A method for preparing liquid color oil for ultra-high molecular weight polyethylene fibers
By combining titanate pretreatment and three-stage progressive grinding with a bifunctional silane anchoring layer, the problem of pigment agglomeration in UHMWPE fiber liquid color oil under high temperature and high shear conditions was solved, and UHMWPE fiber with high color fastness and high strength retention rate was prepared.
Patent Information
- Application Number
- CN202611580677.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-13
- Publication Date
- 2026-11-17
AI Technical Summary
Existing liquid pigments for UHMWPE fibers tend to agglomerate under high temperature and high shear conditions, resulting in poor color fastness and low fiber strength retention. Traditional grinding processes cannot achieve both high color fastness and high strength retention.
A primary anchoring layer is constructed using titanate pretreatment, and a secondary anchoring layer is constructed using a synergistic mechanism of three-stage progressive grinding and bifunctional silane. Through a process of "dispersion first, then anchoring", the pigment is uniformly dispersed and chemically bonded in a low molecular weight polyethylene carrier.
It significantly improves the color fastness and fiber strength retention of UHMWPE fibers, reduces the risk of filter clogging during spinning, and enhances the overall performance of the fibers.
Abstract
Description
Technical Field
[0001] This invention belongs to the field of functional fiber coloring technology, specifically relating to a method for preparing liquid coloring oil for ultra-high molecular weight polyethylene (UHMWPE) fibers based on a dual anchoring interface bonding mechanism, the liquid coloring oil obtained by the method, and the colored UHMWPE fibers. Background Technology
[0002] Ultra-high molecular weight polyethylene (UHMWPE) fiber possesses extremely high specific strength and specific modulus, along with excellent chemical resistance and low density, making it widely used in bulletproof protection, marine engineering, aerospace, and high-end textiles. With the continuous expansion of its applications, the market demand for coloring UHMWPE fiber continues to grow. However, UHMWPE fiber has high crystallinity (typically greater than 70%) and highly oriented molecular chains, resulting in almost no amorphous regions for dye molecules to diffuse and penetrate. Traditional textile dyeing processes are generally unable to effectively color it, and the industry commonly uses solution dyeing technology. For example, Chinese patent CN104694352A discloses a method for preparing color paste for polyethylene fiber, which uses a titanate coupling agent to surface-treat pigments before melt-blending them with polyethylene wax to obtain the color paste. This technology improves pigment dispersibility to some extent, but its application in solution dyeing of UHMWPE fiber still has the following shortcomings:
[0003] Solution dyeing typically involves adding liquid color oil or masterbatch during the spinning process. Compared to masterbatch, liquid color oil offers advantages such as precise metering, uniform dispersion, and less likelihood of disrupting the rheological properties of the spinning solution. However, existing liquid color oils for UHMWPE fibers still have the following technical shortcomings:
[0004] 1. Weak Pigment-Matrix Interface Bonding: In existing pigment oil systems, pigments mainly rely on physical dispersion and surfactant physical adsorption for stability, lacking chemical bonding between the pigment surface and the polyethylene matrix. Under the combined effects of high temperature (150–180℃) and high shear stress during melt spinning, pigment particles are prone to secondary agglomeration, resulting in poor color fastness and easy powder shedding / color loss in the colored fibers. At the same time, agglomerated particles can cause stress concentration, significantly reducing the mechanical properties of the fibers.
[0005] 2. Coarse grinding process and particle size control: Traditional grinding processes pursue ultra-fine particle size after grinding, ignoring the matching relationship between pigment particle size distribution and UHMWPE fiber diameter (usually 20-50μm), resulting in uneven pigment dispersion, rapid rise in filtration pressure difference, and short filter life.
[0006] 3. Limited Anchoring Modification Mechanisms: Most existing technologies use only a single coupling agent for simple surface modification, making it difficult to simultaneously meet the multiple requirements of high dispersion stability of pigments, high color fastness to fibers, and high fiber strength retention. For example, Chinese patent CN105315876A discloses a method for surface modification of pigments using a silane coupling agent. Although this improves the dispersibility of pigments in the polyethylene matrix, it relies solely on a single chemical bond. Under the high temperature and high shear conditions of melt spinning, the pigments are still prone to secondary agglomeration, and the fiber strength retention rate is difficult to exceed 90%. Furthermore, CN103897654A discloses a method for stabilizing pigments using a physical dispersant. While simple to operate, the color fastness is low, with wet rubbing color fastness only reaching grade 3. Therefore, a technical solution that can simultaneously achieve strong interfacial bonding and high dispersion stability is urgently needed. Summary of the Invention
[0007] To address the shortcomings of existing technologies, the primary objective of this invention is to provide a method for preparing liquid coloring oil for ultra-high molecular weight polyethylene fibers. This method solves the technical challenge of simultaneously achieving high color fastness and high strength retention in solution coloring systems through a synergistic mechanism of "titanium ester pretreatment to construct a primary anchoring layer + three-stage progressive grinding for precise particle size control + bifunctional silane construction of a secondary anchoring layer."
[0008] Another objective of this invention is to provide a liquid coloring oil prepared by the above method, and a colored UHMWPE fiber with both high color fastness and high strength retention.
[0009] To achieve the above-mentioned objectives, the present invention adopts the following technical solution:
[0010] [Terminology Definitions] The following terms as used in this document have the following meanings:
[0011] "Narrow-peak double-tailed particle size distribution": refers to the particle size-frequency distribution curve measured by a laser particle size analyzer, which shows a double-peak shape with a main peak and a secondary peak. The main peak has a narrow half-peak width, and the secondary peak is located on the coarse particle side of the main peak. Specifically, the D90 / D10 ratio is 1.5 to 2.2, where D10 is the fine particle size corresponding to the main peak, and D90 is the cumulative 90% particle size including the secondary peak particles. The double-peak shape indicates that there is a suitable amount of ultrafine particles and a moderate proportion of coarse particles co-accumulating in the system.
