A polyethylene fiber with high crystallinity orientation and its preparation method

By introducing functionalized modified carriers and nano-reinforcements into polyethylene fibers, combined with multi-level gradient extraction and hot stretching processes, the problem of anti-aging agent loss was solved, the crystallinity and creep resistance of the fibers were improved, and the long-term weather resistance and mechanical properties of the fibers were ensured.

CN123108759APending Publication Date: 2026-11-17SUZHOU CHENGFANG WEAVING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611312185.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-27
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing polymer molding technologies, anti-aging agents are easily lost during the gel spinning process, making it difficult to achieve both mechanical and anti-aging properties of polyethylene fibers. Furthermore, conventional ultraviolet absorbers disrupt the regular arrangement of the crystal lattice, reducing fiber strength.

Method used

Functionalized modified polyethylene carriers and nano-reinforcers with polar groups on their surfaces are introduced into a polyethylene matrix. Through stepwise ultrasonic pre-dispersion and in-situ reactive extrusion, combined with multi-level gradient extraction and thermal stretching processes, an intramolecular rigid anchor point and sliding network structure is constructed to achieve the curing of anti-aging components.

Benefits of technology

It improves the crystallinity, creep resistance, and interfacial adhesion of fibers to meet the stringent requirements of high-end protective fabrics and special cables, achieving a balance between long-term weather resistance and mechanical properties of fibers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108759A_ABST
    Figure CN123108759A_ABST
Patent Text Reader

Abstract

This invention relates to the field of polyethylene fiber preparation technology, specifically to a high-crystallinity polyethylene fiber and its preparation method. This invention overcomes the problem of insufficient mechanical and anti-aging properties caused by the easy loss of anti-aging agents during the gel spinning purification process of existing polyethylene fibers. This invention introduces functionalized modified polyethylene carriers and nano-reinforcers with polar groups on their surfaces into a polyethylene matrix. Through stepwise ultrasonic pre-dispersion and in-situ reactive extrusion in a mixed solvent system, a sliding network structure with intramolecular rigid anchor points and steric hindrance is constructed within the matrix. Subsequently, a multi-level gradient extraction and gradient thermal stretching process is employed to induce epitaxial crystallization of macromolecular chains using a one-dimensional template effect. This invention not only achieves minimal loss of anti-aging components to impart long-term weather resistance to the fiber, but also improves the fiber's crystallinity, creep resistance, and coating interfacial adhesion, effectively meeting the stringent weaving requirements of high-end protective fabrics and special cables.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of polyethylene fiber preparation technology, specifically to a polyethylene fiber with high crystallinity orientation and its preparation method. Background Technology

[0002] Ultra-high molecular weight polyethylene (UHMWPE) fiber, as one of the three major high-performance specialty fibers, holds an irreplaceable strategic position in national defense, aerospace, and high-performance civilian textiles due to its high specific strength and specific modulus. Current industrial production primarily employs gel spinning to prepare single-component polyethylene fibers, achieving high axial orientation of the macromolecular chains through solvent dissolution, quenching and molding, multi-stage extraction, and ultra-high thermal stretching. Therefore, the fiber must not only exhibit high breaking strength and initial modulus under sudden impact to absorb destructive kinetic energy, but also maintain stable mechanical properties under long-term outdoor exposure, marine salt spray, and repeated washing, possessing excellent long-term anti-aging and weather resistance.

[0003] However, in existing polymer molding technologies, in order to pursue high crystallinity and orientation, the process requires large molecular chains to be stretched and de-entangled significantly. If conventional UV absorbers or antioxidants are physically blended into the spinning solution at this time, these inorganic or small molecule impurities will disrupt the regular arrangement of the crystal lattice, resulting in a decrease in the stretchability and severely weakening the absolute strength of the fiber. In addition, the gel spinning process requires multi-stage solvent extraction to remove the spinning solvent. Physically added anti-aging auxiliaries will precipitate and be lost with the extract during this stage. In later outdoor fabric applications, they will also continuously migrate and be lost due to the free movement of macromolecules, leading to a decrease in the UV resistance of the fiber and causing the protective fabric to become brittle and fail.

[0004] Therefore, how to solve the problem of efficient detangling of molecular chains to achieve a breakthrough in crystal orientation in the preparation system of single-component polyethylene fibers, and how to solidify anti-aging components in the polyethylene matrix through non-physical doping, thereby achieving a balance between the mechanical properties and anti-aging properties of polyethylene fibers, has become a technical bottleneck that urgently needs to be overcome in the current chemical fiber field.

