A method for preparing a cooling and wind-resistant fiber
By using hexagonal boron nitride powder and jade powder to form a thermally conductive network in the cooling fiber and optimizing the matrix crystallization, the problem of discontinuous thermally conductive network was solved, achieving rapid heat conduction and long-lasting cooling effects, while also improving the mechanical properties of the fiber.
Patent Information
- Application Number
- CN202611512693.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-28
- Publication Date
- 2026-11-17
AI Technical Summary
Existing cooling and wind-absorbing fibers suffer from uneven dispersion of thermal conductive fillers and weak interfacial bonding, resulting in a discontinuous thermal conductive network that cannot quickly conduct heat away from the skin surface, thus reducing the user experience.
Hexagonal boron nitride powder is used as the core thermal conductive framework, combined with jade powder to form a multi-scale thermal conductive pathway, and the matrix crystallization behavior is optimized by pre-treating polyethylene terephthalate slices to form a stable thermal conductive network.
It achieves rapid heat conduction and a long-lasting cooling experience with cooling fibers, while also possessing good mechanical properties, thus solving the problem of low thermal conductivity.
Smart Images

Figure CN123108765A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of fiber materials technology, specifically to a method for preparing a cooling and wind-resistant fiber. Background Technology
[0002] Cooling and wind-resistant fiber is a differentiated fiber with excellent thermal conductivity and heat dissipation properties. By giving the fiber a high thermal diffusivity, it can quickly conduct away heat from the body surface when in contact with the skin, producing a cooling sensation. At the same time, it takes into account the necessary mechanical and processing properties of the fiber, thereby meeting people's ever-increasing demands for quality of life.
[0003] Existing cooling and wind-feeling fibers, which use a large amount of thermally conductive fillers to achieve high thermal conductivity, often fail to form a continuous and efficient thermally conductive network in the polymer matrix due to uneven dispersion and weak interfacial bonding. Consequently, the fibers cannot quickly conduct heat away from the skin surface after application, reducing the user experience. Therefore, this invention provides a method for preparing cooling and wind-feeling fibers. Summary of the Invention
[0004] The purpose of this invention is to provide a method for preparing cooling and wind-resistant fibers. The cooling and wind-resistant fibers prepared by this invention not only have good thermal conductivity and cooling sensation, but also good mechanical properties.
[0005] To achieve the above objectives, the present invention provides the following technical solution: 1. A method for preparing a cooling and wind-resistant fiber, comprising the following steps: S1: Raw material preparation, the raw materials include the following weight components: 105-110 parts base material, 3-4 parts filler, 2-3 parts polyethylene glycol, 2-3 parts sorbitan fatty acid ester, 0.6-1 part dispersant, 0.5-0.8 parts lubricant and 0.2-0.5 parts antioxidant; The raw materials for the filler include hexagonal boron nitride powder and jade powder; S2: Fiber preparation, the raw materials are mixed and processed to obtain cool and wind-resistant fibers.
[0006] Preferably, the filler is prepared by the following method: hexagonal boron nitride powder and NMP are added to a mixer for processing to obtain a mixture. The resulting product is centrifuged, and the obtained solids are washed with deionized water and then mixed with deionized water to obtain a dispersion for later use. KH570, anhydrous ethanol and deionized water are added to a mixer and stirred to obtain coarse material. The dispersion, coarse material and jade powder are mixed and centrifuged. The resulting precipitate is sent to an oven for drying to obtain the filler.
[0007] Preferably, the mass ratio of hexagonal boron nitride powder to NMP is 1:30-40, the mass ratio of KH570, anhydrous ethanol and deionized water is 3-5:30-40:4-6, and the mass ratio of dispersion, coarse material and jade powder is 100:30-40:15-20.
[0008] Preferably, the pretreated polyethylene terephthalate (PET) chips are prepared by the following method: PET chips and polybutylene terephthalate (PET) chips are fed into a mixer and stirred at 80–90°C. The temperature is then lowered to 75–80°C and stirred for 30–40 minutes. During the stirring process, aluminophosphate, lignite wax, and carbodiimide are added sequentially. The resulting product is fed into a screw extruder, with the following temperatures set: Zone 1 temperature 235°C, Zone 2 temperature 255°C, Zone 3 temperature 270°C, Zone 4 temperature 280°C, and die head temperature 270°C. After melt blending, the product is granulated and dried to obtain the pretreated PET chips.
