A core-sheath composite fiber and its preparation method, a reinforced subfloor, and an impermeable board.

By using light rare earth element-modified copolymer polyester and nano-montmorillonite-modified polyester core composite fiber, the problems of easy aging and insufficient water resistance of polymer materials under ultraviolet radiation have been solved, achieving high tensile strength and durability, making it suitable for harsh environments such as pumped storage power stations.

CN123108773APending Publication Date: 2026-11-17BEIJING DONGFANG YUHONG ANTICORROSION TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611307044.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-26
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing polymer materials are prone to aging under ultraviolet radiation, have insufficient tensile and tear strength, and their water resistance decreases under long-term immersion conditions, making it difficult to meet engineering requirements under complex stress conditions.

Method used

The fiber uses a light rare earth element modified copolyester as the sheath and nano-montmorillonite modified polyester as the core. By forming coordination chemical bonds between the copolyester and modified bitumen, combined with the labyrinth effect of nano-montmorillonite, the fiber's anti-aging, water resistance and mechanical properties are improved.

Benefits of technology

It achieves chemical cross-linking between the core-sheath composite fiber and modified asphalt, improves interfacial bonding ability, prevents asphalt separation and spillage, and has excellent fatigue resistance and durability, making it suitable for harsh environments such as pumped storage power stations.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108773A_ABST
    Figure CN123108773A_ABST
Patent Text Reader

Abstract

This application provides a core-sheath composite fiber and its preparation method, a reinforced subbase, and an impermeable board, belonging to the technical field of impermeable materials. The core-sheath composite fiber includes a sheath layer and a core layer. The sheath layer is a light rare earth element modified copolyester, which is a copolymer of sodium isophthalate sulfonate and polyester. The core layer includes nano-montmorillonite modified polyester.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of seepage-proof materials, and relates to a core-sheath composite fiber and its preparation method, a reinforced base layer and a seepage-proof board. More specifically, it relates to a core-sheath composite fiber for reinforcing the base layer of a modified asphalt seepage-proof board, a two-layer fabric-one-film reinforced base layer containing the core-sheath composite fiber, a reinforced base layer containing the core-sheath composite fiber and having a two-layer fabric-one-film structure, and a modified asphalt seepage-proof board containing the same. This seepage-proof board is particularly suitable for harsh environments such as seepage prevention in pumped storage power station reservoir basins, dam surface seepage prevention, and lining of water conveyance tunnels. Background Technology

[0002] With the rapid development of the water conservancy engineering field, more severe challenges and higher requirements have been put forward for the seepage prevention materials of its seepage prevention system.

[0003] Geotextiles, as a core component of seepage control systems, are currently commonly made from synthetic fibers such as polypropylene (PP) and polyethylene terephthalate (PET). However, during service, the molecular chains of these polymer materials are susceptible to breakage due to ultraviolet radiation, leading to UV aging. Furthermore, their tensile and tear strengths often fail to meet the engineering requirements under complex stress conditions. Simultaneously, in long-term immersion environments, the internal microstructure of geotextile materials may swell or hydrolyze, reducing their water resistance and severely limiting their long-term reliability.

[0004] Therefore, developing geotextiles with excellent properties such as high resistance to ultraviolet aging, good mechanical properties, and long-term water resistance stability is very important for promoting the development of high-performance seepage prevention materials. Summary of the Invention

[0005] In view of the above, in order to at least partially solve at least one of the aforementioned technical problems, this application provides a core-sheath composite fiber and its preparation method, a reinforced tire base layer, and an impermeable board.

[0006] As a first aspect of this application, a core-sheath composite fiber is provided, comprising: a core layer and a sheath layer, the sheath layer being a light rare earth element modified copolyester, the copolyester being a copolymer of sodium isophthalate sulfonate and polyester, and the core layer comprising nano-montmorillonite modified polyester.

[0007] As a second aspect of this application, a method for preparing the aforementioned core-sheath composite fiber is provided, comprising: feeding a light rare earth element complex and a copolyester into a twin-screw extruder for melt mixing, followed by extrusion granulation to obtain a sheath-modified material; feeding polyester and nano-montmorillonite into a twin-screw extruder for melt mixing, followed by extrusion granulation to obtain a core-modified material; feeding the sheath-modified material and the core-modified material into a core-sheath composite spinning assembly respectively, followed by extrusion, stretching, and heat setting to obtain the core-sheath composite fiber.

[0008] As a third aspect of this application, a reinforced tire base layer is provided, which is made of the aforementioned core-sheath composite fiber.

[0009] As a fourth aspect of this application, a seepage-proof board is provided, comprising the aforementioned reinforced base layer.