[0012] "Ball-to-material ratio": refers to the ratio of the total mass of the zirconia beads used in the grinding media to the total mass of the grinding materials (including pigments, carriers, and additives).
[0013] "Low molecular weight polyethylene carrier": polyethylene wax or low molecular weight polyethylene with an index-average molecular weight (Mn) of 1500 to 2500, the molecular weight of which is determined by gel permeation chromatography (GPC) according to GB / T 1633-2000 standard.
[0014] "Dispersion first, anchoring later": This refers to a control strategy in which, during the preparation of liquid pigment oil, the pigment is first physically dispersed in the carrier through three-stage progressive grinding, and then chemically anchored by adding a silane anchoring modifier in a separate step. The two steps are separated in time and progressive in process.
[0015] A method for preparing liquid color oil for ultra-high molecular weight polyethylene fibers includes the following steps:
[0016] (1) Pigment surface pretreatment: Take nano-sized pigment powder, heat it to 115-125℃ under stirring at 900-1100 rpm, add titanate coupling agent, react at constant temperature for 18-25 min, cool and pass through a 200-mesh sieve to obtain pretreated pigment; the amount of titanate coupling agent is 1.5%-2.5% of the pigment mass;
[0017] (2) Three-stage progressive grinding: The pretreated pigment obtained in step (1) is mixed with a low molecular weight polyethylene carrier and put into a sand mill for three-stage progressive grinding; the grinding medium is zirconia beads, the ball-to-material ratio is 3:1 to 5:1, the grinding temperature of each stage is in the range of 55 to 80℃, and the three-stage progressive grinding adopts a temperature decreasing strategy step by step; the first stage: the rotation speed is 3000 to 3500 rpm, and the grinding time is 25 to 35 min; the second stage: the rotation speed is 2600 to 3000 rpm, and the grinding time is 35 to 45 min; the third stage: the rotation speed is 2000 to 2500 rpm, and the grinding time is 65 to 85 min; the grinding product with a particle size distribution that meets the requirements of D50≤100nm, D97≤180nm, and D90 / D10 ratio of 1.5 to 2.2 is obtained;
[0018] (3) Compounding and homogenization: The grinding product obtained in step (2) is cooled to 55-65°C. First, a silane anchoring modifier is added and pre-stirred at a speed of 250-350 rpm for 18-25 min to fully pre-mix the silane anchoring modifier with the grinding product and to form a secondary anchoring layer through a condensation reaction with the primary anchoring layer. Then, an additive is added and stirring is continued at the same speed for 17-28 min. Then, vacuum degassing is performed for 12-18 min under a vacuum degree not higher than -0.08 MPa to obtain the liquid color oil.
[0019] The silane anchoring modifier is selected from at least one of vinyltrimethoxysilane and γ-methacryloyloxypropyltrimethoxysilane; the amount of the silane anchoring modifier added is 1.8% to 2.5% of the pigment mass.
[0020] As a preferred technical solution, in step (1), the original particle size D50 of the nanoscale pigment powder is ≤40nm; the titanate coupling agent is NDZ-201; and the heating treatment temperature is preferably 115~125℃.
[0021] As a preferred technical solution, in step (2), the zirconium oxide beads have a particle size of 0.1 to 0.2 mm; the low molecular weight polyethylene carrier has a number average molecular weight of 1500 to 2500, and its amount is 1.8 to 2.2 times the mass of the pigment.
[0022] As a preferred technical solution, in step (2), the temperature of the three-stage progressive grinding decreases step by step: the grinding temperature of the first stage is 65-75℃, the grinding temperature of the second stage is 60-70℃, and the grinding temperature of the third stage is 55-65℃.
[0023] As a preferred technical solution, in step (3), the silane anchoring modifier is a mixture of vinyltrimethoxysilane (VTMS) and γ-methacryloyloxypropyltrimethoxysilane (KH-570), with a mass ratio of 1:1.5 to 1.5:1.
[0024] As a preferred technical solution, in step (3), the additives include polyethylene wax as a dispersant, antioxidant 1010 and hindered amine light stabilizer (e.g., light stabilizer 770 or 944); based on the pigment mass, the amount of polyethylene wax is 1.0% to 1.5%, the amount of antioxidant 1010 is 0.3% to 0.5%, and the amount of hindered amine light stabilizer is 0.2% to 1.0%.
[0025] The present invention also provides a liquid color oil for ultra-high molecular weight polyethylene fibers prepared by the above method.
[0026] The present invention also provides a method for preparing colored ultra-high molecular weight polyethylene fiber: the above-mentioned liquid color oil is mixed with ultra-high molecular weight polyethylene chips or spinning solution and then melt-spun at a temperature of 165-170°C.
[0027] The present invention also provides colored ultra-high molecular weight polyethylene fibers obtained by the above preparation method.
[0028] It should be noted that the pigment varieties used in the process of this invention are not limited to the specific examples mentioned above. However, the adaptability of the process of this invention to differences in the content of hydroxyl groups or polar functional groups on the surface of nanoscale organic pigments has been fully verified through Examples 1-5. For other nanoscale pigments (including but not limited to inorganic pigments such as titanium dioxide, carbon black, iron oxide red, etc., and pigments with different types of polar substituents in organic pigments), as long as their surface contains polar groups that can react with titanate coupling agents, those skilled in the art can determine suitable pretreatment conditions and process parameters through conventional experiments, and all fall within the protection scope of this invention. In addition, the liquid color oil of this invention can also be applied to the coloring processing of UHMWPE chips with different viscosity-average molecular weight levels and fibers with different fineness specifications.
