Core-shell coaxial fibers, their fabrication methods, and nanogenerators containing them

By using core-shell coaxial fiber design and gallium-based liquid metal, the problems of incompatibility between rigidity and flexibility and low single energy conversion efficiency of triboelectric nanogenerators have been solved, realizing a self-powered solution with high energy density and stability, which is suitable for wearable electronics and implantable medical devices.

CN123108770APending Publication Date: 2026-11-17FUJIAN UNIV OF TECH
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202510635966.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-16
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing triboelectric nanogenerators suffer from problems such as incompatibility between rigid materials and flexible electronics, a single energy conversion mechanism limiting energy density improvement, low polarization efficiency of piezoelectric materials, and poor stability of conductive networks, leading to device failure under complex deformation and low energy conversion efficiency.

Method used

The coaxial fiber design with a core-shell structure achieves in-situ composite of triboelectric and piezoelectric functions through the combination of gallium-based liquid metal and PVDF fiber. By combining the self-healing properties of liquid metal and the stress buffering function of the shell, the interface electric field is optimized to regulate the direction of charge migration and simplify the mechanical energy transfer path.

Benefits of technology

This improves the electrical output performance and stability of nanogenerators, enabling a high-energy-density and ultra-thin, flexible self-powered solution suitable for wearable electronics and implantable medical devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108770A_ABST
    Figure CN123108770A_ABST
Patent Text Reader

Abstract

This invention relates to a core-shell coaxial fiber, comprising a shell fiber prepared from a PVDF spinning solution of gallium or a gallium alloy and a core fiber prepared from a PVP spinning solution of gallium or a gallium alloy, wherein the outer diameter of the coaxial fiber is 0.4-2.5 micrometers. It also relates to a method for preparing the core-shell coaxial fiber, a nanofiber film comprising the core-shell coaxial fiber, and a triboelectric-piezoelectric nanogenerator comprising the nanofiber film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the fields of electrospinning, triboelectric, and piezoelectric nanogenerators, specifically to the preparation of core-shell coaxial fibers using piezoelectric material PVDF, the preparation method thereof, and the triboelectric-piezoelectric nanogenerator comprising the core-shell coaxial fibers. Background Technology

[0002] Triboelectric nanogenerators (TENGs), as an emerging energy harvesting technology, have shown great potential in wearable electronics, self-powered sensing, and the Internet of Things (IoT) due to their ability to efficiently convert environmental mechanical energy into electrical energy. However, existing technologies still face key bottlenecks: First, traditional TENGs are mostly based on rigid substrates (such as metal electrodes or hard polymers), whose mechanical properties are inherently contradictory to the stretchable and bendable characteristics required for flexible electronics, leading to easy interface delamination or structural failure under complex deformations. Second, the energy conversion mechanism is singular; most studies focus only on the independent utilization of triboelectric or piezoelectric effects, while the synergistic enhancement mechanism of dual effects lacks systematic design, limiting further improvement in energy density. Therefore, coupling multiple energy conversion mechanisms to form hybrid nanogenerators (HNGs) has become a key research focus.

[0003] Current high-performance nanoparticles (HNGs) have achieved significant performance improvements through multi-effect coupling (triboelectric, piezoelectric, thermoelectric, etc.) and flexible structural innovations. However, HNG design still faces core challenges. From a structural design perspective, existing composite solutions often employ physically stacked discrete devices, leading to complex mechanical energy transfer paths, significant interfacial energy loss, and insufficient volume redundancy to meet the ultra-thin requirements of flexible electronics. Furthermore, it is difficult to simultaneously achieve the polarization efficiency and dynamic conductive network stability of piezoelectric materials. For example, while single PVDF fibers possess piezoelectric properties, their polarization efficiency is limited by insufficient β-phase crystallinity, and their surface charge density is significantly reduced by environmental humidity. In addition, traditional conductive fillers (such as carbon nanotubes and silver nanowires) are prone to fracture due to interfacial stress concentration during dynamic deformation, resulting in discontinuous conductive networks and further weakening charge collection efficiency.

[0004] Chinese patent document CN118842346A discloses a method for fabricating a hybrid dual piezoelectric-triboelectric nanogenerator based on all-piezoelectric nanofibers. The hybrid generator uses piezoelectric polymer PAN nanofiber films and piezoelectric polymer PVDF nanofiber films as the negative and positive friction layers, respectively, of the triboelectric nanogenerator. Both films are prepared by electrospinning, and their electrical output performance is significantly better than that of PAN / PVDF-based TENGs and conventional PTNGs. This invention designs a material and device structure to couple all factors, including electrostatic induction and piezoelectric effects, to improve the output of the nanogenerator, providing a new strategy for the development of nanogenerators. However, it does not discuss the role of the electric field within the core-shell interface in regulating charge migration in the core-shell structure; therefore, its advantages can be referenced to fabricate an integrated triboelectric-piezoelectric nanogenerator based on a coaxial fiber structure.