[0009] Preferably, the mass ratio of polyethylene terephthalate chips to polybutylene terephthalate chips is 100:7-8, the mass of aluminophosphate is 0.8-1% of the mass of polyethylene terephthalate chips, and the mass ratio of aluminophosphate, lignite wax and carbodiimide is 1:0.2-0.3:1.
[0010] Preferably, the polyethylene glycol is PEG10000.
[0011] Preferably, the fiber preparation method is as follows: polyethylene terephthalate chips, pretreated polyethylene terephthalate chips, fillers, polyethylene glycol, sorbitan fatty acid esters, dispersants, lubricants, and antioxidants are weighed as needed and added to a mixer for stirring. The resulting product is fed into a screw extruder, where the temperatures are set to 260°C in zone one, 275°C in zone two, 280°C in zone three, 284°C in zone four, and 284°C in the spinning box. The resulting melt is extruded, cooled, oiled, and wound to obtain polyester POY fibers. The polyester POY fibers are then heated, false-twisted, heat-set, and wound to form cool-feeling and wind-resistant fibers.
[0012] Preferably, the extrusion temperature is 260-285℃, the cooling is achieved by side blowing at a temperature of 25℃, the oiling is TK-3182A with an oiling rate of 0.45%, the winding speed is 2800-3000m / min, the texturing heating box temperature is 180-200℃, the false twist rate is 550-700m / min, the false twist ratio is 1.7-1.9, and the heat setting temperature is 180-190℃.
[0013] Preferably, the dispersant is BYK163.
[0014] Preferably, the lubricant is pentaerythritol stearate, and the antioxidant is PEP36.
[0015] Compared with the prior art, the beneficial effects of the present invention are: 1. In this invention, the filler uses hexagonal boron nitride powder as the core thermally conductive framework, which has a high thermal conductivity. Combined with jade powder as an auxiliary heat conduction point, it forms a stable thermally conductive pathway with multi-scale bonding in the matrix. The introduction of polybutylene terephthalate into the pretreated polyethylene terephthalate chips further optimizes the matrix crystallization behavior and reduces crystallization defects caused by the introduction of filler, thereby significantly reducing the interfacial thermal resistance. This allows heat to be quickly and directionally conducted along the filler network, effectively solving the problem of low heat dissipation efficiency caused by imperfect thermal conductive pathways. This enables the fiber to quickly conduct heat away from the body when in contact with the skin and provides a lasting cooling experience. Attached Figure Description
[0016] Figure 1 The flowchart illustrates a method for preparing cooling and wind-resistant fibers according to the present invention. Detailed Implementation
[0017] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0018] It should be noted that the raw materials used in the following embodiments are all commercially available. Example 1:
[0019] S1: Raw material preparation, the raw materials include the following weight components: 105 parts base material, 3 parts filler, 2 parts polyethylene glycol, 2 parts sorbitan fatty acid ester, 0.6 parts dispersant, 0.5 parts lubricant and 0.2 parts antioxidant; The polyethylene glycol used is PEG10000, the dispersant is BYK163, the lubricant is pentaerythritol stearate, and the antioxidant is PEP36. The raw materials for the filler include hexagonal boron nitride powder and jade powder; S2: Fiber preparation, the raw materials are mixed and processed to obtain cool and wind-resistant fibers.
[0020] The filler was prepared by the following method: hexagonal boron nitride powder and NMP were added to a mixer and processed to obtain a mixture. The product was centrifuged, and the solids were washed with deionized water and then mixed with deionized water to obtain a dispersion. KH570, anhydrous ethanol and deionized water were added to a mixer and stirred to obtain coarse material. The dispersion, coarse material and jade powder were mixed and centrifuged. The precipitate was sent to an oven for drying to obtain the filler.