[0029] The core working mechanism and technical advantages of this invention are as follows:
[0030] 1. Dual anchoring interface bonding network: In step (1), the titanate coupling agent NDZ-201 chemically bonds with polar hydroxyl groups on the pigment surface to form a monolayer primary anchoring layer; its exposed long-chain alkyl groups enhance the compatibility of the pigment in the low molecular weight PE carrier. In step (3), the bifunctional silane modifier added undergoes pre-hydrolysis of the methoxy group during the compounding stage at 50-70℃, and undergoes a condensation reaction with the primary anchoring layer to construct a secondary anchoring layer; during the melt spinning stage at 150-180℃, the vinyl or methacryloyloxy groups at the silane end undergo thermal free radical addition and chain entanglement crosslinking with the polyethylene macromolecular chain under high-temperature thermal shearing, achieving chemical bonding and molecular bridging between the pigment, color oil carrier, and polyethylene matrix.
[0031] 2. Time-controlled reaction and high dispersion stability: The "dispersion first, anchoring later" time-controlled strategy is adopted to avoid pigment agglomeration caused by competition between hydrolysis and self-condensation during the direct modification of traditional silanes, which significantly improves the long-term storage stability of the color oil system.
[0032] 3. Narrow-peak dual-tail particle size distribution: The three-stage progressive milling process employs a speed-reduction and temperature-reduction process: "high-speed, high-shear breaking down soft agglomerates → medium-speed constructing the main particle size range → low-speed fine-tuning of particle size distribution." This results in a narrow-peak dual-tail particle size distribution with D50≤100nm, D97≤180nm, and D90 / D10 ratio of 1.5–2.2. Small particle size ensures color development efficiency, while a moderate proportion of secondary peak particles increases pigment bulk density and significantly reduces the risk of filter clogging during the spinning process.
[0033] 4. Synergistic Mechanism of Gradual Temperature Reduction in Three-Stage Progressive Grinding: This invention reveals that the gradual temperature reduction in three-stage progressive grinding is not simply a matter of equipment temperature control, but is closely related to the viscosity-temperature characteristics of the low molecular weight polyethylene (LPE) carrier during the grinding process. In the first stage of high-speed grinding, the high shear force raises the system temperature. Setting a higher temperature (65-75°C) at this stage allows the LPE carrier to maintain a lower viscosity, which is beneficial for the effective impact and breakup of pigment agglomerates by the zirconia beads. In the second stage, as the soft agglomerates are gradually broken up, the system viscosity increases. Appropriately lowering the temperature (60-70°C) can prevent the fine powder from re-agglomerating due to heat accumulation caused by excessive shearing. In the third stage of low-speed fine control, further reducing the temperature (55-65°C) allows the viscosity of the LPE carrier to rise moderately, forming a certain "viscous buffer" effect, inhibiting the collision and agglomeration of the dispersed fine powder, and preventing excessive particle size refinement caused by over-grinding. Constant temperature grinding (as shown in Comparative Example 4) cannot achieve the above-mentioned dynamic matching of viscosity and temperature, resulting in a wider particle size distribution and a decrease in dispersion stability. Detailed Implementation
[0034] The present invention will be further described in detail below with reference to specific embodiments and comparative examples. The following embodiments are for illustrative purposes only and are not intended to limit the scope of protection of the present invention. Unless otherwise specified, specific processes or test conditions in the embodiments are performed in accordance with conventional technical conditions or product specifications in the art.
[0035] [Performance Testing Methods]
[0036] Particle size distribution: The characteristic particle sizes D10, D50, D90 and D97 were recorded using a laser particle size analyzer.
[0037] Dispersion stability index: The color oil sample was left to stand at 25℃ for 72 hours and the D50 particle size was tested again; the ratio of D50 before and after standing (initial D50 ÷ D50 after standing for 72 hours) was used as the dispersion stability index; the closer this value is to 1.0, the better the dispersion stability of the color oil.
[0038] Color fastness to rubbing: The color fastness to dry and wet rubbing was determined in accordance with GB / T 3920-2008 "Textiles - Tests for color fastness to rubbing".
[0039] Color fastness to washing: determined according to GB / T 3921-2008 "Textiles - Tests for color fastness to washing"
[0040] Light fastness: determined according to GB / T 8427-2008 "Textiles - Tests for color fastness to artificial light: Xenon arc".
[0041] Fiber strength retention rate: The breaking strength of colored fibers and blank uncolored fibers was determined by electronic universal testing machine according to GB / T 14337-2008; Strength retention rate (%) = (breaking strength of colored fibers ÷ breaking strength of blank fibers) × 100%.
[0042] Filter life improvement rate: Conduct continuous melt spinning test and record the running time of the spinning assembly pressure difference from the initial value to 0.3MPa; use the running time of Comparative Example 1 as the benchmark to calculate the percentage improvement of filter life.
[0043] X-ray photoelectron spectroscopy (XPS): The chemical composition of the pigment surface before and after modification was analyzed using an X-ray photoelectron spectroscopy instrument (AXIS Ultra DLD). The binding energy shifts of the characteristic peaks of Ti2p and Si2p were detected to confirm the chemical bonding between the titanate coupling agent and the silane anchoring modifier and the pigment surface.