[0005] Traditional heterogeneous generation (HNG) achieves multi-effect coupling by physically stacking different functional units (such as triboelectric and piezoelectric layers). Mechanical energy transfer between heterogeneous interfaces requires traversing a viscoelastic medium, leading to interfacial frictional losses and stress dispersion, significantly reducing energy conversion efficiency. This invention proposes an integrated heterogeneous structure that simplifies the mechanical energy transfer path and reduces interfacial viscoelastic dissipation through intrinsic material coupling—specifically, in-situ composite of triboelectric and piezoelectric functional phases—replacing physical stacking. Furthermore, the electromechanical coupling between discrete units in traditional HNGs relies on external circuits, and the charges generated by triboelectric and piezoelectric effects are difficult to vector superimpose through a built-in electric field, limiting energy density to the physical limits of a single effect. This invention, however, modulates the migration direction of triboelectric and piezoelectric charges through an internal electric field at the core-shell interface, achieving directional superposition of multi-effect charges and enabling output power density to break through the theoretical boundaries of traditional discrete HNGs. Moreover, traditional dielectric fillers (such as ZnO, MXene, and BaTiO3) are costly to manufacture and have complex synthesis methods, hindering large-scale production and application. The liquid metal filler used in this invention is inexpensive and easy to synthesize. Its unique fluidity provides self-healing properties to maintain the stability of the conductive network. Combined with the stress buffering function of the shell material, it suppresses microstructure damage under cyclic loading and improves the durability and stability of the device. Summary of the Invention

[0006] To address the aforementioned technical problems, this invention is proposed. This invention aims to provide a method for fabricating an integrated triboelectric-piezoelectric nanogenerator based on a coaxial fiber structure, solving the problems of structural complexity and increased interfacial resistance caused by the physical superposition of existing hybrid nanogenerators. Simultaneously, it introduces a coaxial structure capable of controlling the migration direction of triboelectric and piezoelectric charges within the core-shell interface using an internal electric field, and a liquid metal nanofiller with unique fluidity, thereby simultaneously solving the challenges of efficiency, volume, flexibility, and stability. This improves the electrical output performance of the nanogenerator, providing a self-powered solution with both high energy density and ultra-thin flexibility for wearable electronics, implantable medical devices, and other applications.

[0007] A first aspect of the present invention provides a core-shell coaxial fiber comprising a shell fiber prepared from a PVDF spinning solution of gallium or a gallium alloy and a core fiber prepared from a PVP spinning solution of gallium or a gallium alloy, wherein the outer diameter of the coaxial fiber is 0.4-2.5 micrometers.

[0008] In a preferred embodiment of the coaxial fiber of the present invention, the average outer diameter of the core-shell structured coaxial fiber is 0.8-1.5 micrometers.

[0009] A second aspect of the present invention provides a method for preparing coaxial fibers with a core-shell structure, the method comprising:

[0010] 1) Disperse gallium or gallium alloy in a first solvent to obtain a first dispersion of gallium or gallium alloy;

[0011] 2) Add polyvinylidene fluoride (PVDF) to a first dispersion of gallium or gallium alloy and stir under heating to obtain a PVDF spinning solution of gallium or gallium alloy, which is the first spinning solution;

[0012] 3) Disperse gallium or gallium alloy in a second solvent to obtain a second dispersion of gallium or gallium alloy;

[0013] 4) Add polyvinylpyrrolidone (PVP) to the second dispersion of gallium or gallium alloy and stir under heating to obtain a PVP spinning solution of gallium or gallium alloy, which is the second spinning solution;

[0014] 5) Using the first spinning solution obtained in step 2) as the shell layer and the second spinning solution obtained in step 4) as the core layer, prepare PVDF / gallium or gallium alloy@PVP / gallium or gallium alloy coaxial nanofibers with a core-shell structure.

[0015] In a preferred embodiment of the method of the present invention, in step 1), the weight ratio of gallium or gallium alloy to the first solvent is 0.3-1.5:100, preferably 0.5-1.0:100.

[0016] Preferably, in step 3), the weight ratio of gallium or gallium alloy to the second solvent is 0.3-1.5:100, more preferably 0.5-1.0:100.

[0017] In a preferred embodiment of the method of the present invention, in step 2), the PVDF concentration of the first spinning solution is 10-40% by weight, and preferably, the amount of gallium or gallium alloy in the first spinning solution relative to PVDF is 0.5-10% by weight.