[0010] Based on the above technical solutions, the core-sheath composite fiber and its preparation method, the reinforced subgrade, and the impermeable board provided in this application have at least one of the following beneficial effects:

[0011] (1) In this application, the core-sheath composite fiber can be used as a raw material for weaving geotextiles, improving the interfacial bonding strength with modified asphalt. Specifically, on the one hand, through the coordination chemical bonds formed between the light rare earth elements in the sheath and the modified asphalt, cross-linking with the asphalt is achieved, effectively preventing asphalt separation and spillage; on the other hand, through the anti-aging function of the light rare earth elements and the labyrinth effect of nano-montmorillonite, the core-sheath composite fiber has excellent properties such as aging resistance, water immersion resistance, resistance to alternating wet and dry conditions, and resistance to water pressure cycle fatigue. The core layer of nano-montmorillonite-modified polyester provides mechanical reinforcement and physical barrier, achieving crack resistance.

[0012] (2) In this application, the preparation method of the core-sheath composite fiber is simple and suitable for industrialization. In addition, the reinforced base layer and the seepage barrier prepared using the above-mentioned core-sheath composite fiber have excellent mechanical properties, seepage prevention performance, durability, water immersion resistance and freeze-thaw cycle performance, and are particularly suitable for harsh environments such as seepage prevention of reservoir basins of pumped storage power stations, seepage prevention of dam surfaces, and lining of water conveyance tunnels. Attached Figure Description

[0013] Figure 1 This is a schematic diagram of the cross-sectional structure of the core-sheath composite fiber of this application;

[0014] Figure 2 This is a schematic diagram of the seepage-proof board of this application.

[0015] [Attached image labels]

[0016] 10-cortex, 11-light rare earth elements, 20-core layer, 21-polyester, 22-nano-montmorillonite;

[0017] 1-Upper protective material layer, 2-Overlapping edge membrane, 3-Upper surface modified asphalt coating layer, 4-Upper geotextile layer, 5-Polymer membrane layer, 6-Lower geotextile layer, 7-Lower surface modified asphalt coating layer, 8-Lower protective isolation layer. Detailed Implementation

[0018] To make the objectives, technical solutions, and advantages of this application clearer, the following detailed description is provided in conjunction with specific embodiments and the accompanying drawings.

[0019] Pumped storage power stations are developing rapidly as a key regulating power source in the new power system. The seepage prevention systems of pumped storage power stations face a series of more stringent service environments than conventional building waterproofing projects. For example, the seepage prevention systems of pumped storage power stations withstand higher hydrostatic pressures, typically requiring no less than 1.5 MPa, and even exceeding 2.0 MPa at high-head dams. Conventional building waterproofing typically only needs to withstand water pressures of 0.3 to 0.6 MPa. Under high water pressure, the seepage prevention layer of pumped storage power stations must have the ability to maintain high water pressure for extended periods, meaning it must be able to withstand 2.0 MPa for 30 consecutive days without leakage. It must also withstand frequent water pressure cycling fatigue. Simulating the repeated impacts from 0 to 2.0 MPa due to daily water level changes, it must maintain a performance retention rate of no less than 93% after 1000 cycles, a requirement not met by conventional building waterproofing. During their designed service life of 50 to 100 years, the waterproofing materials used in pumped storage power stations must not only withstand continuous water immersion but also cope with repeated wet-dry cycles caused by water level changes, as well as freeze-thaw cycles (up to 200 cycles) during winter operation in high-altitude and cold regions. Furthermore, the seepage prevention layer of a pumped storage power station must be fused integrally with the dam surface concrete to ensure long-term stable operation. Therefore, its bonding strength requirements are much higher than those for ordinary parts such as roofs or basement exterior walls, and it must possess excellent resistance to hydrostatic pressure delamination to ensure it does not peel off under high water pressure. Simultaneously, the seepage prevention materials for pumped storage power stations must also withstand heat aging (performance retention rate ≥80% after 80℃ and 168h) and long-term water immersion (performance retention rate ≥85%), while building waterproofing typically has no or lower requirements for these indicators.

[0020] Currently, there is a lack of modified asphalt anti-seepage materials specifically designed for water conservancy, especially pumped storage power stations, which are subject to high water pressure, frequent water level changes, long-term water immersion, alternating wet and dry conditions, and freeze-thaw cycles. In response, this application develops a core-sheath composite fiber specifically for anti-seepage in pumped storage power stations, its preparation method, a core-sheath composite fiber reinforced base layer, and an anti-seepage board with a core-sheath composite fiber reinforced base layer.

[0021] Figure 1 This is a schematic diagram of the interface structure of the core-sheath composite fiber in this application.

[0022] like Figure 1 As shown, the core-sheath composite fiber of this application includes: a sheath layer 10 and a core layer 20. The sheath layer 10 is a copolyester modified with light rare earth element 11, and the copolyester is a copolymer of sodium isophthalate sulfonate and polyester. The core layer 20 includes polyester 21 modified with nano-montmorillonite 22.