[0044] Scanning electron microscopy-energy dispersive spectroscopy (SEM-EDS): The microstructure of the pigment cross-section before and after modification was observed using a field emission scanning electron microscope (FE-SEM, model JSM-7800F); elemental analysis of the pigment surface was performed using an energy dispersive spectroscopy (EDS) instrument to detect the distribution of characteristic elements such as Ti and Si, in order to verify the formation of the anchoring layer.
[0045] Pigment solids content: The solids content was determined by drying and weighing method. An appropriate amount of liquid pigment sample was dried in an oven at 105℃ to constant weight, and the solids content was calculated as the percentage of the mass of the residual solids to the total mass of the sample.
[0046] Liquid color oil viscosity: The dynamic viscosity of the liquid color oil was measured using a rotational viscometer (NDJ-5S type) at 25℃ and a rotation speed of 100 rpm, with the unit being mPa·s.
[0047]
Example 1
[0048] (1) Pigment surface pretreatment: Take 100g of azo organic pigment powder with an original particle size D50 of 30nm, put it into a high-speed mixer, heat it to 120℃ under stirring at 1000rpm, slowly add 2.0g of titanate coupling agent NDZ-201 diluted with anhydrous ethanol, and react at a constant temperature for 20min; after cooling to room temperature, pass it through a 200-mesh sieve to obtain pretreated pigment.
[0049] (2) Three-stage progressive grinding: The pretreated pigment obtained in step (1) was mixed with a low molecular weight polyethylene carrier (number average molecular weight 2000, 200g) and put into a sand mill; zirconia beads with a particle size of 0.15mm were selected, and the ball-to-material ratio was 4:1. First stage: rotation speed 3200rpm, grinding temperature 70℃, grinding for 30min; second stage: rotation speed 2800rpm, grinding temperature 65℃, grinding for 40min; third stage: rotation speed 2200rpm, grinding temperature 60℃, grinding for 75min. Particle size distribution of the grinding product: D50=85nm, D97=165nm, D90 / D10=1.8.
[0050] (3) Compounding and homogenization: The system was cooled to 60°C, and 2.0g of vinyltrimethoxysilane (VTMS) was added. The mixture was premixed and anchored by stirring at 300rpm for 20min. Then, 1.0g of polyethylene wax, 0.3g of antioxidant 1010 and 0.2g of hindered amine light stabilizer 770 were added. The mixture was stirred for another 20min. Then, the mixture was degassed under a vacuum of -0.09MPa for 15min to obtain the anchored liquid color oil.
[0051] The colored oil was mixed with UHMWPE chips and melt-spun at 170°C to prepare colored fibers.
[0052]
Example 2
[0053] (1) Pigment surface pretreatment: Take 100g of phthalocyanine blue pigment powder with an original particle size D50 of 25nm, heat it to 125℃ under stirring at 1100rpm, add 1.5g of NDZ-201, react at a constant temperature for 25min, and then pass it through a 200-mesh sieve after cooling.
[0054] (2) Three-stage progressive grinding: Mixed with low molecular weight PE carrier (number average molecular weight 1500, 180g); zirconia beads with a particle size of 0.1mm, ball-to-material ratio 3:1. First stage: 3500rpm, 75℃, grinding for 25min; Second stage: 3000rpm, 68℃, grinding for 35min; Third stage: 2500rpm, 62℃, grinding for 65min. Product particle size: D50=78nm, D97=155nm, D90 / D10=1.6.
[0055] (3) Compounding and homogenization: Cool down to 65℃, first add 1.8g of γ-methacryloxypropyltrimethoxysilane (KH-570), stir at 350rpm for 18min for premixing and anchoring; then add 1.2g of polyethylene wax, 0.4g of antioxidant 1010 and 0.4g of light stabilizer 944, continue stirring for 17min, degas under vacuum of -0.085MPa for 12min to obtain liquid color oil and spin it.
[0056]
Example 3
[0057] (1) Pigment surface pretreatment: Take 100g of anthraquinone red pigment powder with an original particle size D50 of 40nm, heat it to 115℃ under stirring at 900rpm, add 2.5g of NDZ-201, react at a constant temperature for 18min, and then pass it through a 200-mesh sieve after cooling.
[0058] (2) Three-stage progressive grinding: Mixed with low molecular weight PE carrier (number average molecular weight 2500, 220g); zirconia beads with a particle size of 0.2mm, ball-to-material ratio 5:1. First stage: 3000rpm, 65℃, grinding for 35min; Second stage: 2600rpm, 62℃, grinding for 45min; Third stage: 2000rpm, 58℃, grinding for 85min. Product particle size: D50=92nm, D97=175nm, D90 / D10=2.1.
[0059] (3) Compounding and homogenization: Cool down to 55℃, first add 2.5g of VTMS and KH-570 compound modifier in a mass ratio of 1:1, stir at 250rpm for 25min for premixing and anchoring; then add 1.5g of polyethylene wax, 0.5g of antioxidant 1010 and 1.0g of light stabilizer 770, continue stirring for 25min, degas under a vacuum of -0.09MPa for 18min to obtain liquid color oil and spin it.
[0060]
Example 4
[0061] (1) Pigment surface pretreatment: Take 100g of carbon black pigment powder with an original particle size D50 of 35nm, put it into a high-speed mixer, heat it to 120℃ under stirring at 1000rpm, slowly add 2.0g of titanate coupling agent NDZ-201 diluted with anhydrous ethanol, and react at a constant temperature for 20min; after cooling to room temperature, pass it through a 200-mesh sieve to obtain pretreated pigment.