[0018] Preferably, in step 4), the PVP concentration of the second spinning solution is 5-30% by weight, and preferably, the amount of gallium or gallium alloy in the second spinning solution relative to PVP is 0.5-10% by weight.

[0019] In a preferred embodiment of the method of the present invention, in step 5), the spinning conditions are: a shell-core flow rate ratio of 2-5:1. Preferably, the shell solution push rate is 0.5-5 mL / h, and the core solution push rate is 0.2-3 mL / h.

[0020] In a preferred embodiment of the method of the present invention, in step 5), the spinning voltage is 5-20kV, the collection speed is 80-150rpm, and the collection distance is 10-20cm.

[0021] In a preferred embodiment of the method of the present invention, in step 1), the first solvent is a mixture of dimethylformamide and acetone. Preferably, the mass ratio of DMF to acetone is 2-5:1.

[0022] A third aspect of the present invention provides a nanofiber film comprising a core-shell coaxial fiber, wherein the core-shell coaxial fiber is a core-shell coaxial fiber of the present invention or is prepared by the method described in the present invention.

[0023] A fourth aspect of the present invention provides a triboelectric-piezoelectric nanogenerator comprising the nanofiber film of the present invention. Preferably, the nanofiber film serves as the negative electrode.

[0024] This invention addresses the following technical problems existing in the prior art:

[0025] 1. Traditional triboelectric nanogenerators are limited by rigid material systems and single energy conversion mechanisms (such as relying solely on triboelectric or piezoelectric effects), making it difficult to achieve multi-effect coupling and synergy on flexible substrates. Rigid materials prevent devices from adapting to complex deformation scenarios, while the single energy conversion mechanism limits the improvement of energy harvesting density, thus restricting their application potential in wearable devices, flexible electronics, and other fields.

[0026] 2. The polarization process of existing piezoelectric materials (such as PVDF) is complex and inefficient, resulting in insufficient β phase content and limited piezoelectric performance. At the same time, traditional conductive fillers (such as metal particles and carbon materials) are prone to fracture or interface debonding during mechanical deformation, resulting in poor dynamic stability and inability to maintain a continuous conductive network, which seriously weakens charge transport efficiency and device durability.

[0027] 3. Single-material systems (such as pure PVDF fibers) lack heterogeneous interface design, making it impossible to enhance polarization efficiency through core-shell synergy. Furthermore, charge separation relies solely on surface triboelectric effects, resulting in uneven internal polarization field distribution and a lack of interfacial dipole gradients. Single-component structures struggle to achieve directional charge migration and efficient trapping, hindering the construction of multiple energy conversion channels and limiting energy output density and device functionality.

[0028] The present invention can achieve the following beneficial effects:

[0029] (1) Simplified integrated design: Abandoning the complex architecture of traditional multi-component stacking, the integration of triboelectric, piezoelectric and conductive functions is achieved through a single fiber, forming a compact integrated structure, which greatly reduces system complexity and improves mechanical reliability;

[0030] (2) Interface optimization of core-shell structure: The core-shell layered design is adopted. Through the synergistic effect of the core layer (functional material) and the shell layer (encapsulation / control layer), the energy loss at the interface of heterogeneous materials is eliminated, the migration direction of triboelectric charge and piezoelectric charge is controlled, and the efficient coupling and transmission of mechanical stress and electrical signal is achieved.

[0031] (3) Addition of liquid metal filler: The addition of conductive filler increases the polarization of the material during electrospinning, enhances the output performance of the nanogenerator, and the unique fluidity of liquid metal has self-healing properties to maintain the stability of the conductive network. Combined with the stress buffering function of the shell material, it suppresses microstructure damage under cyclic load and improves the durability and stability of the device.

[0032] This invention employs a core-shell structure design, using the internal electric field at the core-shell interface to control the migration direction of triboelectric and piezoelectric charges, achieving directional superposition of multiple effect charges and enabling efficient coupling and transmission of mechanical stress and electrical signals. Furthermore, the addition of a gallium-based liquid metal with high conductivity and strong chemical stability enhances molecular polarization during electrospinning, while its unique fluidity maintains the stability of the conductive network. Combined with the stress-buffering function of the shell material, this suppresses microstructural damage under cyclic loading, improving device durability and stability. Attached Figure Description

[0033] The following figures are for illustrative and explanatory purposes only and do not limit the scope of the invention, wherein:

[0034] Figure 1 A flowchart illustrating the preparation process of a nanofiber film according to one embodiment of the present invention is shown.

[0035] Figure 2 (a)-(d) respectively show a surface SEM image, a cross-sectional SEM image, a fiber diameter distribution statistical analysis, and a TEM image of a single fiber of a PP nanofiber membrane according to one embodiment of the invention.

[0036] Figure 3 A physical image of a PP-TPU-based nanogenerator is shown.