[0005] Therefore, a polyethylene fiber with high crystallinity orientation and its preparation method are proposed. Summary of the Invention

[0006] The purpose of this invention is to provide a polyethylene fiber with high crystallinity and orientation, and its preparation method. This invention overcomes the problem of insufficient mechanical and anti-aging properties caused by the easy loss of anti-aging agents during the gel spinning purification process of existing polyethylene fibers. This invention introduces a functionalized modified polyethylene carrier and nano-reinforcements with polar groups on their surface into a polyethylene matrix. Through stepwise ultrasonic pre-dispersion and in-situ reactive extrusion in a mixed solvent system, a sliding network structure with intramolecular rigid anchor points and steric hindrance is constructed within the matrix. Subsequently, a multi-level gradient extraction and gradient thermal stretching process is used to induce epitaxial crystallization of macromolecular chains using a one-dimensional template effect. This invention not only achieves less loss of anti-aging components to impart long-term weather resistance to the fiber, but also improves the fiber's crystallinity, creep resistance, and coating interfacial adhesion, effectively meeting the stringent weaving requirements of high-end protective fabrics and special cables.

[0007] To achieve the above objectives, the present invention provides the following technical solution: This invention provides a method for preparing polyethylene fibers with high crystallinity orientation, comprising the following steps: adding 0.5-2.0 parts by weight of aminated multi-walled carbon nanotubes, 0.8-1.5 parts by weight of anti-aging additives, and antioxidant 168... Mix 0.2-0.4 parts of polyethylene with 150-300 parts of decahydronaphthalene, and ultrasonically treat at 35-45℃ with an ultrasonic frequency of 20-40kHz and an ultrasonic power of 800-1200W for 25-40 minutes to obtain an ultrasonic system. Add 3-6 parts of modified polyethylene and 500-750 parts of white oil to the ultrasonic system, heat to 70-80℃, and mechanically stir at 300-500 rpm for 25-40 minutes to obtain a mixed system. Add 100 parts of ultra-high molecular weight polyethylene powder to the mixed system, heat to 95-105℃, and simultaneously turn on ultrasonic and mechanical stirring at 100-200 rpm for 1.5-2.5 hours to obtain a swollen slurry. The swollen slurry is pumped into a co-rotating twin-screw extruder with a length-to-diameter ratio of 52:1. The feeding section temperature is set at 120-130℃, the reaction melting section temperature at 185-195℃, the homogenization section temperature at 210-220℃, and the screw speed at 180-220 rpm to achieve a melting reaction and obtain a molten stock solution. The molten stock solution is extruded through a spinneret with a length-to-diameter ratio of 15:1, and after passing through a 15-20 mm air layer, it is quenched in an 8-12℃ water bath to obtain gel fibers. Subsequently, it is processed with n-hexane at 35-40℃. Multi-stage extraction is performed, with each extraction lasting 10-20 minutes. After 3-5 extractions, a micro-tension of 1.0-1.2 cN / dtex is applied to obtain treated fibers. The treated fibers are then subjected to three-stage hot stretching in an oven. The first-stage oven stretching temperature is 115-120℃ with a stretching ratio of 5-7 times; the second-stage oven stretching temperature is 135-145℃ with a stretching ratio of 4-6 times; and the third-stage oven stretching temperature is 148-152℃ with a stretching ratio of 1.5-2.0 times, to obtain the polyethylene fibers.

[0008] During melt extrusion, the extruder is designed to withstand a pressure of no less than 25.0 MPa. The feed port uses a forced water-cooled mechanical seal and is protected by a slightly positive pressure nitrogen gas to prevent solvent vapor backflow and oxygen ingress. The extrusion process adopts a fully enclosed, non-devouring design, maintaining the melt pressure inside the extruder at 3.5-8.0 MPa to ensure that decahydronaphthalene is in a pressurized liquid phase. The pressure difference of the screen filter is strictly controlled within 1.5 MPa to monitor the dispersion of amination carbon nanotubes and prevent filter clogging. The screw speed is adjusted to stabilize the actual torque between 55% and 75%, and the average residence time of the material in the extruder is controlled at 4-7 minutes. This ensures sufficient interfacial reaction and uniform mixing between modified polyethylene and amination carbon nanotubes, while avoiding uncontrollable and severe thermal decomposition of the anti-aging agent due to prolonged high-temperature shearing. The extrusion system is equipped with an overpressure interlock protection device. When the melt pressure at the die head or the internal pressure of the barrel exceeds 15.0 MPa, the shutdown interlock will be automatically triggered, and the explosion-proof pressure relief valve will be activated for safe release.