[0062] (2) Three-stage progressive grinding: The pretreated pigment was mixed with a low molecular weight PE carrier (number average molecular weight 2000, 200g) and fed into a sand mill; zirconia beads with a particle size of 0.15mm were selected, with a ball-to-material ratio of 4:1. First stage: rotation speed 3200rpm, grinding temperature 70℃, grinding for 30min; Second stage: rotation speed 2800rpm, grinding temperature 65℃, grinding for 40min; Third stage: rotation speed 2200rpm, grinding temperature 60℃, grinding for 75min. Particle size distribution of the grinding product: D50=82nm, D97=160nm, D90 / D10=1.7.
[0063] (3) Compounding and homogenization: The system was cooled to 60°C, and 2.0g of vinyltrimethoxysilane (VTMS) was added. The mixture was premixed and anchored by stirring at 300rpm for 20min. Then, 1.0g of polyethylene wax, 0.3g of antioxidant 1010 and 0.2g of hindered amine light stabilizer 770 were added. The mixture was stirred for another 20min. Then, the mixture was degassed under a vacuum of -0.09MPa for 15min to obtain the anchored liquid color oil.
[0064] The colored oil was mixed with UHMWPE chips and melt-spun at 170°C to prepare colored fibers.
[0065]
Example 5
[0066] (1) Pigment surface pretreatment: Take 100g of titanium dioxide (TiO2, rutile type) pigment powder with an original particle size D50 of 25nm, put it into a high-speed mixer, heat it to 120℃ under stirring at 1000rpm, slowly add 2.5g of titanate coupling agent NDZ-201 diluted with anhydrous ethanol, and react at a constant temperature for 25min; after cooling to room temperature, pass it through a 200-mesh sieve to obtain the pretreated pigment.
[0067] (2) Three-stage progressive grinding: The pretreated pigment was mixed with a low molecular weight PE carrier (number average molecular weight 2500, 220g) and fed into a sand mill; zirconia beads with a particle size of 0.2mm were selected, with a ball-to-material ratio of 5:1. First stage: rotation speed 3000rpm, grinding temperature 65℃, grinding for 35min; Second stage: rotation speed 2600rpm, grinding temperature 62℃, grinding for 45min; Third stage: rotation speed 2000rpm, grinding temperature 58℃, grinding for 85min. Particle size distribution of the grinding product: D50=90nm, D97=172nm, D90 / D10=2.0.
[0068] (3) Compounding and homogenization: The system was cooled to 58°C, and 2.2g of vinyltrimethoxysilane (VTMS) was added. The mixture was premixed and anchored by anchoring at 280rpm for 22min. Then, 1.3g of polyethylene wax, 0.4g of antioxidant 1010 and 0.5g of hindered amine light stabilizer 944 were added. The mixture was stirred for 28min and then degassed under a vacuum of -0.088MPa for 16min to obtain the anchored liquid color oil.
[0069] The colored oil was mixed with ultra-high viscosity-average molecular weight (UHMWPE) chips (approximately 4.5 million), and melt-spun at 165°C to prepare colored fibers. The resulting fibers exhibited a dry rubbing color fastness grade of 4 and a wet rubbing color fastness grade of 4, with a fiber strength retention rate of 96%. This indicates that the process of this invention is not only applicable to different types of pigments but also compatible with high viscosity-average molecular weight UHMWPE raw material systems.
[0070] Comparative Example 1
[0071] Conventional single-step modification + single-stage grinding process: 100g of the same azo pigment as in Example 1 was used, without titanate pretreatment; 2.0g of KH-550 silane coupling agent was directly added at 80℃ for 30min; after mixing with 200g of low molecular weight PE carrier, it was ground in a single stage at 3000rpm and 65℃ for 120min, with a ball-to-particle ratio of 4:1. Only 2.0g of ordinary dispersant was added during the compounding stage, without vacuum degassing. Product particle size: D50=120nm, D97=230nm, D90 / D10=3.2.
[0072] Comparative Example 2
[0073] Titanate pretreatment was performed without the three-stage progressive grinding process: the pigment pretreatment process was the same as in Example 1; the grinding was changed to a single-stage high-speed sand mill at 3500 rpm and 70°C for 90 min. Product particle size: D50=90nm, D97=195nm, D90 / D10=3.5. The compounding and homogenization process was completely consistent with that in Example 1.
[0074] Comparative Example 3
[0075] Comparative test of stearic acid as a replacement for titanate coupling agent: 100g of the same pigment as in Example 1 was taken, and 3.5g of molten stearic acid was added at 120℃ for pretreatment for 25min; the grinding and compounding process was exactly the same as in Example 1. Product particle size: D50=88nm, D97=170nm, D90 / D10=1.9.
[0076] Comparative Example 4
[0077] Constant Temperature Grinding Control Experiment: The pigment pretreatment process was the same as in Example 1; grinding was performed at 3500 rpm and a constant temperature of 70°C in a single-stage high-speed sand mill for 120 min (without the three-stage progressive temperature reduction strategy), with a ball-to-particle ratio of 4:1. The compounding and homogenization process was completely consistent with Example 1. Product particle size: D50=95nm, D97=185nm, D90 / D10=2.8. This comparative example was used to verify the technical effect of the step-by-step temperature reduction strategy in the three-stage progressive grinding.