[0037] Figure 4 (a)-(b) show the (a) open-circuit voltage and (b) short-circuit current of pure PVDF, PVDF / 3wt.%LMs, and PP fiber membrane (time axis from left to right) assembled with TPU to form nanogenerators.

[0038] Figure 5 (a1)-(a2) and Figure 5 (b)-(d) illustrate the self-powered applications and human signal monitoring of PP-TPU-based nanogenerators, in which... Figure 5 (a1) is a diagram of a bridge rectifier circuit for supplying power to a light bulb; Figure 5 (a2) is according to Figure 5 (a1) The current generated after connecting the circuit lit up the LED light; Figure 5 (b) The electrical signal generated when a fist is clenched; Figure 5 (c) Electrical signals generated when the arm is bent; Figure 5 (d) Electrical signals generated by arm compression during walking. Detailed Implementation

[0039] To provide a clearer understanding of the technical features, objectives, and effects of the invention, specific embodiments of the invention are now described with reference to the accompanying drawings, in which the same reference numerals denote the same parts.

[0040] Unless otherwise specified, all reactions in this article were carried out at room temperature and atmospheric pressure, and all reactants and reagents used were commercially available.

[0041] Unless otherwise specified, the concentration units mM and mmol / L have the same meaning in this article.

[0042] In this invention, unless otherwise specified, each amount is by weight and the ratio of amounts is by weight.

[0043] A first aspect of the present invention provides a core-shell coaxial fiber, comprising a shell fiber prepared from a PVDF spinning solution of gallium or a gallium alloy and a core fiber prepared from a PVP spinning solution of gallium or a gallium alloy, wherein the outer diameter of the coaxial fiber is 0.4-2.5 micrometers, preferably 0.4-1.8 micrometers. More preferably, the average outer diameter of the coaxial fiber is 0.8-1.5 micrometers, more preferably 0.9-1.2 micrometers.

[0044] Unless otherwise specified, the diameter of coaxial fibers in this article refers to their outer diameter. The outer diameter of the coaxial fibers was measured using Image-Pro Plus software. The average outer diameter was calculated by measuring the outer diameter of 100 fibers using Image-Pro Plus software, then creating a statistical distribution chart of the fiber diameters using Origin software, and finally calculating the average value D.

[0045] In this document, gallium (Ga) refers to pure gallium metal. Gallium alloys are alloys of gallium with one or more other metals such as indium (In), tin (Sn), and aluminum (Al). Examples of gallium alloys include, for instance, Ga-In alloys containing 75-95% Ga; Ga-Sn alloys containing 80-90% Ga; Ga-In-Sn alloys containing 60-75% Ga; and Ga-Al alloys containing 94-98% Ga. Preferably, gallium is a gallium-based liquid metal (LMs).

[0046] A second aspect of the present invention provides a method for preparing coaxial fibers with a core-shell structure, the method comprising:

[0047] 1) Disperse gallium or gallium alloy in a first solvent to obtain a first dispersion of gallium or gallium alloy;

[0048] 2) Add polyvinylidene fluoride (PVDF) to a first dispersion of gallium or gallium alloy and stir under heating to obtain a PVDF spinning solution of gallium or gallium alloy, which is the first spinning solution;

[0049] 3) Disperse gallium or gallium alloy in a second solvent to obtain a second dispersion of gallium or gallium alloy;

[0050] 4) Add polyvinylpyrrolidone (PVP) to the second dispersion of gallium or gallium alloy and stir under heating to obtain a PVP spinning solution of gallium or gallium alloy, which is the second spinning solution;

[0051] 5) Using the first spinning solution obtained in step 2) as the shell layer and the second spinning solution obtained in step 4) as the core layer, prepare PVDF / gallium or gallium alloy@PVP / gallium or gallium alloy coaxial nanofibers with a core-shell structure.

[0052] In step 1), the weight ratio of gallium or gallium alloy to the first solvent is 0.3-1.5:100, preferably 0.5-1.0:100.

[0053] In step 1), the first solvent can be one or more selected from N,N-dimethylformamide (DMF), acetone, and ethanol. Preferably, the first solvent is a mixture of DMF and acetone. More preferably, the mass ratio of DMF to acetone is 2-5:1, preferably 2-4:1, for example, 3:1.

[0054] In step 1), gallium or gallium alloy and the first solvent can be mixed ultrasonically for 1-5 hours, preferably 2-4 hours, for example 2 hours.

[0055] In step 2), heating is performed at 40-90°C, preferably 50-70°C. Heating can be, for example, oil bath heating. The heating time is 2-6 hours, preferably 3-5 hours, for example 4 hours.