[0023] In the embodiments of this application, the sheath and core layers are modified respectively, and the synergistic effect of the sheath and core layers is utilized to give the sheath-core composite fiber superior mechanical properties, durability, aging resistance, water immersion resistance, dry-wet alternation resistance, and water pressure cyclic fatigue resistance.

[0024] Specifically, the copolyester network structure formed by copolymerizing sodium isophthalate sulfonate (SIPA) with polyester can fix the light rare earth element complex, thereby obtaining a light rare earth element modified copolyester, which is the sheath of the core-sheath composite fiber. In the light rare earth element modified copolyester, the light rare earth elements act as coordination centers. On the one hand, they can form coordination bonds with polar groups (such as carboxyl groups and hydroxyl groups) in the modified asphalt, anchoring the asphalt molecules to the surface of the core-sheath composite fiber. On the other hand, they can form stable coordination bonds and ionic bonds with ester groups and sulfonic acid groups in the sheath copolyester, allowing the light rare earth elements to be anchored in situ in the sheath copolyester network. This enables the light rare earth elements to form molecular bridges between the modified asphalt and the core-sheath composite fiber, achieving chemical cross-linking and improving the interfacial bonding ability between the core-sheath composite fiber and the modified asphalt. Furthermore, the sodium isophthalate sulfonate (SIPA) in the copolyester contains sodium sulfonate (-SO3Na) polar groups, which improve the polarity of the skin layer and enhance its compatibility with asphalt. Thus, by chemically cross-linking the skin layer to improve interfacial bonding and compatibility with modified asphalt, the migration, separation, and leakage of modified asphalt during long-term use are effectively prevented, ensuring long-term stability of the impermeability. Simultaneously, the core-skin composite fiber exhibits excellent fatigue resistance, remaining unbroken under repeated water pressure. Light rare earth elements also possess unique electronic transition characteristics and low-temperature toughening effects (no cracking at -35℃). Utilizing their unique electronic transition characteristics, they can absorb 200-400nm ultraviolet light and convert it into heat or fluorescence, and can quench polymer free radicals, inhibiting photo-oxidative degradation, thereby achieving aging resistance. In addition, the low-temperature toughening properties of light rare earth elements ensure that the core-skin composite fiber does not crack during long-term use and in low-temperature environments.

[0025] In the core layer, layered nano-montmorillonite (OMMT) is uniformly exfoliated and dispersed within the polyester matrix, forming a nanoscale interpenetrating network to enhance the strength and modulus of the core-sheath composite fiber. This network also extends the stress transmission path and reduces stress concentration. Under external stress, the nanoscale interpenetrating network provides dynamic mechanical support, maintaining stability. Furthermore, the layered structure of the nano-montmorillonite, to some extent, forms a dense barrier network and creates a labyrinth effect within the polyester matrix, extending the migration path of water molecules and blocking their penetration. Combined with the hydrolysis-resistant chemical coordination bonds formed between the aforementioned light rare earth elements and bitumen, this ensures the stable performance of the core-sheath composite fiber under long-term water immersion and alternating wet-dry cycles.

[0026] In some embodiments, the weight ratio of the skin layer to the core layer is 5-10:95-90, for example, 5:95, 8:92, or 10:90. This ratio balances impermeability and mechanical properties. If the skin layer ratio is too low, the interfacial bonding force between it and the modified asphalt is insufficient, failing to anchor the modified asphalt molecules and leading to delamination over long-term use. If the skin layer ratio is too high, the core layer's supporting force is insufficient, resulting in a decrease in the overall mechanical strength and impermeability of the skin-core composite fiber.

[0027] In some implementations, the light rare earth element may be selected from at least one of lanthanum, cerium, praseodymium, and neodymium.

[0028] The light rare earth elements selected in this application can react with the sulfonic acid groups (-SO3) on the copolymer molecular chain. - The ester group (-COO-) forms coordinate and ionic bonds, and the skin matrix is ​​SIPA sulfonated copolyester, with a molecular chain containing high density sulfonic acid groups (-SO3). - The modified ester groups in the core layer have a much higher functional group density than those in pure PET, allowing them to form stable coordination bonds with light rare earth elements. This anchors the light rare earth elements in situ within the copolyester network of the sheath layer, effectively preventing the loss of rare earth components during high-temperature processing and long-term service. Although the core layer contains ester groups, it is only ordinary PET and lacks strong coordination groups such as sulfonic acid groups, resulting in weak binding force for rare earth ions and an inability to adsorb rare earth elements. Therefore, the rare earth functional components are stably enriched in the sheath layer. Simultaneously, the interface between the sheath and core layers is dense, with no molecular diffusion channels, thus maintaining stability during subsequent high-temperature spinning, thermal lamination, asphalt coating, and long-term service, without desorption or migration loss. Furthermore, the light rare earth elements can form stable coordination bonds with polar groups (carboxyl groups, hydroxyl groups, etc.) in the asphalt, enhancing the chemical and interfacial bonding between the sheath-core composite fiber and the asphalt.