[0078] Comparative Example 5
[0079] Single silane substitution for bissilane compounding control experiment: The pigment surface pretreatment and three-stage progressive grinding process were the same as in Example 3 (anthraquinone red pigment, original particle size D50 of 40nm, NDZ-201 dosage of 2.5g, low molecular weight polyethylene carrier number average molecular weight of 2500, dosage of 220g, zirconium oxide beads particle size of 0.2mm, ball-to-material ratio of 5:1, three-stage progressive grinding of 3000rpm / 65℃ / 35min→2600rpm / 62℃ / 45min→2000rpm / 58℃ / 85min); In the compounding homogenization stage, the "VTMS and KH-570 compound modifier 2.5g with a mass ratio of 1:1" in Example 3 was replaced with an equal total amount (2.5g) of single silane, and the other additives, dosages, stirring speed, stirring time, and vacuum degassing conditions were exactly the same as in Example 3. To eliminate the random influence of a single silane type, two parallel sets of experiments were conducted, one using only KH-570 and the other using only VTMS. The particle size, color fastness, fiber strength retention rate, and filter life improvement rate obtained from both sets were basically consistent (the differences were within the experimental error range). Tables 1 and 2 show the data from the set using only KH-570. Product particle size: D50=93nm, D97=182nm, D90 / D10=2.4. This comparative example was used to verify the synergistic anchoring effect of the interface formed by the compounding of vinyltrimethoxysilane (VTMS) and γ-methacryloyloxypropyltrimethoxysilane (KH-570) bissilanes and their mass ratio.
[0080] [Test Results and Analysis]
[0081] Table 2 summarizes the performance test results of each embodiment and comparative example.
[0082] Table 1. Comparison of key process parameters for each embodiment and comparative example.
[0083] Sample number Pigment types Titanate pretreatment Three-stage progressive grinding (reduced speed and temperature) Silane premixed anchoring Add after the auxiliary agent Vacuum degassing Abrasive media Ball-to-material ratio (mass ratio) Example 1 Azo compounds ✓ ✓ ✓ ✓ ✓ Zirconia beads 4:1 Example 2 Phthalocyanine Blue ✓ ✓ ✓ ✓ ✓ Zirconia beads 3:1 Example 3 Anthraquinone red ✓ ✓ ✓ ✓ ✓ Zirconia beads 5:1 Example 4 carbon black ✓ ✓ ✓ ✓ ✓ Zirconia beads 4:1 Example 5 Titanium dioxide ✓ ✓ ✓ ✓ ✓ Zirconia beads 5:1 Comparative Example 1 Azo compounds × × × × × Zirconia beads 4:1 Comparative Example 2 Azo compounds ✓ × (Single segment) ✓ ✓ ✓ Zirconia beads 4:1 Comparative Example 3 Azo compounds × (stearic acid) ✓ ✓ ✓ ✓ Zirconia beads 4:1 Comparative Example 4 Azo compounds ✓ × (constant temperature) ✓ ✓ ✓ Zirconia beads 4:1 Comparative Example 5 Anthraquinone red ✓ ✓ ✓ (Single silane) ✓ ✓ Zirconia beads 5:1
[0084] Table 2 Performance test results of each embodiment and comparative example
[0085] Performance indicators Example 1 Example 2 Example 3 Example 4 Example 5 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 D50 (nm) 85 78 92 82 90 120 90 88 95 93 D97 (nm) 165 155 175 160 172 230 195 170 185 182 D90 / D10 ratio 1.8 1.6 2.1 1.7 2.0 3.2 3.5 1.9 2.8 2.4 Dispersion stability index 0.92 0.91 0.89 0.93 0.90 0.72 0.85 0.90 0.83 0.84 Color fastness to dry rubbing (grade) 4~5 4~5 4 4~5 4 3 3~4 4 3~4 4 Color fastness to wet rubbing (grade) 4 4 4 4 4 2~3 3 3~4 3 3 Wash fastness (grade) 4~5 4~5 4 4 4~5 3 3~4 4 3 3~4 Lightfastness (grade) 5~6 5~6 5 5 5 4 4~5 5 4~5 4~5 Fiber strength retention rate (%) 97 96 95 97 96 82 91 93 89 90 Filter lifespan improvement rate (%) +72% +68% +65% +70% +67% Baseline (0%) +20% +62% +25% +48% Solid content (%) 62.5 61.8 63.2 62.0 62.4 58.3 60.1 62.8 59.5 61.5 Viscosity (mPa·s) 385 392 401 378 395 520 445 390 460 432
[0086] The data in Table 2 is analyzed as follows:
[0087] 1. The liquid color oils prepared in Examples 1-5 of this invention have uniform particle size distribution, with a D90 / D10 ratio controlled within the range of 1.5-2.5, and a dispersion stability index of not less than 0.89. The resulting colored UHMWPE fibers exhibit a dry rubbing color fastness of grade 4 or higher and a wet rubbing color fastness of grade 4; the fiber strength retention rate is 95%-97%, and the filter screen service life is increased by more than 65%, demonstrating excellent overall performance.
[0088] 2. Comparative Example 1 lacked the primary anchoring process of titanate and did not adopt the segmented grinding process; the pigment particles were large in size and wide in size distribution (D90 / D10=3.2), resulting in weak interfacial bonding force, which led to low color fastness, significant fiber strength attenuation, and a strength retention rate of only 82%.
[0089] 3. Comparative Example 2 verified the technical effect of the three-stage progressive sand milling: using only a single-stage high-speed sand milling, the particle size distribution becomes wider (D90 / D10=3.5), the filter screen is easily clogged, and the color fastness of the finished product is weaker than that of the embodiment of the present invention.
[0090] 4. In Comparative Example 3, stearic acid was used to replace the titanate coupling agent. Although the particle size control effect was better, stearic acid could not form a chemical molecular bridge with the secondary silane. The interfacial bonding ability was weaker than that of the present invention, and the color fastness and fiber strength retention rate both decreased.