[0021] The mass ratio of hexagonal boron nitride powder to NMP is 1:30, the mass ratio of KH570, anhydrous ethanol and deionized water is 3:30:4, and the mass ratio of dispersion, coarse material and jade powder is 100:30:15.
[0022] Pretreated polyethylene terephthalate (PET) chips were prepared by the following method: PET chips and polybutylene terephthalate (PET) chips were fed into a mixer and stirred at 80°C. The temperature was then lowered to 75°C and stirred for 30 minutes. During the stirring process, aluminophosphate, lignite wax, and carbodiimide were added sequentially. The resulting product was fed into a screw extruder, with the following temperatures set: Zone 1 temperature 255°C, Zone 2 temperature 265°C, Zone 3 temperature 280°C, Zone 4 temperature 285°C, and the spinning box temperature 280°C. After melt blending, the product was granulated and dried to obtain pretreated PET chips.
[0023] The mass ratio of polyethylene terephthalate chips to polybutylene terephthalate chips is 100:7, the mass of aluminophosphate is 0.8% of the mass of polyethylene terephthalate chips, and the mass ratio of aluminophosphate, lignite wax and carbodiimide is 1:0.2:1.
[0024] The fiber preparation method is as follows: Polyethylene terephthalate chips, pretreated polyethylene terephthalate chips, fillers, polyethylene glycol, sorbitan fatty acid esters, dispersants, lubricants, and antioxidants are weighed as needed and added to a mixer for stirring. The resulting product is fed into a screw extruder, where the temperatures are set to 268℃ in zone one, 278℃ in zone two, 285℃ in zone three, 286℃ in zone four, and 288℃ in the spinning box. The resulting melt is extruded, cooled, oiled, and wound to obtain polyester POY fibers. The polyester POY fibers are then heated, false-twisted, heat-set, and wound to form cool-feeling and wind-resistant fibers.
[0025] The extrusion temperature is 280℃, the cooling method is side blowing, the temperature is 25℃, the oiling method is TK-3182A, the oiling rate is 0.45%, the winding speed is 2800m / min, the texturing heating box temperature is 180℃, the false twist rate is 550m / min, the false twist ratio is 1.7, and the heat setting temperature is 180℃. Example 2:
[0026] S1: Raw material preparation, the raw materials include the following weight components: 107 parts base material, 3.5 parts filler, 2.5 parts polyethylene glycol, 2.5 parts sorbitan fatty acid ester, 0.8 parts dispersant, 0.6 parts lubricant and 0.4 parts antioxidant; The polyethylene glycol used is PEG10000, the dispersant is BYK163, the lubricant is pentaerythritol stearate, and the antioxidant is PEP36. The raw materials for the filler include hexagonal boron nitride powder and jade powder; S2: Fiber preparation, the raw materials are mixed and processed to obtain cool and wind-resistant fibers.
[0027] The filler was prepared by the following method: hexagonal boron nitride powder and NMP were added to a mixer and processed to obtain a mixture. The product was centrifuged, and the solids were washed with deionized water and then mixed with deionized water to obtain a dispersion. KH570, anhydrous ethanol and deionized water were added to a mixer and stirred to obtain coarse material. The dispersion, coarse material and jade powder were mixed and centrifuged. The precipitate was sent to an oven for drying to obtain the filler.
[0028] The mass ratio of hexagonal boron nitride powder to NMP is 1:35, the mass ratio of KH570, anhydrous ethanol and deionized water is 4:35:5, and the mass ratio of dispersion, coarse material and jade powder is 100:35:17.
[0029] Pretreated polyethylene terephthalate (PET) chips were prepared by the following method: PET chips and polybutylene terephthalate (PET) chips were fed into a mixer and stirred at 85°C. The temperature was then lowered to 77°C and stirred for 35 minutes. During the stirring process, aluminophosphate, lignite wax, and carbodiimide were added sequentially. The resulting product was fed into a screw extruder, with the following temperatures set: Zone 1 temperature 255°C, Zone 2 temperature 265°C, Zone 3 temperature 280°C, Zone 4 temperature 285°C, and the spinning box temperature 280°C. After melt blending, the product was granulated and dried to obtain pretreated PET chips.