[0029] Furthermore, based on copolyester, the amount of light rare earth element complex added is 0.5-1.0 wt%, for example, 0.5 wt%, 0.8 wt%, or 1.0 wt%. At the aforementioned amounts of light rare earth element complex, the coordination effect of light rare earth elements can be effectively utilized. If the amount of light rare earth element complex added is too low (e.g., <0.5 wt%), the chemical bonding and anti-aging effects will not be fully realized. If the amount of light rare earth element complex added is too high (e.g., >1.0 wt%), the effect will not be effectively improved, and costs may increase.

[0030] In some embodiments, the copolymerization ratio of sodium isophthalate sulfonate (SIPA) in the copolyester is 3-6 mol%, for example, 3 mol%, 5 mol%, or 6 mol%. The sodium sulfonate group (-SO3Na) of SIPA is a polar group, which can improve the compatibility between the copolyester and the asphalt, thereby enhancing the interfacial bonding between the skin layer and the modified asphalt. By controlling the SIPA copolymerization ratio within the range of 3-6 mol%, the regularity of the polyester molecular chain can be maintained while introducing polar groups. If the SIPA copolymerization ratio is too low (<3 mol%), the number of polar groups is insufficient, and the compatibility improvement effect is not obvious; if the SIPA copolymerization ratio is too high (>6 mol%), it may destroy the regularity of the polyester molecular chain, leading to a decrease in crystallinity and mechanical properties.

[0031] In some embodiments, based on polyester, the addition amount of nano-montmorillonite (OMMT) is 0.3-0.8 wt%, for example, 0.3 wt%, 0.5 wt%, or 0.8 wt%. This addition range ensures the uniform dispersion of nano-montmorillonite in the polyester matrix and fully utilizes its mechanical properties and labyrinth effect, while avoiding core brittleness due to excessive agglomeration. The interlayer spacing of nano-montmorillonite is ≥3.0 nm. On the one hand, an appropriate interlayer spacing is beneficial for nano-montmorillonite to construct a dense barrier network within the polyester matrix, thereby improving mechanical properties. On the other hand, it can fully utilize the labyrinth effect, significantly extending the migration path of water molecules, thus effectively improving the hydrolytic stability and durability of the core-sheath composite fiber.

[0032] In some embodiments, the core layer further includes 1.0-2.0 wt% compatibilizer, with the addition amount being, for example, 1.0 wt%, 1.5 wt%, or 2.0 wt%. The addition of the compatibilizer improves the compatibility of nano-montmorillonite within the polyester matrix, preventing the nano-montmorillonite from migrating or overflowing during long-term service.

[0033] In some embodiments, the compatibilizer is selected from polyester grafted with maleic anhydride, that is, maleic anhydride (MAH) is grafted onto the molecular chain segments of the polyester. The aforementioned polyester can be polyethylene terephthalate (PET), and the grafting rate of MAH is 0.8-1.5 wt%, for example, 0.8 wt%, 1.0 wt%, or 1.5 wt%. In other words, the compatibilizer used in this application is polyethylene terephthalate grafted with maleic anhydride (PET-g-MAH). Using polyester grafted with maleic anhydride as a compatibilizer improves the compatibility between nano-montmorillonite and polyester by chemically bonding maleic anhydride with the hydroxyl groups on the surface of nano-montmorillonite in the core layer. On the other hand, the polyester in the grafted material has the same structure as the polyester matrix in the core layer, which also helps to improve the compatibility between nano-montmorillonite and polyester.

[0034] In some embodiments, the core layer further includes 0.1-0.2 wt% of a flowability improver, for example, 0.1 wt%, 0.15 wt%, or 0.2 wt%, preferably 0.15 wt%-0.2 wt%. The added flowability improver reduces apparent viscosity by inhibiting intermolecular hydrogen bonding, thereby effectively reducing the melt flowability of the core layer system, reducing spinning breakage, and improving processing rheology. While improving flowability at the aforementioned addition amounts, excessive addition avoids deterioration of mechanical properties, achieving a balance between processing performance and core layer mechanical properties. Further, in this application, the flowability improver is selected from at least one of organic complex rheology modifiers, hyperbranched polymers, and dendritic polymer flow lubricants.

[0035] As a second aspect of this application, a method for preparing the above-mentioned core-sheath composite fiber is provided, comprising: steps A1-A3.