[0056] In step 2), the PVDF concentration of the first spinning solution is 10-40% by weight, preferably 15-30% by weight.

[0057] In step 2), the amount of gallium or gallium alloy in the first spinning solution relative to PVDF is 0.5-10% by weight, preferably 2-8% by weight, more preferably 2-5% by weight, and even more preferably 3-5% by weight.

[0058] In step 2), the amount of gallium or gallium alloy relative to PVDF is 1-5% by weight, preferably 2-4% by weight, for example 3% by weight.

[0059] In step 3), the weight ratio of gallium or gallium alloy to the second solvent is 0.3-1.5:100, preferably 0.5-1.0:100.

[0060] In step 3), the second solvent can be one or more selected from N,N-dimethylformamide (DMF), acetone, and ethanol. Preferably, the second solvent is ethanol.

[0061] In step 3), gallium or gallium alloy and the second solvent can be mixed using ultrasound. The ultrasound time can be 1-5 hours, preferably 2-4 hours, for example, 2 hours.

[0062] In step 4), heating is performed at 40-90°C, preferably 50-70°C. Heating can be, for example, oil bath heating. The heating time is 2-6 hours, preferably 3-5 hours, for example 4 hours.

[0063] In step 4), the PVP concentration of the second spinning solution is 5-30% by weight, preferably 10-25% by weight.

[0064] In step 4), the amount of gallium or gallium alloy in the second spinning solution relative to PVP is 0.5-10% by weight.

[0065] In step 4), the amount of gallium or gallium alloy relative to PVP is 1-5% by weight, preferably 2-4% by weight, for example 3% by weight.

[0066] In step 5), the spinning conditions are: the core-shell flow rate ratio is 2-5:1.

[0067] In step 5), the shell solution is pushed at a rate of 0.5-5 mL / h, and the core solution is pushed at a rate of 0.2-3 mL / h.

[0068] In step 5), the spinning voltage is 5-20kV, preferably 10-15kV; the collection speed is 80-150rpm, preferably 100-130rpm; and the collection distance is 10-20cm, preferably 15-20cm.

[0069] In step 5), the coaxial needle can be, for example, a 21G / 17G coaxial needle or a 17G / 14G coaxial needle.

[0070] The PVDF / gallium or gallium alloy@PVP / gallium or gallium alloy coaxial nanofibers with core-shell structure prepared by the method of the present invention may be referred to as PP coaxial fibers in this paper.

[0071] The preferred embodiments of the coaxial fiber with the core-shell structure of the present invention are also applicable to the method of the present invention, and will not be described in detail here.

[0072] A third aspect of the present invention provides a nanofiber film comprising a core-shell coaxial fiber, wherein the core-shell coaxial fiber is a core-shell coaxial fiber of the present invention or is prepared by the method described in the present invention.

[0073] The nanofiber film of the present invention can be prepared by spinning with the first spinning solution described herein as the shell layer and the second spinning solution described herein as the core layer.

[0074] Spinning parameters can be:

[0075] The core-shell flow velocity ratio is 2-5:1;

[0076] The shell solution was pushed at a rate of 0.5-5 mL / h, and the core solution was pushed at a rate of 0.2-3 mL / h.

[0077] The spinning voltage is 5-20kV, preferably 10-15kV;

[0078] The collection speed is 80-150 rpm, preferably 100-130 rpm;

[0079] The collection distance is 10-20cm, preferably 15-20cm.

[0080] The coaxial needle can be, for example, a 21G / 17G coaxial needle or a 17G / 14G coaxial needle.

[0081] For example, the nanofiber film of the present invention can be prepared as follows: using the PVDF solution described herein as the shell layer and the PVP solution described herein as the core layer, adopting a shell-core layer flow rate ratio of 2-5:1, that is, the shell layer solution push rate is 0.5-5 mL / h and the core layer solution push rate is 0.2-3 mL / h, and using a 21G / 17G coaxial needle at a spinning voltage of 5-20 kV, a collection speed of 80-150 rpm and a collection distance of 10-20 cm, to prepare a coaxial nanofiber film.

[0082] Figure 1 A flowchart illustrating the preparation process of a coaxial nanofiber film according to one embodiment of the present invention is shown.

[0083] The prepared coaxial nanofiber film of the present invention was pretreated, for example, dried in an oven at 60°C for 8 hours, and then cut into small pieces for morphology characterization. Unless otherwise specified, the operating conditions for morphology characterization are those well known in the art.