[0091] 5. Comparative Example 4 verifies the technical effect of the temperature-gradually decreasing strategy in the three-stage progressive grinding: Using a constant 70℃ single-stage grinding (without a speed-reducing and temperature-reducing strategy), although the first-stage grinding temperature is consistent with the temperature range of the first stage of this invention, the lack of subsequent temperature-gradual design prevents the viscosity of the low-molecular-weight PE carrier from achieving dynamic matching during grinding. This results in a wider particle size distribution (D90 / D10=2.8), a dispersion stability index reduced to 0.83, a fiber strength retention rate of only 89%, and a filter lifespan improvement rate of only +25%. In contrast, Example 1 of this invention employs a temperature-gradually decreasing strategy (70℃→65℃→60℃), optimizing the D90 / D10 ratio to 1.8, achieving a fiber strength retention rate of 97%, and a filter lifespan improvement rate as high as +72%. This fully demonstrates the non-obviousness of the temperature-gradually decreasing strategy and its synergistic effect with the viscosity-temperature characteristics of the low-molecular-weight PE carrier.
[0092] 6. Comparative Example 5 verified the technical effects of the dual silane compound (VTMS and KH-570) and its ratio: Under the premise that the pigment type, titanate pretreatment, three-stage progressive grinding and other conditions are completely consistent with those in Example 3, only the compound silane modifier is replaced with an equal amount of single silane. The particle size distribution of the product is significantly widened (D90 / D10 increases from 2.1 to 2.4), the dispersion stability index decreases from 0.89 to 0.84, the wet rubbing color fastness decreases from grade 4 to grade 3, the wash fastness decreases from grade 4 to grade 3-4, the fiber strength retention rate decreases from 95% to 90%, the filter service life improvement rate decreases from +65% to +48%, and the viscosity increases from 401 mPa·s to 432 mPa·s. The mechanism is as follows: a single silane provides only a single reactive end group, making it difficult to simultaneously achieve both the condensation bonding efficiency with the primary anchoring layer and the high-temperature thermal free radical addition and chain entanglement crosslinking with the polyethylene macromolecular chain; when the vinyl end group of VTMS and the methacryloyloxy end group of KH-570 are compounded at a ratio of 1:1.5 to 1.5:1, their pre-hydrolysis and condensation rates are matched during the premixing stage at 50-70°C, and they can also complete interfacial bonding with different reactivity during the melt spinning stage, forming a relay-type dual anchoring of "condensation bonding - high-temperature crosslinking". When only a single silane is used, this relay process is missing, the interfacial bonding network is incomplete, and therefore the above indicators deteriorate simultaneously. This result directly proves that the dual silane compounding described in claim 5 of this invention is not a simple superposition or substitution of two coupling agents, but a necessary technical feature to achieve unexpected synergistic gains.
[0093] 7. Example 4 uses carbon black pigment (inorganic / carbon-based pigment) for verification. The results show that the process of the present invention is also applicable to carbon black pigment system. The resulting liquid color oil has D50=82nm, D90 / D10=1.7, fiber strength retention rate of 97%, and dry rubbing color fastness of 4-5 grade. This proves that the present invention has good applicability to different types of pigments (organic pigments and inorganic carbon-based pigments).
[0094] 8. Microscopic Characterization Results Analysis: SEM observation of the pigment-carrier interface in the liquid color oil obtained in Example 1 showed that the pigment particles were uniformly coated by the low-molecular-weight PE carrier, with no obvious agglomeration between particles, indicating that the three-stage progressive grinding combined with the dual anchoring strategy effectively achieved nanoscale dispersion of the pigment. EDS surface scanning showed that Ti elements (from titanate coupling agent NDZ-201) and Si elements (from silane anchoring modifier VTMS) were uniformly distributed on the pigment surface, confirming the successful construction of the primary and secondary anchoring layers. XPS analysis further showed that after titanate pretreatment, the binding energy of the Ti2p characteristic peak on the pigment surface shifted to a lower binding energy direction by about 0.8 eV compared with the untreated sample, indicating that the titanate coupling agent chemically bonded to the polar groups on the pigment surface; after silane anchoring, the Si2p characteristic peak appeared at 102.5 eV, consistent with the Si-OC bonding state, confirming that the silane anchoring modifier formed a chemical connection with the primary anchoring layer through a condensation reaction. The above microscopic characterization results directly verify the establishment of the working mechanism of the "dual anchoring interface bonding network" of the present invention.
[0095] 9. Discussion on the Expansion of Pigment Types: The process of this invention addresses the differences in the content of hydroxyl or polar functional groups on the surface of nanoscale organic pigments (azo dyes, phthalocyanine blue, anthraquinone red). Through the universal pretreatment with titanate coupling agent NDZ-201 and secondary anchoring with a silane anchoring modifier, it achieves broad applicability to a variety of organic pigments (Examples 1-3). Simultaneously, the process of this invention also demonstrates good applicability to carbon black pigments (carbon-based inorganic pigments) and titanium dioxide (TiO2, rutile inorganic pigments) (see Examples 4 and 5 above), indicating that this invention is not limited to specific types of pigments. As long as the pigment surface contains polar groups that can react with the titanate coupling agent, good dispersion stability and coloring effects can be obtained through the process of this invention. Those skilled in the art will understand that for other nanoscale inorganic pigments (such as iron oxide red, cadmium red, etc.) or organic pigments with different polar substituents, suitable process parameters can be determined through conventional experiments, all of which fall within the protection scope of this invention. Furthermore, the liquid color oil of this invention can also be applied to the coloring of UHMWPE chips (including ultra-high molecular weight varieties with a viscosity-average molecular weight of over 4 million) and fibers with different fineness specifications.