[0036] Step A1: The light rare earth element complex and the copolyester are fed into a twin-screw extruder for melt mixing, and then extruded and granulated to obtain the skin-modified material, which is a light rare earth element modified copolyester.

[0037] Step A2: The polyester and nano-montmorillonite are fed into a twin-screw extruder for melt mixing, and then extruded and granulated to obtain the core layer modified material.

[0038] Step A3: The modified sheath material and the modified core material are fed into the sheath-core composite spinning assembly, and after extrusion, stretching, and heat setting, the sheath-core composite fiber is obtained.

[0039] In this application, sodium isophthalate sulfonate (SIPA) is copolymerized with polyester, and the resulting copolyester is then fed into a twin-screw extruder for in-situ polymerization or melt mixing. Following extrusion granulation, a sheath-modified material is obtained. Similarly, a core-modified material can be obtained through a twin-screw melt mixing process. Finally, the sheath-modified material and the core-modified material are fed into an existing sheath-core composite spinning assembly, and a sheath-core composite fiber is obtained using a sheath-core composite spinning process. The sheath-core composite fiber weaving process of this application is simple and suitable for existing production equipment.

[0040] In some embodiments, the light rare earth element complex, by mass fraction, consists of 20% La2O3, 45% CeO2, and 5% Pr6O3. 11 It consists of 30% Nd2O3.

[0041] In some embodiments, the temperature of the melt mixing in the twin-screw extruder in steps A1-A2 is 260-280°C, the rotation speed of the twin screw is 200-400 rpm, and the residence time is 1-3 min.

[0042] In some embodiments, the core-sheath composite fiber is woven using a core-sheath composite spinning process in step A3. During the spinning process, the modified sheath material and the modified core material are fed into the core-sheath composite spinning assembly respectively, and the weight ratio of the sheath to the core is controlled at (5-10):(95-90), the spinning temperature is controlled at 275-285℃, the stretch ratio is controlled at 3.5-4.5 times, and the heat setting temperature is set at 180-200℃. The resulting core-sheath composite fiber has excellent mechanical properties.

[0043] In some embodiments, a compatibilizer and / or flow improver are added to the twin-screw extruder during the preparation of the core layer modified material. The compatibilizer may be 1.0-2.0 wt% polyethylene terephthalate grafted maleic anhydride (PET-g-MAH).

[0044] As a third aspect of this application, a reinforced tire base layer is provided, which is made of the aforementioned core-sheath composite fiber.

[0045] In this application, the geotextile woven with core-sheath composite fibers as the reinforcing base layer exhibits excellent mechanical properties and does not crack under long-term use and low-temperature environments. Furthermore, it demonstrates excellent interfacial bonding with modified asphalt, is resistant to delamination over long-term use, water immersion, alternating wet and dry conditions, and freeze-thaw cycles.

[0046] In some embodiments, the reinforcing base layer of this application may have a one-layer geotextile-one-membrane structure, i.e., geotextile / polymer membrane; or it may have a two-layer geotextile-one-membrane structure, i.e., upper geotextile / polymer membrane / lower geotextile, wherein the upper geotextile layer and / or the lower geotextile layer are woven from the aforementioned core-sheath composite fibers. Compared to the one-layer geotextile-one-membrane structure, the two-layer geotextile-one-membrane structure is preferred as the structure of the reinforcing base layer. The polymer membrane layer material may be selected from at least one of high-density polyethylene (HDPE) and polyvinyl chloride (PVC), with a thickness of 0.3-1.0 mm, for example, 0.3 mm, 0.5 mm, or 1.0 mm. The geotextile, or the upper geotextile layer / lower geotextile layer, has a basis weight of 50-200 g / m². 2 For example, it can be 50g / m 2 100g / m 2 200g / m 2 .

[0047] In summary, this application combines a geotextile layer woven from core-sheath composite fibers with a polymer membrane layer. By utilizing the synergistic effect of the two, the resulting reinforced subgrade possesses excellent mechanical properties, outstanding impermeability, and good asphalt compatibility.

[0048] As a fourth aspect of this application, a seepage-proof board is provided, comprising the aforementioned reinforced base layer.

[0049] In some embodiments, the impermeable board further includes an upper surface modified bitumen coating layer formed by coating modified bitumen coating material onto the upper surface of the reinforced base course, a lower surface modified bitumen coating layer formed by coating modified bitumen coating material onto the lower surface, a lower cover isolation and protection layer adhered to the lower surface modified bitumen coating layer, and an upper cover protective material layer located on the upper surface modified bitumen coating layer.

[0050] In some implementations, a reinforced base layer with a one-layer fabric-one-layer membrane structure or a reinforced base layer with a two-layer fabric-one-layer membrane structure can be used to make an impermeable board.

