wt% (lower concentration, resulting in a finer core layer).

[0066] The two spinning solutions are respectively stored in two independent hollow double-walled spinning solution tanks (33, 34), and the temperature of the spinning solution is adjusted to 35°C by the first temperature control system 4. The storage tanks are made of 316L stainless steel and have online pressure degassing function.

[0067] 2. Extrusion and solidification: A stable air pressure of 0.2 MPa is provided to the storage tank via an air compressor and air pressure controller (a knob-type precision air pressure controller with an adjustment range of 0~0.8 MPa and a digital real-time display). A hand-cranked rotary lifting platform 314 lowers the position of the storage tank, immersing the coaxial spinneret 312 (0.5 mm inner diameter at the skin channel outlet and 0.2 mm inner diameter at the core channel outlet) below the liquid surface of the first coagulation bath 5. The skin spinning solution and the core spinning solution are simultaneously extruded through the coaxial spinneret 312, forming a skin-core structure spinning fine stream.

[0068] The spun fibers first enter the first coagulation bath 5, where deionized water is used as the coagulation medium, and the temperature is controlled at 50℃ (medium-high temperature coagulation) by the second temperature control unit 6. The spun fibers undergo initial solidification in the bath, forming a porous skin structure (the PES skin is relatively thin, and the pore size is relatively large). Subsequently, the fibers are guided by a detachable alumina ceramic pressing guide wheel at the right end of the first coagulation bath and enter the second bath 10.

[0069] The second coagulation bath 10 contains deionized water, and the temperature is controlled at 90℃ by the third temperature control unit 9. Inverted triangular arrangement of drawing rollers is installed on both sides of the second coagulation bath. The drawing rollers 72, 73, and 74 of each drawing machine are arranged in an inverted triangle, with the two rollers at the base of the triangle rotating in the same direction and the roller opposite the base rotating in the opposite direction. All three rollers in each group of drawing rollers move at the same speed. By adjusting the speed difference of the drawing rollers, the fibers are stretched and oriented in a high-temperature bath. The draw ratio is 1.2 times (low draw, lower core layer orientation, limited densification, and relatively finer core layer diameter), promoting the orderly arrangement and densification of the PVA molecular chains in the core layer, forming a dense core layer network.

[0070] 3. Washing, drying and winding: The stretched fibers are then placed in a room-temperature water bath, where the temperature is controlled at 15°C by the fourth temperature control unit 12, to remove residual solvent. The washed fibers then enter a drying device 14 (a normal-pressure hot air drying device) at a drying temperature of 60°C. The dried fibers are then continuously wound and collected by a winding and collecting device 15 to obtain high-strength aerogel fibers.

[0071] Example 1: Continuous process throughout the entire process.

[0072] Fiber structure and properties: Testing revealed that the aerogel fiber skin prepared in this embodiment has a loose, porous structure (PES, relatively thin) and a dense core (PVA). The total fiber diameter (outer diameter of the skin) is 0.32 mm, and the core diameter is 0.15 mm. The skin porosity is approximately 85% (numerous pores, but due to the thin skin, the overall thermal insulation contribution is limited), with an average pore size of approximately 450 nm. The fiber tensile strength is 82 MPa (the core is relatively thin and has low draw, resulting in lower strength), and the thermal conductivity is 0.098 W / (m·K) (moderate thermal insulation performance).

[0073] Example 2 use Figure 1 The equipment shown follows the same process steps as in Example 1, with the following differences in parameters: 1. Preparation of spinning solution: Cortex spinning solution: Polyarylsulfone (PES) mass fraction of 20 wt% (medium concentration, moderate cortex thickness).

[0074] Core spinning solution: PVA mass fraction of 12.5 wt% (medium concentration, suitable core diameter).

[0075] The spinning solution temperature is 30℃.

[0076] 2. Extrusion and solidification: Storage tank pressure: 0.03 MPa.

[0077] Coaxial spinneret assembly: skin channel outlet inner diameter 0.6 mm, core channel outlet inner diameter 0.25 mm.

[0078] First coagulation bath 5: Deionized water, temperature 65℃.