[0084] Figure 2 (a) An SEM image of the surface of a coaxial nanofiber film according to one embodiment of the present invention. Figure 2 (b) An SEM image showing the cross-sectional morphology of a coaxial nanofiber film according to one embodiment of the present invention. Figure 2 (c) shows a diameter distribution chart of coaxial nanofibers according to one embodiment of the present invention. It can be observed that the overall fiber diameter distribution is relatively concentrated and the thickness is uniform. Figure 2 (d) is a TEM image of one of the coaxial nanofibers in one embodiment of the present invention. The coaxial structure of the fiber can be clearly observed from the image. It can be seen that the surface electrospinning process parameters are reasonably designed.

[0085] A fourth aspect of the present invention provides a triboelectric-piezoelectric nanogenerator comprising the nanofiber film of the present invention. Preferably, the nanofiber film serves as the negative electrode.

[0086] An exemplary fabrication method of the triboelectric-piezoelectric nanogenerator of the present invention is as follows:

[0087] TPU is added to a mixed solvent of DMF and tetrahydrofuran (THF) (mass ratio of, for example, 1:2-5), heated and stirred to obtain a TPU spinning solution;

[0088] TPU was electrospun using a single needle. The electrospinning process parameters were as follows: precursor solution solubility 19-20 wt.%, spinning voltage 5-20 kV, temperature 20-30℃, solution flow rate 0.5-2 mL / h, drum collection speed 100-400 rpm, and collection distance 10-30 cm. This yielded a uniformly shaped TPU nanofiber film, which served as the positive electrode of a triboelectric-piezoelectric nanogenerator.

[0089] The coaxial nanofiber thin film, i.e., PP nanofiber film of the present invention, is used as the negative electrode of the triboelectric-piezoelectric nanogenerator.

[0090] Both PP and TPU nanofiber films were cut into square blocks (e.g., 3cm × 3cm). Then, a polyimide (PI) film (e.g., 0.2mm thick) was selected as the substrate, and a PI film of the same size (e.g., 3cm × 3cm) was tightly bonded to its center. Next, wires, copper electrode sheets, and the PP nanofiber film were neatly stacked on top of the central PI film, thus successfully constructing one electrode of the TENG. The other electrode was constructed by stacking a TPU nanofiber film in the same manner. Finally, a sponge (e.g., 40ppi, 1.5cm high) was used to connect the two electrodes, fabricating a PP-TPU-based triboelectric-piezoelectric nanogenerator. Figure 3 As shown.

[0091] In this article, the raw materials used, such as polyvinylidene fluoride (PVDF), thermoplastic polyurethane (TPU) and polyvinylpyrrolidone (PVP), can be pretreated before use, for example, dried in an oven at 50-90°C for 2-8 hours to remove moisture.

[0092] The triboelectric-piezoelectric nanogenerator, including the coaxial fiber with a core-shell structure of this invention, exhibits significantly improved electrical output performance. The introduction of the coaxial structure further enhances the coupling between the triboelectric and piezoelectric effects, breaking through the upper limit of output performance. The nanogenerator assembled from a PP fiber membrane with a coaxial structure and a TPU fiber membrane demonstrates significantly higher electrical output performance than other types of nanogenerators.

[0093] Example

[0094] raw material

[0095]

[0096] Preprocessing

[0097] Polyvinylidene fluoride (PVDF) powder, thermoplastic polyurethane (TPU) beads, and polyvinylpyrrolidone (PVP) powder were dried in an oven at 60°C for 4 hours to remove moisture.

[0098] Preparation of core-shell structured coaxial fibers

[0099] 1. Add 0.06g of gallium-based liquid metal (LMs) to a mixed solvent of 8g of N,N-dimethylformamide (DMF) and acetone, wherein the mass ratio of DMF to acetone is 3:1, and sonicate the solution for 2 hours to completely disperse the LMs.

[0100] 2. Add 2g of dried PVDF powder to the dispersion in (2), and heat and stir in an oil bath at 60°C. After 4h, a PVDF spinning solution with a content of 3wt.% LMs (relative to PVDF) of 20wt.% is obtained.

[0101] 3. Add 0.048g LMs to 8.4g anhydrous ethanol and sonicate the solution for 2 hours to completely disperse the LMs;

[0102] 4. Add 1.6g of dried PVP powder to the dispersion in (4), heat and stir in an oil bath at 60°C, and after 4h, obtain a 16wt.% PVP spinning solution with 3wt.% LMs content (relative to PVP);

[0103] 5. Using the PVDF solution from step 3 as the shell layer and the PVP solution from step 5 as the core layer, and adopting a shell-core layer flow rate ratio of 5:2 (i.e., the shell layer solution push rate is 1 mL / h and the core layer solution push rate is 0.4 mL / h), a PVP / LMs@PVDF / LMs(PP) coaxial nanofiber film is prepared using a 21G / 17G coaxial needle at a spinning voltage of 10 kV, a collection speed of 120 rpm, and a collection distance of 15 cm.