[0051] Figure 2 This is a schematic diagram of the seepage-proof board of this application.

[0052] like Figure 2 As shown, the impermeable board includes, from top to bottom: an upper protective material layer 1, an upper modified asphalt coating layer 3, a reinforced base layer, a lower modified asphalt coating layer 7, a lower isolation and protection layer 8, and a removable overlap membrane 2 that is reserved on the upper modified asphalt coating layer 3 and the lower modified asphalt coating layer 7. The reinforced base layer is composed of an upper geotextile layer 4, a polymer membrane layer 5, and a lower geotextile layer 6.

[0053] In some embodiments, the upper protective material layer 1 is at least one of sintered sand and basalt sand, with a mesh size of 10-40 mesh, for example, 10 mesh, 20 mesh, or 40 mesh.

[0054] In some embodiments, the modified asphalt coating material used in the upper surface modified asphalt coating layer 3 and the lower surface modified asphalt coating layer 7 comprises the following components in parts by weight: 55-65 parts petroleum asphalt, 1-6 parts styrene-butadiene-styrene block copolymer (SBS), 1-6 parts styrene-butadiene rubber (SBR), 1-5 parts isotactic polypropylene (IPP), 1-5 parts random polyalphaolefin (APAO), and 5-20 parts inorganic filler. Among these components, SBS and SBR synergistically toughen the material, IPP improves heat resistance and dimensional stability, and APAO enhances strength and reduces cost. Utilizing the synergistic effect of these components, the modified asphalt coating layer possesses both excellent mechanical properties and durability.

[0055] In some embodiments, the lower protective layer 8 can be a non-woven fabric or a polymer isolation film, which can be selected from either polyethylene (PE) film or polypropylene (PP) film.

[0056] In some embodiments, the overlapping edge film 2 is an adhesive material, which can be selected from either PE film or PP film.

[0057] The impermeable board prepared using the reinforced base layer of this application has a maximum peak tensile strength ≥1000N / 50mm, hydrostatic pressure ≥2.0MPa, no leakage after 30 days of constant pressure at 2.0MPa, water pressure cycle fatigue retention rate ≥93%, fatigue resistance retention rate ≥88%, retention rate ≥90% after 500 cycles of wet and dry alternation, and retention rate ≥90% after 200 cycles of freeze-thaw cycle. It can meet the use requirements of harsh environments such as high water pressure (≥2.0MPa), water pressure cycle fatigue, wet and dry alternation, and freeze-thaw cycle.

[0058] In summary, the core-sheath composite fiber, reinforced substrate, and impermeable board provided in this application can be industrially applied in water conservancy and hydropower engineering fields such as whole reservoir basin seepage prevention in pumped storage power stations, dam surface seepage prevention, and water conveyance tunnel lining.

[0059] The method and process described in this application are feasible, and the raw materials are widely available. Large-scale production can be achieved by relying on existing core-sheath composite spinning equipment and modified bitumen roll production lines.

[0060] To make the objectives, technical solutions and advantages of this application clearer, the following detailed description of the core-sheath composite fiber, the preparation method of the core-sheath composite fiber, the reinforced tire base layer and the impermeable board provided by this application is provided in conjunction with specific embodiments, but these descriptions should not be construed as limiting the scope of protection of this application.

[0061] Raw material source and specifications

[0062] The sources and specifications of the raw materials used in this embodiment and the comparative example are shown in Table 1.

[0063] Table 1. Sources and specifications of raw materials used in the examples and comparative examples

[0064]

[0065] Performance testing methods

[0066] The performance testing methods for the embodiments and comparative examples of this application are shown in Tables 2 and 3.

[0067] Table 2. Performance testing methods for examples and comparative examples

[0068]

[0069] Table 3. Performance testing methods for examples and comparative examples

[0070]

[0071] Preparation of core-sheath composite fibers

[0072] Example 1

[0073] The preparation method of core-sheath composite fiber includes steps B1-B3.

[0074] Step B1: The copolyester formed by copolymerizing sodium isophthalate sulfonate (SIPA) with PET is blended with a light rare earth element complex, and the content of the light rare earth element complex is controlled at 0.8 wt%. After twin-screw extrusion granulation, the skin-modified material is obtained. The blending temperature is 270℃, the screw speed is 300 rpm, and the residence time is 2 min.

[0075] Step B2: PET, 0.5wt% nano montmorillonite, 1.5wt% PET-g-MAH, and 0.15wt% flowability improver are blended at a blending temperature of 270℃, a screw speed of 300rpm, and a residence time of 2min. The mixture is then granulated using a twin-screw extruder to obtain the core layer modified material.