[0030] The mass ratio of polyethylene terephthalate chips to polybutylene terephthalate chips was 100:7.5, the mass of aluminophosphate was 0.9% of the mass of polyethylene terephthalate chips, and the mass ratio of aluminophosphate, lignite wax and carbodiimide was 1:0.25:1.
[0031] The fiber preparation method is as follows: Polyethylene terephthalate chips, pretreated polyethylene terephthalate chips, fillers, polyethylene glycol, sorbitan fatty acid esters, dispersants, lubricants, and antioxidants are weighed as needed and added to a mixer for stirring. The resulting product is fed into a screw extruder, where the temperatures are set to 268℃ in zone one, 278℃ in zone two, 285℃ in zone three, 286℃ in zone four, and 288℃ in the spinning box. The resulting melt is extruded, cooled, oiled, and wound to obtain polyester POY fibers. The polyester POY fibers are then heated, false-twisted, heat-set, and wound to form cool-feeling and wind-resistant fibers.
[0032] The extrusion temperature is 275℃, the cooling method is side blowing, the temperature is 25℃, the oiling method is TK-3182A, the oiling rate is 0.45%, the winding speed is 2900m / min, the texturing heating box temperature is 190℃, the false twist rate is 650m / min, the false twist ratio is 1.8, and the heat setting temperature is 185℃. Example 3:
[0033] S1: Raw material preparation, the raw materials include the following weight components: 110 parts base material, 4 parts filler, 3 parts polyethylene glycol, 3 parts sorbitan fatty acid ester, 1 part dispersant, 0.8 parts lubricant and 0.5 parts antioxidant; The polyethylene glycol used is PEG10000, the dispersant is BYK163, the lubricant is pentaerythritol stearate, and the antioxidant is PEP36. The raw materials for the filler include hexagonal boron nitride powder and jade powder; S2: Fiber preparation, the raw materials are mixed and processed to obtain cool and wind-resistant fibers.
[0034] The filler was prepared by the following method: hexagonal boron nitride powder and NMP were added to a mixer and processed to obtain a mixture. The product was centrifuged, and the solids were washed with deionized water and then mixed with deionized water to obtain a dispersion. KH570, anhydrous ethanol and deionized water were added to a mixer and stirred to obtain coarse material. The dispersion, coarse material and jade powder were mixed and centrifuged. The precipitate was sent to an oven for drying to obtain the filler.
[0035] The mass ratio of hexagonal boron nitride powder to NMP is 1:40, the mass ratio of KH570, anhydrous ethanol and deionized water is 5:40:6, and the mass ratio of dispersion, coarse material and jade powder is 100:40:20.
[0036] Pretreated polyethylene terephthalate (PET) chips were prepared by the following method: PET chips and polybutylene terephthalate (PET) chips were fed into a mixer and stirred at 90°C. The temperature was then lowered to 80°C and stirred for 40 minutes. During the stirring process, aluminophosphate, lignite wax, and carbodiimide were added sequentially. The resulting product was fed into a screw extruder, with the following temperatures set: Zone 1 temperature 255°C, Zone 2 temperature 265°C, Zone 3 temperature 280°C, Zone 4 temperature 285°C, and the spinning box temperature 280°C. After melt blending, the product was granulated and dried to obtain pretreated PET chips.
[0037] The mass ratio of polyethylene terephthalate chips to polybutylene terephthalate chips is 100:8, the mass of aluminophosphate is 1% of the mass of polyethylene terephthalate chips, and the mass ratio of aluminophosphate, lignite wax and carbodiimide is 1:0.3:1.
[0038] The fiber preparation method is as follows: Polyethylene terephthalate chips, pretreated polyethylene terephthalate chips, fillers, polyethylene glycol, sorbitan fatty acid esters, dispersants, lubricants, and antioxidants are weighed as needed and added to a mixer for stirring. The resulting product is fed into a screw extruder, where the temperatures are set to 268℃ in zone one, 278℃ in zone two, 285℃ in zone three, 286℃ in zone four, and 288℃ in the spinning box. The resulting melt is extruded, cooled, oiled, and wound to obtain polyester POY fibers. The polyester POY fibers are then heated, false-twisted, heat-set, and wound to form cool-feeling and wind-resistant fibers.