[0079] Second coagulation bath 10: deionized water, temperature 95℃, draw ratio 2.5 times (medium draw, improved core orientation and compaction, moderate core diameter).

[0080] 3. Washing, drying and winding Bathing with room temperature water: 20℃.

[0081] Drying temperature: 80℃.

[0082] Example 2: Continuous process throughout the entire process.

[0083] Fiber structure and properties: The total fiber diameter is 0.38 mm, and the core diameter is 0.22 mm; the skin porosity is about 92% (the skin is thicker and has more pores), with an average pore size of about 180 nm; the tensile strength is 125 MPa (the core is thicker and the stretching is increased, resulting in a significant increase in strength), and the thermal conductivity is 0.025 W / (m·K) (the thermal insulation performance is better than that of Example 1).

[0084] Example 3 use Figure 1 The equipment shown follows the same process steps as in Example 1, with the following differences in parameters: 1. Preparation of spinning solution: Skin spinning solution: Polyacrylonitrile (PAN) is dissolved in DMSO, with a PAN mass fraction of 25 wt% (a relatively high concentration, but PAN has good porosity and can form a thicker skin with more pores).

[0085] Core spinning solution: PVA mass fraction of 15 wt% (higher concentration, coarser core layer).

[0086] The spinning solution temperature is 35℃.

[0087] 2. Extrusion and solidification: Air pressure: 0.04 MPa.

[0088] Coaxial spinneret assembly: skin channel outlet inner diameter 0.8 mm, core channel outlet inner diameter 0.35 mm.

[0089] First coagulation bath 5: Deionized water, temperature 80℃.

[0090] Second coagulation bath 10: deionized water, temperature 98℃, draw ratio 5.0 times (high draw, which makes the core layer highly oriented and dense, while the overall diameter becomes thinner).

[0091] 3. Washing, drying and winding Bathing with room temperature water: 25℃.

[0092] Drying temperature: 100℃.

[0093] Example 3: Continuous process throughout the entire process.

[0094] Fiber structure and properties: Although the original extruded diameter of the core layer was relatively large (0.35 mm), due to the high draw ratio of 5.0 times, the total fiber diameter (outer diameter of the sheath) was actually finer at 0.48 mm (slightly larger than the 0.38 mm in Comparative Example 2); the core layer diameter was 0.28 mm. The sheath porosity was as high as 95% (the PAN sheath was thick and porous), with an average pore size of approximately 80 nm (small and dense pores). The tensile strength was 155 MPa (higher strength due to the coarse and highly oriented core layer), and the thermal conductivity was 0.018 W / (m·K) (optimal thermal insulation performance).

[0095] Figure 6 This is a photograph of the high-strength aerogel fiber prepared in Example 1.

[0096] Figure 7 The images shown are scanning electron microscope (SEM) images of the high-strength aerogel fibers in Example 1, where a is a surface SEM image of the fiber, b is a cross-sectional SEM image of the fiber sheath, c is a 500x SEM image of the cross-section of the fiber sheath, d is a 2000x SEM image of the cross-section of the sheath fiber, e is a cross-sectional SEM image of the PVA core layer, and f is a 5000x SEM image of the cross-section of the PVA core layer.

[0097] Depend on Figure 7 As can be seen from b, the cross-section of the high-strength aerogel fiber has a porous structure. C also shows the loose skin structure of the high-strength aerogel fiber. E reflects the dense core structure of the high-strength aerogel fiber.

[0098] Comparative Example 1 Referring to the existing technology (Jiangnan University Liu Tianxi / Fan Wei team, "Advanced Fiber Materials" 2025), 2.1.2, soluble fluorinated polyimide (PI-6FDA / ODA) was used as the sheath spinning solution and polyamic acid (PAABPDA / ODA) was used as the core spinning solution to prepare polyimide aerogel fiber (HPPAF).

[0099] This process is a step-by-step post-processing, not a continuous production process.

[0100] Fiber structure and properties: The total fiber diameter is approximately 0.35 mm, and the core diameter is approximately 0.18 mm; the tensile strength is 55.2 MPa, and the thermal conductivity is 0.0372 W / (m·K).