[0009] This invention utilizes ultrasonic swelling, leveraging the cavitation microjets generated by ultrasound in a liquid to break the van der Waals force aggregation of carbon nanotubes. During the stepwise addition process, a low-viscosity solvent is used to first disperse the nanoparticles, followed by steric hindrance coating through the dissolution of modified polyethylene. Finally, the system is allowed to penetrate the interior of the polymer powder, ensuring the macroscopic and microscopic uniformity of the multi-component hybrid system. Overcoming a significant energy barrier is required to disentangle and transform the crystal structure of polyethylene macromolecules. Using a single high-temperature thermal stretching method would lead to stress concentration and fiber breakage. In the three-stage thermal stretching process, a gradient stretching from low to high temperatures allows the amorphous regions to be straightened first when the molecular chains have a certain degree of mobility. Then, at temperatures close to the melting point, the template effect of carbon nanotubes induces the molecular chains to align regularly along the axial direction, ultimately forming a highly crystalline, highly oriented tandem crystal structure.

[0010] Preferably, the preparation of the anti-aging adjuvant includes the following steps: Add 150 parts acetone and 50 parts deionized water to a reaction vessel, turn on mechanical stirring, and maintain the stirring speed at 200-400 rpm. Cool to 0-5℃, add 18.4 parts cyanuric chloride, and stir to dissolve for 10-20 minutes to obtain a mixed system. Slowly add 15.6 parts 2,2,6,6-tetramethyl-4-piperidinamine to the mixed system over 30-50 minutes, while simultaneously adding a 10% sodium carbonate aqueous solution, maintaining the pH of the system at 7-8. Keep the system at 0-5℃ and collect the solution. The substitution reaction is carried out for 1.5-2.5 hours to obtain the substituted product; then, 15.6 parts of sodium azide are added to the substituted product, the system is slowly heated to 70-80℃, and the reaction is carried out under reflux for 6-8 hours to obtain the reaction system; after the reaction is completed, the reaction system is poured into 300-500 parts of ice water, filtered to obtain a white solid, washed 3-5 times with deionized water until neutral, and dried in a vacuum drying oven at 35-45℃ and a vacuum degree of 0.08-0.1MPa for 10-14 hours to obtain the anti-aging additive.

[0011] Preferably, the preparation of the modified polyethylene includes the following steps: 100 parts of high-density polyethylene, 1.2-2.0 parts of maleic anhydride, and 0.03-0.08 parts of dicumyl peroxide are added to a high-speed mixer and mixed at 500-800 rpm for 5-10 minutes to obtain a premix. The premix is ​​then added to a twin-screw extruder and reacted and granulated at 180-200°C with a screw speed of 150-250 rpm. The modified polyethylene is obtained by melt extrusion, wherein the grafting rate of maleic anhydride is 1.0%-1.5%.

[0012] The choice of ultra-high molecular weight polyethylene (UHMWPE) as the matrix in this invention is fundamental to providing the fiber with good mechanical strength. Its long macromolecular chains can form a continuous network across multiple crystalline regions. The introduction of aminated carbon nanotubes not only serves as a rigid mechanical reinforcement but also as a one-dimensional nucleating agent, inducing the polyethylene molecular chains to crystallize on its surface during stretching. However, polar carbon nanotubes have poor compatibility with non-polar polyethylene. By introducing a modified polyethylene carrier, the interfacial reaction and polar interaction between MAH-grafted polyethylene and aminated carbon nanotubes are utilized to improve dispersion. At the same time, the sufficiently long carbon chains physically entangle with the UHMWPE matrix, eliminating the risk of interfacial phase separation. The selection of reactive anti-aging agents in this invention is to solve the problem of loss of traditional small molecule auxiliaries during extraction and washing. Through covalent anchoring, the fiber is not only endowed with long-term anti-aging properties, but the rigid triazine ring in its structure can also act as an intramolecular anchor point, restricting the creep of molecular chains in amorphous regions, thereby improving the fiber's creep resistance.

[0013] The present invention also provides a polyethylene fiber with high crystallinity orientation, the raw materials for which include aminated multi-walled carbon nanotubes, anti-aging additives, modified polyethylene, ultra-high molecular weight polyethylene, decahydronaphthalene and white oil.

[0014] Compared with the prior art, the beneficial effects of the present invention are as follows: 1. In existing technologies, conventional polyethylene fiber gel spinning relies solely on physical blending and single high-temperature stretching, which makes it difficult to untangle the ultra-long molecular chains, resulting in a bottleneck in crystallinity and stress concentration during stretching, leading to fiber breakage. This invention uses aminated carbon nanotubes in conjunction with functionalized modified carriers and a multi-level gradient thermal stretching process. By utilizing the nucleation effect of one-dimensional rigid nanomaterials under a gradient temperature field, it induces regular epitaxial crystallization of polyethylene macromolecular chains along the stretching axis, forming a dense beaded crystal network. This eliminates the risk of tensile fracture and endows single-component polyethylene fibers with good tensile strength and initial modulus, meeting the load-bearing requirements under ultimate load conditions.