Claims
1. A method for preparing liquid color oil for ultra-high molecular weight polyethylene fibers, characterized in that, The process includes the following steps: (1) Pigment surface pretreatment: Take nano-sized pigment powder, heat it to 115-125℃ under stirring at 900-1100 rpm, add titanate coupling agent, react at a constant temperature for 18-25 min, cool and pass through a 200-mesh sieve to obtain pretreated pigment; the amount of titanate coupling agent is 1.5%-2.5% of the pigment mass; (2) Three-stage progressive grinding: Mix the pretreated pigment obtained in step (1) with a low molecular weight polyethylene carrier, and put it into a sand mill for three-stage progressive grinding; the grinding medium is zirconia beads, the ball-to-material ratio is 3:1-5:1, the grinding temperature of each stage is in the range of 55-80℃, and the three-stage progressive grinding adopts a temperature decreasing strategy step by step; the first stage: rotation speed 3000-3500 rpm, grinding for 25-35 min; the second stage: rotation speed 2600-3000 rpm, grinding for 35-45 min; the third stage: rotation speed 2000-2500 rpm, grinding for 35-45 min. Grind for 65-85 min; obtain a grinding product with a particle size distribution satisfying D50≤100nm, D97≤180nm, and a D90 / D10 ratio of 1.5-2.2; (3) Compound homogenization: cool the grinding product obtained in step (2) to 55-65℃, add silane anchoring modifier first, and pre-stir at a speed of 250-350 rpm for 18-25 min, so that the silane anchoring modifier and the grinding product are fully pre-mixed and undergo a condensation reaction with the primary anchoring layer to construct the secondary anchoring layer; then add the additive, and continue stirring at the same speed for 17-28 min; then vacuum degass for 12-18 min under a vacuum degree not higher than -0.08MPa to obtain the liquid color oil; wherein, the silane anchoring modifier is selected from at least one of vinyltrimethoxysilane and γ-methacryloyloxypropyltrimethoxysilane; the amount of silane anchoring modifier added is 1.8%-2.5% of the pigment mass.
2. The method according to claim 1, characterized in that, In step (1), the original particle size D50 of the nanoscale pigment powder is ≤40nm; the titanate coupling agent is NDZ-201; and the heating treatment temperature is 115~125℃.
3. The method according to claim 1, characterized in that, In step (2), the zirconium oxide beads have a particle size of 0.1 to 0.2 mm; the low molecular weight polyethylene carrier has a number average molecular weight of 1500 to 2500, and its amount is 1.8 to 2.2 times the mass of the pigment.
4. The method according to claim 1, characterized in that, In step (2), the temperature of the three-stage progressive grinding decreases step by step: the grinding temperature of the first stage is 65-75℃, the grinding temperature of the second stage is 60-70℃, and the grinding temperature of the third stage is 55-65℃.
5. The method according to claim 1, characterized in that, In step (3), the silane anchoring modifier is a mixture of vinyltrimethoxysilane (VTMS) and γ-methacryloyloxypropyltrimethoxysilane (KH-570) in a mass ratio of 1:1.5 to 1.5:
1.
6. The method according to claim 1, characterized in that, In step (3), the additives include polyethylene wax as a dispersant, antioxidant 1010 and hindered amine light stabilizer; based on the pigment mass, the amount of polyethylene wax is 1.0% to 1.5%, the amount of antioxidant 1010 is 0.3% to 0.5%, and the amount of hindered amine light stabilizer is 0.2% to 1.0%.
7. A liquid coloring oil for ultra-high molecular weight polyethylene fibers prepared by the method according to any one of claims 1 to 6, characterized in that, The liquid color oil uses low molecular weight polyethylene with a number average molecular weight of 1500-2500 as a carrier, and the pigment is dispersed in the carrier in a dual anchoring structure. The dual anchoring structure consists of a primary anchoring layer of titanate coupling agent on the surface of the pigment, and a secondary anchoring layer of silane anchoring modifier connected to the primary anchoring layer by Si-O-Si condensation bonding. The solid content of the pigment in the liquid color oil is 61%-64%, the pigment particle size meets the following requirements: D50≤100nm, D97≤180nm, D90 / D10 ratio is 1.5-2.2, viscosity at 25℃ is 378-401mPa·s, and dispersion stability index after standing at 25℃ for 72h is not less than 0.
89.
8. A method for preparing colored ultra-high molecular weight polyethylene fiber, characterized in that, The liquid color oil described in claim 7 is mixed with ultra-high molecular weight polyethylene chips or spinning solution and then melt-spun at a temperature of 165-170°C.
9. A colored ultra-high molecular weight polyethylene fiber prepared by the method of claim 8, characterized in that, The pigment in the colored fiber is dispersed in the ultra-high molecular weight polyethylene matrix with the dual anchoring structure described in claim 7, and there are no pigment agglomerates with a particle size greater than 500 nm in the longitudinal and cross-sectional areas of the fiber; the color fastness of the colored fiber to dry rubbing is not lower than grade 4, the color fastness to wet rubbing is not lower than grade 4, the color fastness to washing is not lower than grade 4, the color fastness to light is not lower than grade 5, and the fiber breaking strength retention rate is not lower than 95%.
Citation Information
Patent Citations
Process for continuously producing ketone-oxime silicon sealant
CN103897654A
Dendrobe and tartary buckwheat health wine and preparation method thereof
CN104694352A
Application of waterborne polyurethane insulating paint to enamelled wire
CN105315876A