[0101] Comparative Example 2 Referring to existing technology (Zhuang Xupin / Yang Guang team, Tianjin University of Technology, "Advanced Functional Materials" 2025), aramid nanofiber (ANF) spinning sol precursor was used as raw material (solid content 3 wt%). A two-step coagulation process was employed: first, extrusion into a room-temperature (25℃) formic acid coagulation bath for rapid gelation for 5 seconds (forming a dense skin layer); then, transfer to a room-temperature (25℃) deionized water coagulation bath for slow gelation for 1 minute (generating a porous core layer). The resulting gel fibers were collected, washed with deionized water, subjected to tert-butanol solvent exchange, and supercritical drying to obtain aramid aerogel fibers (SEAAFs).

[0102] Fiber structure and properties: The fiber has a dense outer layer and a porous core (the opposite of the "porous outer layer and dense core" structure of this invention); the total fiber diameter is approximately 0.30 mm, and the core diameter is approximately 0.16 mm; the breaking stress is 64.3 MPa, and the thermal conductivity is 0.0283 W / (m·K). This process involves intermittent solvent exchange and freeze-drying, and is a non-continuous production process.

[0103] Comparative Example 3 Aramid nanofibers (ANF) were used as raw material (6 wt% solids content, DMSO solvent). The fibers were extruded through a single-channel spinneret (0.5 mm orifice) at an extrusion pressure of 0.02 MPa. The spun fibers were directly coagulated in a deionized water coagulation bath at room temperature (25°C) for 60 seconds. The resulting gel fibers were washed with deionized water, wound and collected without stretching, and then freeze-dried (-50°C, 48 h).

[0104] Fiber structure and properties: The fiber has a uniform internal pore structure with no obvious differentiation between the cortex and core layers; the total fiber diameter is approximately 0.40 mm; the tensile strength is only 9.2 MPa, and the thermal conductivity is 0.042 W / (m·K). This process does not employ cortex-core phase separation control or drawing, and it is an intermittent freeze-drying process.

[0105] Comparison of results: Compared to Comparative Example 1 (coaxial wet spinning at Jiangnan University, 55.2 MPa), Example 1 of this invention, through an independent high-temperature bath drafting process and a superior combination of skin / core materials, achieves a strength increase of approximately 1.5 to 2.8 times and realizes continuous production throughout the entire process. Comparative Examples 2 and 3 use high-strength aramid raw materials recognized in the art. Compared to Comparative Example 2 (two-step solidification at Tianjin University of Technology, 64.3 MPa), this invention achieves a reverse pore distribution structure (porous skin and dense core), resulting in higher strength and avoiding intermittent steps such as solvent exchange and freeze-drying. Compared to Comparative Example 3 (conventional wet spinning without skin / core structure, 9.2 MPa), this invention improves strength by an order of magnitude through skin / core phase separation control and drafting.

[0106] This invention successfully solves the technical problems of existing aerogel fibers being difficult to reconcile with strength and thermal insulation performance, and the difficulty in continuous production due to the intermittent post-processing of the preparation process.

[0107] This invention addresses the technical bottlenecks of existing aerogel fiber production processes, which struggle to achieve a balance between strength and thermal insulation performance, and rely heavily on intermittent post-processing steps, hindering continuous production. The invention proposes a continuous molding scheme for high-strength aerogel fibers based on a synergistic control technology of high- and low-temperature gradient coagulation and high-temperature bath drawing. The spinning solution is extruded through a coaxial spinneret under stable pressure, sequentially passing through a first coagulation bath (50-80℃ medium-high temperature coagulation) and a second coagulation bath (above 90℃ high-temperature drawing), followed by room temperature washing, drying, and winding, thus achieving continuous wet spinning production throughout the entire process. This process, through the synergistic effect of high and low temperature gradient solidification and high-temperature bath stretching, forms a multi-scale, multi-level structure with a porous outer layer and a dense core: the outer layer is a loose, porous structure that balances thermal insulation performance and functional requirements; the core layer is a dense network that bears the main mechanical load, with a tensile strength of 80–160 MPa and a thermal conductivity as low as 0.018–0.098 W / (m·K). This invention enables the large-scale, continuous, and stable production of high-strength aerogel fibers, which can be widely used in the preparation of high-performance aerogel fibers, composite functional fibers, and advanced thermal insulation materials.