[0104] Fabrication of integrated triboelectric-piezoelectric nanogenerators with fiber structures

[0105] 2g of dried TPU granules were added to a mixed solvent of 8g DMF and tetrahydrofuran (THF) (mass ratio 1:2), and the mixture was heated and stirred in an oil bath at 60°C for 6 hours to obtain a 20wt.% TPU spinning solution.

[0106] TPU was electrospun using a 20G needle. The electrospinning process parameters were: precursor solution solubility 20wt.%, spinning voltage 10kV, temperature 25℃, solution flow rate 1mL / h, roller collection speed 300rpm, and collection distance 15cm. A uniform TPU nanofiber film was obtained and used as the positive electrode of HNG.

[0107] The prepared PVP / LMs@PVDF / LMs(PP) coaxial nanofiber film was used as the negative electrode of HNG;

[0108] Both PP and TPU nanofiber films were cut into 3×3 cm blocks. A 0.2 mm thick commercial polyimide (PI) film was then used as a substrate, and a 3×3 cm PI film was tightly bonded to its center. Next, wires, copper electrodes, and the PP nanofiber film were neatly stacked on top of the central PI film, thus constructing one electrode of the TENG. The other electrode was constructed by stacking a TPU nanofiber film in the same manner. Finally, a 40 ppi, 1.5 cm high sponge was used to connect the two electrodes, fabricating a PP-TPU-based triboelectric-piezoelectric nanogenerator (HNG). Figure 3 As shown.

[0109] Performance testing

[0110] 1. PP fiber structure

[0111] The PP fiber membrane was placed in a 60℃ oven for 8 hours, then removed and cut into small pieces for morphology characterization testing. Its morphology characterization is as follows: Figure 2 As shown, Figure 2 (b) An SEM image showing the cross-sectional morphology of a coaxial nanofiber film according to one embodiment of the present invention. Figure 2 (c) shows a diameter distribution chart of coaxial nanofibers according to one embodiment of the present invention. It can be observed that the overall fiber diameter distribution is relatively concentrated and the thickness is uniform. Figure 2 (d) is a TEM image of one of the coaxial nanofibers in one embodiment of the present invention. The coaxial structure of the fiber can be clearly observed from the image. It can be seen that the surface electrospinning process parameters are reasonably designed.

[0112] 2. Statistical methods for fiber diameter

[0113] Using Image-Pro Plus software, the diameters of 100 fibers used in the SEM of the PP fiber film were measured and statistically analyzed. Subsequently, Origin software was used to generate a statistical distribution map of the fiber diameters, and the average value D was calculated. Figure 2 As shown in (a), the average outer diameter of the fiber is 0.4-1.6 micrometers and the average fiber diameter is 1.005 micrometers.

[0114] 3. Open-circuit voltage and short-circuit current of PP-TPU-based nanogenerators

[0115] The open-circuit voltage and short-circuit current of the PP-TPU-based nanogenerator are tested as follows:

[0116] Figure 3The image shows a PP-TPU-based HNG. Connect the wires on both sides to the positive and negative terminals of an electrometer (Keithley 6514). Fix the lower surface to the triboelectric testing device. Start the homemade triboelectric testing device. The device will output a cyclic force from the upper surface of the HNG, allowing the upper and lower films of the HNG to continuously contact and separate. Then, adjust the magnitude and frequency of the force output by the device, and switch the voltage and current modes of the electrometer to measure the open-circuit voltage and short-circuit current under a contact pressure of 20N and a contact frequency of 2Hz.

[0117] Figure 4 (a) Nanogenerators were assembled with TPU using pure PVDF, PVDF / 3wt.%LMs, and PP fiber films (time axis from left to right), and their open-circuit voltages (V) at a contact pressure of 20N and a contact frequency of 2Hz were measured. oc ), Figure 4 (b) is its corresponding short-circuit current (I) sc It can be observed that the electrical output performance of the three types gradually increases, with the PP-TPU-based nanogenerator exhibiting the highest electrical output performance. This indicates that the addition of LMs fillers significantly improves the output voltage of the nanogenerator, while the introduction of the coaxial structure further enhances the coupling of triboelectric and piezoelectric effects, further breaking through the upper limit of output performance. The nanogenerator assembled from PP fiber membranes with coaxial structures and TPU fiber membranes exhibits significantly higher electrical output performance than other types of nanogenerators.

[0118] 4. Self-powered applications and human signal monitoring of PP-TPU-based HNGs

[0119] according to Figure 5 In the circuit in (a1), HNG is directly connected to the light bulb. Then, HNG is tapped by hand to separate the upper and lower electrodes, which generates current and lights up the light bulb. Figure 5 (b) to Figure 5 (d) For human signal detection, first fix the HNG in a specific position, such as the palm, elbow, or side of the clothing (using double-sided tape). Then connect the wires on both sides of the HNG to the electrometer. Finally, perform human movements to obtain the corresponding electrical signal curve (voltage curve).