[0076] Step B3: Control the weight ratio of the modified sheath material to the modified core material to be 8:92, the spinning temperature to be 280℃, the draw ratio to be 4.0, and the heat setting temperature to be 190℃ to carry out composite spinning and obtain the sheath-core composite fiber.

[0077] Example 2

[0078] The core-sheath composite fiber was prepared using the same method as in Example 1, except that: the amount of nano-montmorillonite was 0.3wt%, the amount of PET-g-MAH was 1.0wt%, the amount of flow agent was 0.1wt%, the content of light rare earth element complex was 0.5wt%, and the weight ratio of sheath to core was 5:95.

[0079] Example 3

[0080] The core-sheath composite fiber was prepared using the same method as in Example 1, except that: the amount of nano-montmorillonite was 0.8 wt%, the amount of PET-g-MAH was 2.0 wt%, the amount of flow agent was 0.2 wt%, the content of light rare earth element complex was 1.0 wt%, and the weight ratio of sheath to core was 10:90.

[0081] Example 4

[0082] The core-sheath composite fiber was prepared using the same method as in Example 1, except that: the amount of nano-montmorillonite was 0.6 wt%, the amount of PET-g-MAH was 1.5 wt%, the amount of flow agent was 0.15 wt%, the content of light rare earth element complex was 0.8 wt%, and the weight ratio of sheath to core was 8:92.

[0083] Comparative Example 1

[0084] The core-sheath composite fiber was prepared using the same method as in Example 1, except that it was a conventional PET fiber.

[0085] Comparative Example 2

[0086] The core-sheath composite fiber was prepared using the same method as in Example 1, except that only nano-montmorillonite modified PET was used, without a sheath layer.

[0087] Comparative Example 3

[0088] The core-sheath composite fiber was prepared using the same method as in Example 1, except that only light rare earth element modified PET fiber was used, without a core layer.

[0089] Preparation of reinforced tire base

[0090] The above-mentioned core-sheath composite fibers are woven into polyester geotextile (150 g / m²). 2 The geotextile is used as the upper and lower layers, and the HDPE membrane (0.5mm thick) is used as the middle layer. The reinforced base layer with a two-layer geotextile and one-layer membrane structure is made by thermal bonding.

[0091] Preparation of modified bitumen coating

[0092] The components for preparing the modified asphalt coating are shown in Table 4.

[0093] Table 4. Components of Modified Asphalt Coating

[0094]

[0095] Note: 70# petroleum asphalt and 200# petroleum asphalt constitute the asphalt matrix. Other components are added in proportion to the mass of the asphalt matrix.

[0096] Method for preparing modified asphalt coating: Heat 70# petroleum asphalt and 200# petroleum asphalt to 170-180℃, add SBS, SBR, IPP and APAO in sequence, stir for 3 hours, add 800 mesh stone powder and 800 mesh montmorillonite inorganic filler, and stir for 1.5 hours.

[0097] Preparation of seepage-proof board

[0098] The modified asphalt coating material was heated to 180±5℃ and applied to the upper and lower surfaces of the reinforced base course (upper surface 2.2kg / m²). 2 The lower surface has a capacity of 1.8 kg / m². 2 The upper surface is covered with sintered sand (10-40 mesh), and the lower surface is bonded with a conventional PE isolation film (0.05-0.15mm thick). The film is removed before construction, and the modified asphalt layer on the lower surface is directly heat-fused to the concrete base. After cooling, rolling, and cutting, the impermeable board is obtained.

[0099] Example and Comparative Test Results

[0100] The performance test results of the impermeable boards in the embodiments and comparative examples of this application are shown in Tables 5-10.

[0101] Table 5. Mechanical property test results of embodiments and comparative examples of this application

[0102]

[0103] Table 6. Test results of seepage prevention performance of the embodiments and comparative examples of this application

[0104]

[0105] Table 7. Joint performance test results of embodiments and comparative examples of this application

[0106]

[0107] Table 8. Test results of interfacial adhesion performance of embodiments and comparative examples of this application

[0108]

[0109] Table 9. Long-term environmental aging performance test results of the embodiments and comparative examples of this application

[0110]

[0111] Table 10. Test results of thermal performance and durability of the embodiments and comparative examples of this application.

[0112]

[0113] According to the test results in Tables 5-10 above, firstly, in terms of mechanical properties: the maximum peak tensile force of Example 1 is 1500 N / 50 mm, which is 76% higher than that of Comparative Example 1, 53% higher than that of Comparative Example 2, and 58% higher than that of Comparative Example 3.

[0114] Secondly, in terms of seepage prevention performance: no leakage under static water pressure of 2.15MPa and constant pressure of 2.0MPa for 30 days, water pressure cycle fatigue retention rate of 95%, and fatigue resistance retention rate of 90%.