[0108] Although the above embodiments have provided a detailed description of the present invention, they are only some embodiments of the present invention, not all embodiments. People can obtain other embodiments based on the present invention without creative effort, and these embodiments all fall within the protection scope of the present invention.

Claims

1. An aerogel fiber wet spinning device, characterized in that, It includes a gas control device, a liquid storage spinning device (3), and a multi-stage coagulation device, a drying device (14), and a winding and collecting device (15) arranged sequentially along the spinning direction. The gas control device includes a gas supply unit (1) and a gas pressure control unit (2). The spinning device (3) includes a spinning solution storage tank, a coaxial spinneret (312), and a first temperature control unit (4) connected to the spinning solution storage tank; the spinning solution storage tank includes a core spinning solution storage tank (33) and a skin spinning solution storage tank (34), which are respectively connected to the core channel and the skin channel of the coaxial spinneret; the top of the core spinning solution storage tank and the skin spinning solution storage tank are provided with air inlets, which are connected to the gas output pipeline of the air pressure control unit (2); The multi-stage coagulation device includes a first coagulation bath (5), a first drawing roller (7), a second coagulation bath (10), a second drawing roller (11), and a third coagulation bath (13) arranged sequentially along the spinning direction, as well as a second temperature control unit (6), a third temperature control unit (9), and a fourth temperature control unit (12) respectively connected to the first coagulation bath (5), the second coagulation bath (10), and the third coagulation bath (13).

2. The aerogel fiber wet spinning equipment according to claim 1, characterized in that, The first coagulation bath (5), the second coagulation bath (10) and the third coagulation bath (13) are all hollow double-walled structures, and each end is provided with an inlet (51) and an outlet (52).

3. The aerogel fiber wet spinning equipment according to claim 1, characterized in that, Detachable alumina ceramic wire pressing guides (8) are provided at the right end of the first coagulation bath, both ends of the second coagulation bath, and both ends of the third coagulation bath.

4. The aerogel fiber wet spinning equipment according to claim 1, characterized in that, The first drafting roller (7) and the second drafting roller (11) each include three drafting rollers arranged in an inverted triangle; the drying device (14) is an atmospheric pressure hot air drying device.

5. A method for preparing aerogel fibers using the aerogel fiber wet spinning equipment according to any one of claims 1 to 4, characterized in that, Includes the following steps: The sheath spinning solution and the core spinning solution are placed in the sheath spinning solution storage tank (34) and the core spinning solution storage tank (33) respectively. The temperature of the sheath-core spinning solution storage tank is controlled at 35~75℃ by the first temperature control unit (4). Under the action of air pressure, the solution is extruded through the coaxial spinneret (312) to form a spinning fine stream with a sheath-core structure. After the spun yarn is subjected to multi-stage coagulation bath treatment by a multi-stage coagulation device, it is dried by a drying device (14) and wound and collected by a winding and collecting device (15) in sequence to obtain aerogel fiber; the temperature of the first coagulation bath treatment in the multi-stage coagulation bath treatment is 30~80℃, the temperature of the second coagulation bath treatment is 90~98℃, and the temperature of the third coagulation bath treatment is 10~25℃.

6. The method according to claim 5, characterized in that, The solutes in the sheath spinning solution include polyimide, aromatic polyamide, polysulfone, cellulose, or polyacrylonitrile; the solutes in the core spinning solution include polyvinyl alcohol, polylactic acid, polyoxyethylene, chitosan, or sodium alginate.

7. The method according to claim 5 or 6, characterized in that, The mass fractions of the skin spinning solution and the core spinning solution are independently 10~30wt%.

8. The method according to claim 5, characterized in that, The pressure applied by the air pressure is 0.05~0.8MPa.

9. The method according to claim 5, characterized in that, During the second coagulation bath treatment, wet heat stretching and fiber structure orientation treatment are performed, wherein the draw ratio of the orientation treatment is 1.2 to 5.0 times.

10. The method according to claim 5, characterized in that, The aerogel fiber has a core-sheath structure, a tensile strength of 80~160MPa, and a thermal conductivity of 0.018~0.098W / (m·K).