[0015] 2. Existing anti-aging modifications of synthetic fibers mostly employ the physical addition of conventional auxiliaries such as hindered phenols. During the gel extraction process and subsequent outdoor exposure to sunlight and rain, small molecules easily migrate to the surface and are washed away by solvents, leading to a rapid decline in weather resistance. This invention introduces triazine hindered amines as reactive reagents. Through reactive extrusion, highly active groups generated by thermal decomposition are inserted into the carbon-hydrogen bonds of the inert polyethylene backbone to achieve covalent bonding. This allows the anti-aging components to be grafted into the fiber backbone, avoiding the loss defects caused by multi-stage solvent extraction. Without damaging the polymer backbone structure, this invention endows the cross-linked network and fiber with long-lasting resistance to ultraviolet radiation and heat-oxidative aging, achieving durable and long-lasting protection.

[0016] 3. Traditional ultra-high molecular weight polyethylene fibers suffer from severe long-term creep degradation due to the unavoidable slippage of macromolecular chains in their amorphous regions. This invention utilizes the physical entanglement of long polymer chains with a polar carrier and the matrix, while its active groups achieve chemical bridging with nano-reinforcement. In addition, reactive additives provide rigid triazine rings as intramolecular physical nodes. Through a multi-dimensional spatial locking mechanism, the free amorphous chain segments are effectively bound, limiting the creep and structural deformation of polymer chains under continuous tension, significantly enhancing the long-term creep resistance and overall dimensional stability of polyethylene fibers.

[0017] 4. A long-standing pain point in the composite weaving industry is that the surface of conventional polyethylene fibers exhibits extreme chemical inertness and low surface energy, resulting in poor wettability between the fibers and resin coatings. Under shear stress, interfacial delamination is likely to occur. This invention uses functionalized polymer grafts as a medium and employs a stepwise ultrasonic cavitation dispersion process to uniformly enrich polar groups and nanoparticles on the fiber surface. This not only improves the micro-roughness and free energy of the fiber surface but also builds strong chemical bonds between the fiber body and the subsequent resin coating, enhancing the interfacial peel strength and ensuring the structural integrity of the special fabric. Attached Figure Description

[0018] Figure 1 Fourier transform infrared spectra of the anti-aging auxiliary intermediate prepared in Example 1 of the present invention and the polyethylene fiber prepared in Example 1 and subjected to multi-stage n-hexane extraction. Figure 2 These are comparison images of one-dimensional wide-angle X-ray diffraction of polyethylene fibers prepared in Example 1, Comparative Example 3, and Comparative Example 7 of the present invention. Figure 3 The changes in the retention rate of anti-aging agent and the retention rate of ultraviolet aging breaking strength of polyethylene fibers obtained in Example 1 and Comparative Examples 4-9 of this invention are shown. Detailed Implementation

[0019] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0020] The ultra-high molecular weight polyethylene used in this invention is in powder form, with a viscosity-average molecular weight of 4,500,000-6,000,000 g / mol, an intrinsic viscosity of 15-30 dL / g, and a density of 0.93-0.94 g / cm³. 3The weight-average molecular weight of high-density polyethylene is 500,000-800,000 g / mol, and the melt flow rate is 0.1-0.5 g / 10 min. The diameter of aminated multi-walled carbon nanotubes is 8-15 nm, the length is 10-30 μm, and the surface amino mass fraction is 0.5%-2.0%.