[0039] The extrusion temperature is 280℃, the cooling method is side blowing, the temperature is 25℃, the oiling method is TK-3182A, the oiling rate is 0.45%, the winding speed is 3000m / min, the texturing heating box temperature is 190℃, the false twist rate is 700m / min, the false twist ratio is 1.9, and the heat setting temperature is 190℃.
[0040] Comparative Example 1: The difference between this comparative example and Example 1 is that this comparative example does not contain filler, and the missing parts by weight of filler are made up by an equal amount of polyethylene terephthalate chips.
[0041] Comparative Example 2 differs from Example 1 in that: this comparative example does not contain pretreated polyethylene terephthalate (PET) chips, and the missing weight of pretreated PET chips is made up by an equal amount of PET chips.
[0042] Performance testing: The cooling and wind-resistant fibers prepared in Examples 1-3 and Comparative Examples 1-3 were subjected to performance testing; Thermal conductivity: The thermal conductivity λ [W / (m·K)] was tested according to GB / T 10297-2015 standard and recorded in Table 1. The higher the value, the stronger the thermal conductivity of the fiber and the greater the cooling potential. Tensile strength: The breaking strength (cN / dtex) was tested according to GB / T 14344-2022 standard and recorded in Table 1. The higher the strength, the stronger the fiber's ability to resist breaking. Contact cooling coefficient: Tested according to GB / T 35263-2017 standard. max The value of / [J / (cm²·s) is recorded in Table 1. The larger the value, the stronger the cooling sensation when the fabric comes into contact with the skin.
[0043] Table 1:
[0044] Analysis and comparison of the data in the table above show that the thermal conductivity, tensile strength, and contact cooling coefficient of the cooling and wind-feeling fibers prepared by the methods of Examples 1-3 are all better than those of Comparative Examples 1-2. The thermal conductivity and cooling experience are due to the hexagonal boron nitride in the filler as the core thermal conductive skeleton, and the jade powder as the auxiliary heat conduction point, forming an efficient and stable three-dimensional thermal conductive network in the matrix. At the same time, the introduction of polybutylene terephthalate in the pretreated polyethylene terephthalate chips optimizes the matrix crystallization, ensuring that heat can be quickly conducted, thereby giving the fiber excellent instantaneous cooling sensation. Its high strength mechanical properties meet the requirements of high-quality fibers. Further analysis revealed that Comparative Example 1, lacking filler, exhibited severely degraded thermal conductivity and cooling properties. This indicates that the absence of filler signifies the complete loss of the crucial thermally conductive network constructed from hexagonal boron nitride, directly reducing the fiber's thermal conductivity and hindering effective heat dissipation, resulting in a significant decrease in the cooling experience. Comparative Example 2, lacking pretreated polyethylene terephthalate (PET) chips, showed a comprehensive and slight decline in all performance data, inferior to Examples 1-3. This is because the absence of pretreated PET chips affects the matrix's crystallization behavior and processing fluidity, easily leading to decreased filler dispersion uniformity and causing more defects within the fiber. Consequently, the efficiency of the thermally conductive network and the overall mechanical integrity are negatively impacted, preventing the overall performance from reaching its optimal state.
[0045] By comparing and analyzing the relevant data in the table, it can be seen that the cooling and wind-resistant fibers prepared by this invention not only have good thermal conductivity and cooling experience, but also good mechanical properties.
[0046] In the description of this specification, references to terms such as "an embodiment," "example," "specific example," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the invention. In this specification, illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.
[0047] The preferred embodiments of the present invention disclosed above are merely illustrative of the invention. These preferred embodiments do not exhaustively describe all details, nor do they limit the invention to the specific implementations described. Clearly, many modifications and variations can be made based on the content of this specification. This specification selects and specifically describes these embodiments to better explain the principles and practical applications of the invention, thereby enabling those skilled in the art to better understand and utilize the invention. The invention is limited only by the claims and their full scope and equivalents.