[0115] Third, regarding joint performance: the joint peel strength is 2.8 N / mm. According to GB / T 328.20-2007, the overlap width is 100 mm, the peeling speed is 50 mm / min, and the technical requirements refer to GB / T 18242-2025 (≥1.5 N / mm). The test results are 87% higher than the requirements of GB / T 18242-2025 (≥1.5 N / mm).

[0116] Fourth, regarding interfacial adhesion: the initial shear strength is 0.52 MPa, which is 160% higher than that of Comparative Example 1; the peel strength from concrete is 1.8 N / mm.

[0117] Fifth, regarding wet-dry cycles and freeze-thaw cycles: the retention rate was 91% after 500 wet-dry cycles and 92% after 200 freeze-thaw cycles.

[0118] Sixth, regarding asphalt overflow and water pressure stratification: no overflow at 80℃ for 168 hours, and no stratification at 1.5MPa for 72 hours.

[0119] In summary, the light rare earth elements in the core-sheath composite fiber of this application form coordination chemical bonds with asphalt, significantly enhancing the cross-linking between asphalt and the reinforced base course, effectively preventing asphalt separation and spillage. Through nano-montmorillonite reinforcement and the anti-aging properties of the light rare earth elements, it achieves properties such as crack resistance, aging resistance, water immersion resistance, and resistance to alternating wet and dry conditions. The reinforced base course prepared from the above-mentioned core-sheath fiber is then used to manufacture a geomembrane. Tests show that the geomembrane has a maximum peak tensile strength of 1500 N / 50 mm, a hydrostatic pressure of 2.15 MPa, no leakage after 30 days of constant pressure at 2.0 MPa, a water pressure cycle fatigue retention rate of 95%, an anti-fatigue retention rate of 90%, a joint peel strength of 2.8 N / mm, a retention rate of 91% after 500 cycles of alternating wet and dry conditions, a retention rate of 92% after 200 freeze-thaw cycles, and no cracks after bending at -35℃. The core-sheath composite fiber, reinforced base layer, and impermeable board of this application are specially designed for harsh environments such as high water pressure, high frequency of water level changes, long-term water immersion, alternating wet and dry conditions, and freeze-thaw cycles in pumped storage power stations.

[0120] The specific embodiments described above further illustrate the purpose, technical solution, and beneficial effects of this application. It should be understood that the above descriptions are merely specific embodiments of this application and are not intended to limit this application. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the protection scope of this application.

Claims

1. A core-sheath composite fiber, characterized in that, include: The product comprises a skin layer and a core layer, wherein the skin layer is a light rare earth element modified copolyester, the copolyester being a copolymer of sodium isophthalate sulfonate and polyester, and the core layer comprising nano-montmorillonite modified polyester.

2. The core-sheath composite fiber according to claim 1, characterized in that, The weight ratio of the cortex to the core is 5-10:95-90.

3. The core-sheath composite fiber according to claim 1, characterized in that, Based on the aforementioned copolyester, the amount of light rare earth element complex added is 0.5-1.0 wt%; Based on the polyester, the amount of nano-montmorillonite added is 0.3-0.8 wt%, and the interlayer spacing of the nano-montmorillonite is ≥3.0 nm.

4. The core-sheath composite fiber according to any one of claims 1-3, characterized in that, The core layer also includes: 1.0-2.0 wt% compatibilizer, wherein the compatibilizer is selected from polyester-grafted maleic anhydride.

5. The core-sheath composite fiber according to claim 4, characterized in that, The core layer also includes: 0.1-0.2 wt% flowability improver, wherein the flowability improver is selected from at least one of organic complex rheology modifiers, hyperbranched polymers, dendritic polymer flow lubricants.

6. The core-sheath composite fiber according to claim 5, characterized in that, The light rare earth element serves as a coordination center, forming coordination bonds with polar groups in the asphalt and with ester groups in the skin layer, thereby achieving chemical bonding between the asphalt and the skin-core composite fiber.

7. A method for preparing core-sheath composite fibers as described in any one of claims 1-6, characterized in that, include: The light rare earth element complex and copolyester are fed into a twin-screw extruder for melt mixing, and then extruded and granulated to obtain the skin-modified material. Polyester and nano-montmorillonite are fed into a twin-screw extruder for melt mixing, and then extruded and granulated to obtain the core layer modified material; The modified sheath material and the modified core material are fed into the sheath-core composite spinning assembly, and after extrusion, stretching, and heat setting, the sheath-core composite fiber is obtained.

8. The method according to claim 7, characterized in that, In the process of preparing the core layer modified material, a compatibilizer and / or a flowability improver are also added to the twin-screw extruder.

9. A reinforced tire base layer, characterized in that, Made from the core-sheath composite fiber as described in any one of claims 1-6.