[0021] Please see Figures 1 to 3 This invention provides a polyethylene fiber with high crystallinity orientation and a method for preparing the same. The technical solution is as follows: Example 1 150 parts of acetone and 50 parts of deionized water were added to a reaction vessel, and mechanical stirring was started at 300 rpm. The mixture was cooled to 0°C, and 18.4 parts of cyanuric chloride were added. The mixture was stirred and dissolved for 20 minutes to obtain a mixed system. 15.6 parts of 2,2,6,6-tetramethyl-4-piperidinamine were slowly added dropwise to the mixed system over 40 minutes, and a 10% sodium carbonate aqueous solution was added dropwise simultaneously to maintain the pH of the system at 7-8. The substitution reaction was carried out at 0°C for 2 hours to obtain the substituted product. Then, 15.6 parts of sodium azide were added to the substituted product, and the system was slowly heated to 70°C and refluxed for 8 hours to obtain the reaction system. After the reaction was completed, the reaction system was poured into 400 parts of ice water, filtered to obtain a white solid, washed 5 times with deionized water until neutral, and dried in a vacuum drying oven at 40°C and a vacuum degree of 0.09 MPa for 12 hours to obtain the anti-aging additive. 100 parts of high-density polyethylene, 1.5 parts of maleic anhydride, and 0.05 parts of dicumyl peroxide were added to a high-speed mixer and mixed for 8 minutes at 600 rpm to obtain a premix. The premix was then added to a twin-screw extruder and reacted and granulated at 180-200°C with a screw speed of 200 rpm. The modified polyethylene was obtained by melt extrusion. 1.2 parts of aminated multi-walled carbon nanotubes, 1.2 parts of anti-aging additives, 0.3 parts of antioxidant 168, and 200 parts of decahydronaphthalene were mixed and ultrasonically assisted at 40°C with a frequency of 30 kHz and a power of 1000 W for 30 minutes to obtain an ultrasonic system. 4 parts of modified polyethylene and 600 parts of white oil were added to the ultrasonic system, and the mixture was heated to 80°C. Mechanical stirring was started at 400 rpm for 30 minutes to obtain a mixed system. 100 parts of ultra-high molecular weight polyethylene powder were added to the mixed system, and the mixture was heated to 100°C. Simultaneously, ultrasonic and mechanical stirring were started at 150 rpm, and the mixture was treated for 2 hours to obtain a swollen slurry. The swollen slurry was pumped into a co-rotating twin-screw extruder with an aspect ratio of 52:1. The feeding section temperature was set at 125°C, the reaction melting section temperature at 190°C, the homogenization section temperature at 215°C, and the screw speed at 200 rpm to achieve a melting reaction and obtain a molten stock solution. The molten stock solution was extruded through a spinneret with an aspect ratio of 15:1, passed through an 18 mm air layer, and then quenched in a 10°C water bath to obtain gel fibers. Subsequently, multi-stage extraction was performed using n-hexane at 40°C, with each extraction lasting 15 minutes. After five extractions, a micro-tension of 1.0 cN / dtex was applied to obtain treated fibers. The treated fibers were then subjected to three-stage hot stretching in an oven. The first stage of the oven stretching temperature was 118°C with a stretching ratio of 6 times; the second stage of the oven stretching temperature was 140°C with a stretching ratio of 5 times; and the third stage of the oven stretching temperature was 150°C with a stretching ratio of 1.8 times to obtain the polyethylene fibers.

[0022] Examples 2-5 follow the same preparation method and parameter conditions as Example 1, with differences shown in Table 1.

[0023] Table 1. Parameter variations in Examples 1-5 Comparative Example 1 is the same as Example 1, except that ultra-high molecular weight polyethylene powder is not used as the matrix, but is replaced with an equal amount of conventional high-density polyethylene powder, while the rest of the process remains unchanged.

[0024] Comparative Example 2 is the same as Example 1, except that aminated multi-walled carbon nanotubes are not added, while the rest of the process remains unchanged.

[0025] Comparative Example 3 is the same as Example 1, except that the three-stage gradient hot stretching process is not used. The gel fiber is directly hot stretched 10 times in an oven at 150°C after treatment, while the rest of the process remains the same.

[0026] Comparative Example 4 is the same as Example 1, except that modified polyethylene is not used, but an equal amount of maleic anhydride grafted onto commercially available low-density polyethylene substrate is used as a carrier additive, while the rest of the process remains unchanged.

[0027] Comparative Example 5 is the same as Example 1, except that it does not use amino-containing multi-walled carbon nanotubes, but instead uses an equal mass of ordinary unmodified multi-walled carbon nanotubes, while the rest of the process remains unchanged.

[0028] Comparative Example 6 is the same as Example 1, except that no anti-aging additive is added, and an equal mass of antioxidant 168 is used instead, while the rest of the process remains unchanged.

[0029] Comparative Example 7 is the same as Example 1, except that the stepwise pre-dispersion process is not used. All powders and mixed solvents are put into the reactor at one time for ultrasonic-assisted mechanical stirring and swelling. The rest of the process remains the same.

[0030] Comparative Example 8 is the same as Example 1, except that ultrasonic assistance is not used, and stepwise pre-dispersion is used to swell by conventional mechanical stirring, while the rest of the process remains unchanged.

[0031] Comparative Example 9 is the same as Example 1, except that decahydronaphthalene is not used, and the spinning solvent is replaced with an equal total amount of single white oil solvent, while the rest of the process remains unchanged.