[0120] Due to its lightweight, fast response, softness, and excellent stability, PP-TPU-based nanogenerators can be widely used in the field of self-powered wearable devices. Figure 5 This demonstrates its potential as a self-powered sensor in human motion signal detection. Figure 5 The bridge rectifier circuit shown in (a1) connects the HNG and the LED. When pressed by hand, the HNG disconnects, and the induced current generated in the external circuit lights the small bulb. Figure 5As shown in (a2). Figure 5 (b) shows the change in HNG electrical signal when the hand is clenched into a fist. Figure 5 (c) illustrates the changes in the HNG electrical signal during arm flexion. For example... Figure 5 As shown in (d), when the HNG is connected to the side of the body, an electrical signal is generated when the arm comes into contact with it during walking. The stability and versatility demonstrated by the above applications indicate that the PLPE-TPU-based nanogenerator self-powered sensor has strong application potential in the fields of human motion and wearable devices.

[0121] The detailed descriptions listed above are merely specific illustrations of feasible embodiments of the present invention and are not intended to limit the scope of protection of the present invention. All equivalent embodiments or modifications made without departing from the spirit of the present invention should be included within the scope of protection of the present invention.

Claims

1. A core-shell coaxial fiber, comprising a shell fiber prepared from a PVDF spinning solution of gallium or a gallium alloy and a core fiber prepared from a PVP spinning solution of gallium or a gallium alloy, wherein, The outer diameter of the coaxial fiber is 0.4-2.5 micrometers.

2. The coaxial fiber with a core-shell structure according to claim 1, wherein, The average outer diameter of the coaxial fibers in the core-shell structure is 0.8-1.5 micrometers.

3. A method for preparing a core-shell coaxial fiber, the method comprising: 1) Disperse gallium or gallium alloy in a first solvent to obtain a first dispersion of gallium or gallium alloy; 2) Add polyvinylidene fluoride (PVDF) to a first dispersion of gallium or gallium alloy and stir under heating to obtain a PVDF spinning solution of gallium or gallium alloy, which is the first spinning solution; 3) Disperse gallium or gallium alloy in a second solvent to obtain a second dispersion of gallium or gallium alloy; 4) Add polyvinylpyrrolidone (PVP) to the second dispersion of gallium or gallium alloy and stir under heating to obtain a PVP spinning solution of gallium or gallium alloy, which is the second spinning solution; 5) Using the first spinning solution obtained in step 2) as the shell layer and the second spinning solution obtained in step 4) as the core layer, prepare PVDF / gallium or gallium alloy@PVP / gallium or gallium alloy coaxial nanofibers with a core-shell structure.

4. The method according to claim 3, wherein, In step 1), the weight ratio of gallium or gallium alloy to the first solvent is 0.3-1.5:100, preferably 0.5-1.0:100; Preferably, in step 3), the weight ratio of gallium or gallium alloy to the second solvent is 0.3-1.5:100, more preferably 0.5-1.0:

100.

5. The method according to claim 4, wherein, In step 2), the PVDF concentration of the first spinning solution is 10-40% by weight, and preferably, the amount of gallium or gallium alloy in the first spinning solution relative to PVDF is 0.5-10% by weight. Preferably, in step 4), the PVP concentration of the second spinning solution is 5-30% by weight, and preferably, the amount of gallium or gallium alloy in the second spinning solution relative to PVP is 0.5-10% by weight.

6. The method according to any one of claims 3-4, wherein, In step 5), the spinning conditions are as follows: The shell-core flow rate ratio is 2-5:

1. Preferably, the shell solution push rate is 0.5-5 mL / h, and the core solution push rate is 0.2-3 mL / h.

7. The method according to any one of claims 3-5, wherein, In step 5), the spinning voltage is 5-20kV, the collection speed is 80-150rpm, and the collection distance is 10-20cm.

8. The method according to any one of claims 3-6, wherein, In step 1), the first solvent is a mixture of dimethylformamide and acetone, preferably, the mass ratio of DMF to acetone is 2-5:

1.

9. A nanofiber film comprising a core-shell coaxial fiber, wherein the core-shell coaxial fiber is prepared according to any one of claims 1-2 or according to any one of claims 3-8.

10. A triboelectric-piezoelectric nanogenerator, comprising the nanofiber film according to claim 9, preferably, wherein the nanofiber film serves as the negative electrode.

Citation Information

Patent Citations

  • Full-piezoelectric nanofiber-based hybrid dual piezoelectric-triboelectric nano generator and application thereof

    CN118842346A