Claims
1. A process for the preparation of cool and wind fibers, characterized by: Includes the following steps: S1: Raw material preparation, the raw materials include the following weight components: 105-110 parts base material, 3-4 parts filler, 2-3 parts polyethylene glycol, 2-3 parts sorbitan fatty acid ester, 0.6-1 parts dispersant, 0.5-0.8 parts lubricant and 0.2-0.5 parts antioxidant; The raw materials for the filler include hexagonal boron nitride powder and jade powder; S2: Fiber preparation, the raw materials are mixed and processed to obtain cool and wind-resistant fibers.
2. The method of claim 1, wherein the cooling and wind fibers are prepared by the steps of: The filler is prepared by the following method: hexagonal boron nitride powder and NMP are added to a mixer and processed to obtain a mixture. The product is centrifuged, and the solids are washed with deionized water and then mixed with deionized water to obtain a dispersion for later use. KH570, anhydrous ethanol and deionized water are added to a mixer and stirred to obtain coarse material. The dispersion, coarse material and jade powder are mixed and centrifuged. The precipitate is sent to an oven for drying to obtain the filler. 3. The method of claim 2, wherein the cooling and air fibers are prepared by the steps of: The mass ratio of hexagonal boron nitride powder to NMP is 1:30-40, the mass ratio of KH570, anhydrous ethanol and deionized water is 3-5:30-40:4-6, and the mass ratio of dispersion, coarse material and jade powder is 100:30-40:15-20. 4. The method of claim 1, wherein the cooling and air fibers are prepared by the steps of: The pretreated polyethylene terephthalate (PET) chips are prepared by the following method: PET chips and polybutylene terephthalate (PET) chips are fed into a mixer and stirred at 80–90°C. The temperature is then lowered to 75–80°C and stirred for 30–40 minutes. During the stirring process, aluminophosphate, lignite wax, and carbodiimide are added sequentially. The resulting product is fed into a screw extruder, where the temperatures are set to 265°C in zone one, 278°C in zone two, 280°C in zone three, 285°C in zone four, and 286°C in the spinning box. After melt blending, the product is granulated and dried to obtain the pretreated PET chips. 5. The method of claim 4, wherein the cooling and air fibers are prepared by the steps of: The mass ratio of polyethylene terephthalate chips to polybutylene terephthalate chips is 100:7-8, the mass of aluminophosphate is 0.8-1% of the mass of polyethylene terephthalate chips, and the mass ratio of aluminophosphate, lignite wax and carbodiimide is 1:0.2-0.3:
1. 6. The method of claim 1, wherein the cooling and air fibers are prepared by the steps of: The polyethylene glycol used is PEG10000. 7. The method for preparing cooling and wind-resistant fibers according to claim 1, characterized in that, The fiber preparation method is as follows: Polyethylene terephthalate chips, pretreated polyethylene terephthalate chips, fillers, polyethylene glycol, sorbitan fatty acid esters, dispersants, lubricants, and antioxidants are weighed as needed and added to a mixer for stirring. The resulting product is fed into a screw extruder, where the temperatures are set to 268°C in zone one, 278°C in zone two, 285°C in zone three, 286°C in zone four, and 288°C in the spinning box. The resulting melt is extruded, cooled, oiled, and wound to obtain polyester POY fibers. The polyester POY fibers are then heated, false-twisted, heat-set, and wound to form cool-feeling and wind-resistant fibers.
8. The method of claim 7, wherein the cooling and air fibers are prepared by the steps of: The extrusion temperature is 270-290 DEG C, the cooling adopts side blowing, the temperature is 25 DEG C, the oiling selects TK-3182A, the oiling rate is 0.45%, the winding speed is 2800-3000 m / min, the elasticizing upper hot box temperature is 180-200 DEG C, the false twist speed is 550-700 m / min, the false twist ratio is 1.7-1.9, and the heat setting temperature is 180-190 DEG C.
9. The method for preparing cooling and wind-resistant fibers according to claim 1, characterized in that, The dispersing agent selects BYK163.
10. The method of claim 1, wherein the cooling and air fibers are prepared by the steps of: The lubricant selects pentaerythritol stearate, and the antioxidant selects PEP36.