[0032] Combination Figure 1 The Fourier transform infrared spectrum shows that, in the spectral curve of the reactive anti-aging additive intermediate, at 2120 cm⁻¹... -1 A sharp and strong characteristic absorption peak appears at 2120 cm⁻¹, which is attributed to the asymmetric stretching vibration of the nitrogen-nitrogen triple bond in the azide group, confirming that the anti-aging additive successfully carries the azide reactive group; while in the polyethylene fiber spectrum obtained in Example 1, at 2120 cm⁻¹... -1 The characteristic peak of azide disappeared at 2920 cm⁻¹; at the same time, the characteristic peak of azide disappeared at 2920 cm⁻¹. -1 2850cm -1 and 1460cm -1 The strong methylene absorption peak of polyethylene is retained at 1530 cm⁻¹. -1 The presence of characteristic absorption peaks belonging to the triazine ring nearby further confirms that the azide group undergoes thermal decomposition in the reaction melting section of the twin-screw extruder at 185-195℃, releasing highly active singlet nitrogen olefins, which are then introduced into the CH bonds of the ultra-high molecular weight polyethylene backbone to complete the in-situ covalent bonding reaction. This chemical anchoring not only avoids loss caused by the extraction process but also achieves a long-term bond between the anti-aging agent and the polyethylene fiber.

[0033] Combination Figure 2 The X-ray diffraction patterns show that the fibers under the three process conditions all exhibit typical diffraction peaks of the polyethylene orthorhombic crystal system near 2θ of 21.4° and 23.8°, corresponding to the (110) crystal plane and the (200) crystal plane, respectively. Among them, the diffraction peaks of the fiber in Example 1 show higher relative intensity and narrow half-peak width, indicating that its internal grain size is large, lattice defects are few, and crystal orientation is high. In contrast, in Comparative Example 3, due to the direct single-stage strong stretching at 150°C, the untangling of the polyethylene macromolecular chains could not overcome the huge energy barrier, and the forced stretching led to stress concentration and failed to form a regular crystal arrangement. In Comparative Example 7, the stepwise pre-dispersion process was not used, resulting in poor uniformity of the nanoparticles at both the macroscopic and microscopic levels. The agglomeration of carbon nanotubes hindered their role in inducing the axial epitaxial crystallization of polyethylene molecular chains, which limited the growth of the (110) crystal plane, and the diffraction peak intensity was significantly weaker than that of Example 1.

[0034] Experimental Example 1: Mechanical Property Testing The polyethylene fibers prepared in Examples 1-5 and Comparative Examples 1-5 were subjected to mechanical property tests. Crystallinity was tested using wide-angle X-ray diffraction. The sound velocity orientation factor was measured using a sound velocity orientation meter and calculated by measuring the propagation speed of sound waves along the fiber axis. The breaking strength and initial modulus were tested using an electronic single yarn tensile tester, in accordance with GB / T14344-2022. The constant load creep rate test was conducted according to DB32 / T 5091-2025. Under standard room temperature of 25°C, a constant tensile stress equivalent to 20% of the rated breaking load was applied to the polyethylene fiber, and the irreversible elongation was recorded after 500 hours of continuous stress. The results are expressed as a percentage, and the residual creep strain after 500 hours of constant load is expressed as the constant load creep rate. The test results are shown in Table 2.

[0035] Table 2 Test results of the examples and comparative examples As shown in Table 2, the polyethylene fibers obtained in the comparative examples, through adjustments to the components and processes, exhibited significant differences in crystal orientation, mechanical properties, and creep resistance compared to the examples. In Comparative Example 1, the short macromolecular chains of conventional high-density polyethylene prevented the formation of a continuous network across multiple crystal regions during stretching, hindering the effective transfer of high tensile stress to the matrix and resulting in a significant reduction in fracture strength and initial modulus. In Comparative Example 2, the absence of aminated multi-walled carbon nanotubes meant the system lacked a rigid mechanical reinforcement and nucleating agent, preventing the induction of polyethylene molecular chains to crystallize on its surface during stretching. This led to a significant decrease in crystallinity and acoustic orientation factor, resulting in poorer mechanical properties. In Comparative Example 3, direct high-temperature stretching at 150°C failed to overcome the significant challenges of disentanglement and crystal transformation of the polyethylene macromolecular chains. The energy barrier of the high-temperature single-stage model directly leads to high stress concentration in the amorphous region, causing microcracks and wire breakage. It is impossible to form a crystal structure with high crystallinity and high orientation, resulting in a significant reduction in mechanical properties. In Comparative Example 4, modified polyethylene was not used and was replaced with commercially available low-density polyethylene substrate maleic anhydride grafts. Because the low-density substrate lacks sufficiently long carbon chains to physically entangle with the ultra-high molecular weight polyethylene matrix, there is a risk of phase separation at the interface between the inorganic and organic phases. Under external force, the interface is prone to slippage and debonding, resulting in increased creep rate and decreased mechanical strength. In Comparative Example 5, unmodified multi-walled carbon nanotubes were used instead. Because their surface lacks amino groups, they cannot form chemical bonds with the polar anhydride groups of the modified polyethylene carrier. They agglomerate and separate in the matrix, and cannot achieve steric hindrance coating, becoming stress concentration defects during tension, resulting in a significant reduction in mechanical properties.

[0036] Experiment Example 2: Anti-aging Performance Test The polyethylene fibers prepared in Examples 1-5 and Comparative Examples 4-9 were subjected to anti-aging performance tests. 5.0 g of polyethylene fiber samples, after multi-stage hexane extraction and thorough drying, were placed in a Soxhlet extractor and extracted with chloroform at 65°C for 24 h under reflux. The extract was concentrated by rotary evaporation and brought to a final volume, then injected into a high-performance liquid chromatograph (HPLC). The chromatographic conditions were set as follows: C18 reversed-phase column (250 mm × 4.6 mm), mobile phase: methanol / water (90 / 10 v / v), flow rate: 1.0 mL / min, UV detector wavelength: 225 nm. The retention was calculated using the external standard method based on peak area, thus determining the retention rate of the anti-aging agent after extraction. According to GB / T 31899-2015, polyethylene fibers were tightly wound onto a stainless steel sample holder and placed in an accelerated UV aging test chamber. A UVA-340 lamp was used to simulate outdoor light spectrum. The single cycle parameters were set as follows: UV irradiation for 8 h (irradiance 0.89). W / (m²·nm), blackboard temperature 60℃), condensation in darkness for 4 hours (blackboard temperature 50℃), continuous alternating cycle for 1000 hours; after aging, humidify for 24 hours, according to GB / T 14344-2022 The tensile strength was tested using an electronic single-yarn tensile tester (tensile speed 250 mm / min, spacing 250 mm, pretension 0.05 cN / dtex), and the UV aging retention rate was tested. A high-precision dynamic contact angle meter was used, with deionized water (known polar component) and diiodomethane (known dispersion component) selected as the test probe liquids. The dynamic contact angle was calculated by precisely recording the force changes of a single polyethylene fiber when immersed in and pulled out of the liquid using a microbalance, and then substituted into the OWRK equation to calculate the total polar surface energy of the fiber. Polyethylene fibers were densely woven into 25 mm wide standard test strips, and a 50 μm thick layer of polyurethane resin was uniformly coated on the surface using a bar coater. After being bonded to a polyester film backing, the strips were cured at 80°C for 2 hours and left at room temperature for 24 hours. A 180° continuous peel test was then performed using a universal testing machine at a speed of 300 mm / min, and the average peel strength during the stable peeling stage was recorded. The changes in the anti-aging agent retention rate and UV aging tensile strength retention rate of the polyethylene fibers obtained in Examples 1 and Comparative Examples 4-9 are as follows: Figure 3 As shown in the figure; the specific test results are shown in Table 3.

[0037] Table 3. Test results of the examples and comparative examples As shown in Table 3, the polyethylene fibers obtained in the comparative examples, through adjustments to the components and processes, exhibited significantly different anti-aging and interfacial properties compared to the examples. In Comparative Example 4, due to the short molecular chains of the low-density polyethylene carrier, the anhydride groups it carried could not be firmly anchored in the ultra-high molecular weight polyethylene network. During coating processing, the surface molecular chains were prone to slippage and detachment, leading to a decrease in fiber surface energy and a significant reduction in coating interfacial peel strength. In Comparative Example 5, the aggregated inorganic particles formed micropores and physical defects on the fiber surface, becoming channels for oxygen and moisture to penetrate into the fiber interior, accelerating local photo-oxidative aging reactions. Simultaneously, the uneven distribution of surface polarity resulted in a decrease in surface energy and coating adhesion. In Comparative Example 6, without the addition of reactive anti-aging additives, the covalent anchoring effect between the rigid triazine ring and the polyethylene main chain was lacking. In the multi-stage n-hexane extraction process, most of the conventional small-molecule antioxidants were eluted, resulting in a significant decrease in the retention rate of anti-aging agents after extraction, thus losing the long-term chemical protection effect and failing to meet the requirements for long-term outdoor use. In Comparative Example 7, the stepwise pre-dispersion process was not used. The unevenness caused by local enrichment of powder resulted in the scattered distribution of anti-aging additives within the matrix, failing to form a continuous anti-UV protection network. This led to protective blind spots within the fiber, which were prone to photo-oxidative degradation and crack propagation under long-term UV irradiation, resulting in a significant reduction in overall fracture strength after aging. In Comparative Example 8, conventional stirring alone could not break the nanotube agglomeration. The agglomerates formed under UV irradiation would absorb light, converting the absorbed light energy into extremely high local heat, accelerating the thermo-oxidative degradation of the surrounding polyethylene matrix, and causing a decrease in mechanical retention rate after UV aging. In Comparative Example 9, the use of only high-viscosity white oil resulted in a high residual oil rate, which easily formed an inert weak boundary layer on the fiber surface, shielding the polar groups on the fiber surface from the chemical interaction with the polyurethane coating, resulting in a significant reduction in the coating interface peel strength. In addition, the residual white oil itself was prone to photothermal oxidation, and the free radicals generated would prematurely consume the hindered amine anti-aging additives in the system, further shortening the overall anti-aging life of the fiber.

[0038] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.

Claims

1. A method for preparing polyethylene fibers with high crystallinity orientation, characterized in that, Includes the following steps: A swellable slurry is prepared by stepwise premixing and ultrasonic-assisted stirring of 0.5-2.0 parts of aminated multi-walled carbon nanotubes, 0.8-1.5 parts of anti-aging additives, 3-6 parts of modified polyethylene, 100 parts of polyethylene powder, and 650-1050 parts of mixed solvent. This slurry is then added to a twin-screw extruder for melt reaction, extruded through a spinneret, and quenched in a water bath to obtain gel fibers. Subsequently, multi-stage extraction is performed, followed by three-stage hot stretching in an oven to obtain the polyethylene fibers. The anti-aging additives are obtained by reacting cyanuric chloride, 2,2,6,6-tetramethyl-4-piperidinamine, and sodium azide in deionized water and acetone. The modified polyethylene is obtained by melt grafting high-density polyethylene and maleic anhydride.

2. The method for preparing high-crystallinity polyethylene fiber according to claim 1, characterized in that, The polyethylene powder is made of ultra-high molecular weight polyethylene with a viscosity-average molecular weight of 4,500,000-6,000,000 g / mol; the mixed solvent is obtained by mixing 150-300 parts of decahydronaphthalene and 500-750 parts of white oil; the high-density polyethylene has a weight-average molecular weight of 500,000-800,000 g / mol.

3. The method for preparing high-crystallinity polyethylene fiber according to claim 1, characterized in that, The preparation of the swelling slurry includes the following steps: mixing the aminated multi-walled carbon nanotubes, the anti-aging additive, antioxidant 168 and decahydronaphthalene, and ultrasonically treating them to obtain an ultrasonic system; then adding the modified polyethylene and the white oil and stirring to obtain a mixed system; subsequently adding ultra-high molecular weight polyethylene powder, and simultaneously turning on ultrasonic and mechanical stirring to mix and obtain the swelling slurry.

4. The method for preparing high-crystallinity polyethylene fiber according to claim 1, characterized in that, The preparation of the polyethylene fiber includes the following steps: The swollen slurry is pumped into a co-rotating twin-screw extruder with a length-to-diameter ratio of 52:1, where it undergoes a melting reaction to obtain a molten stock solution. This solution is then extruded through a spinneret, passes through an air layer, and is subsequently quenched in a water bath. Following this, it undergoes multi-stage extraction with n-hexane. Finally, it is subjected to three stages of hot stretching in an oven. The first stage of the oven stretching temperature is 115-120℃ with a stretching ratio of 5-7 times; the second stage stretching temperature is 135-145℃ with a stretching ratio of 4-6 times; and the third stage stretching temperature is 148-152℃ with a stretching ratio of 1.5-2.0 times to obtain the polyethylene fiber.

5. The method for preparing polyethylene fibers with high crystallinity orientation according to claim 3, characterized in that, The preparation of the anti-aging additive includes the following steps: Acetone and deionized water were added to a reaction vessel, and mechanical stirring was started. Cyanide was added and stirred until dissolved to obtain a mixed system. 2,2,6,6-Tetramethyl-4-piperidinamine was added dropwise to the mixed system, and sodium carbonate aqueous solution was added dropwise simultaneously to obtain a substituted product through a substitution reaction. Sodium azide was then added to the substituted product, and the reaction was refluxed to obtain a reaction system. The system was then filtered in ice water, washed with deionized water, and dried in a vacuum oven to obtain the anti-aging additive.

6. The method for preparing high-crystallinity polyethylene fiber according to claim 3, characterized in that, The preparation of the modified polyethylene includes the following steps: High-density polyethylene, 1.2-2.0 parts of maleic anhydride, and dicumyl peroxide are added to a high-speed mixer and mixed evenly. The mixture is then added to a twin-screw extruder for melt extrusion to obtain the modified polyethylene, wherein the grafting rate of maleic anhydride is 1.0%-1.5%.

7. A polyethylene fiber with high crystallinity orientation, characterized in that, The raw materials include aminated multi-walled carbon nanotubes, anti-aging additives, modified polyethylene, ultra-high molecular weight polyethylene, decahydronaphthalene, and white oil; the polyethylene fiber is prepared by any one of the preparation methods of claims 1-6.