A method for preparing antistatic high-strength polyester fiber containing biocrystal powder for sofa fabric.

By introducing ionic polyether ester and polyamide 6 into polyester fibers, combined with surface-modified dehydrated biocrystal powder and sodium montmorillonite, a "flexible bridging-layer fixation" structure is formed, which solves the problem of antistatic phase isolation caused by reinforcement treatment and realizes the preparation of antistatic high-strength polyester fibers suitable for sofa fabrics.

CN123108778APending Publication Date: 2026-11-17SHANDONG WOLENE NEW MATERIAL TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611611612.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-19
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

How to suppress the encapsulation and isolation of the ionic polyether ester antistatic phase in polyester fibers during reinforcement treatment, maintain their internal connectivity, and at the same time take into account the high-temperature processing stability of biocrystal powder, the spinnability and mechanical strength of the fibers, so as to obtain antistatic high-strength functional polyester fibers suitable for sofa fabrics.

Method used

By introducing ionic polyether ester and polyamide 6 into polyester fibers, combined with surface-modified dehydrated biocrystal powder and sodium montmorillonite, a "flexible bridging-layer fixation" structure is formed, which improves the interfacial bonding strength and charge conduction pathway. Two-stage stretching and tension heat setting technology are used to ensure a balance between antistatic properties and mechanical properties.

Benefits of technology

It achieves the maintenance of continuous charge conduction pathways within the fiber, improving the fiber's breaking strength and dimensional stability, while maintaining good charge dissipation capability and far-infrared function, making it suitable for sofa fabrics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108778A_ABST
    Figure CN123108778A_ABST
Patent Text Reader

Abstract

This invention discloses an antistatic high-strength polyester fiber containing biocrystal powder for sofa fabrics and its preparation method, belonging to the field of polyester fiber technology and patent classification number D01F6 / 92. The invention involves transesterification, pre-condensation, and reduced-compression polymerization of dimethyl terephthalate, sodium isophthalate 5-sulfonate, and ethylene glycol to obtain an ionic polyether ester antistatic copolyester. Fluorite powder, selenite powder, and red jasper powder are mixed and ground, then subjected to tetraethyl orthosilicate hydrolysis and condensation, progressively heated vacuum dehydration, and silane surface treatment to obtain modified dehydrated biocrystal powder. This powder is then reacted and extruded with polyethylene terephthalate and pyromellitic dianhydride to obtain reinforced polyester chips. The reinforced polyester chips, antistatic copolyester, and bridging masterbatch are mixed and melt-spun to obtain the final product. The fiber of this invention possesses both excellent antistatic properties and high tensile strength, meeting the durability requirements of sofa fabrics.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of polyester fiber technology, belonging to patent classification number D01F6 / 92, specifically to an antistatic high-strength polyester fiber containing biocrystal powder for sofa fabric and its preparation method. Background Technology

[0002] Sofa fabrics are constantly subjected to human contact, friction, and pressure during use, especially in indoor environments with low humidity, where static electricity easily accumulates on the fiber surface. Polyester fibers are suitable for sofa fabrics due to their high strength, good abrasion resistance, dimensional stability, and ease of cleaning. However, their relatively compact molecular structure, fewer hydrophilic groups, and low moisture absorption make it difficult for the charge generated by friction to be conducted away promptly. Static electricity buildup not only easily attracts dust to the fabric but can also cause momentary discharges and discomfort upon contact. Therefore, it is necessary to endow polyester fibers with stable and long-lasting charge dissipation capabilities.

[0003] Biocrystalline powder, composed of fluorite powder, selenite powder, and red jasper powder in equal quantities, possesses the unique far-infrared emission characteristics of mineral materials, with a relatively stable radiation frequency. In product functional design, the matching relationship between this radiation characteristic and the human body's thermal radiation band can be utilized to provide a material basis for reducing muscle tension, relaxing breathing, releasing stress, and improving sleep. However, the interfacial properties between these three mineral powders and polyester differ significantly. Reducing the powder particle size increases surface energy, making agglomeration more likely. Furthermore, selenite contains water of crystallization, which dehydrates at polyester melt processing temperatures. If untreated biocrystalline powder is directly added to the polyester melt, the released water may cause hydrolysis of the polyester molecular chains, and agglomerated particles may lead to increased spinning filtration pressure, increased internal fiber defects, and decreased breaking strength. Therefore, the biocrystalline powder needs to undergo refinement, graded dehydration, and interfacial stabilization treatment before entering the polyester melt system.

[0004] Introducing ionic polyether esters containing sodium sulfonate groups and polyethylene glycol segments into the polyester system can improve the fiber's adsorption capacity for trace amounts of moisture and create charge dissipation channels through ion migration. Simultaneously, to counteract the adverse effects of mineral powders on the fiber's mechanical properties, it is necessary to improve the effective entanglement of the polyester molecular chains and the interfacial bonding strength between the polyester and the mineral powders. However, after reinforcement treatment, the polyester matrix's melt elasticity and interfacial constraint increase, making the ionic polyether ester phase prone to shrinkage or encapsulation during melt flow and stretching. The originally interconnected antistatic phase is thus transformed into separated micro-regions. Even if the amount of antistatic component added remains constant, the continuous ion conduction pathways within the fiber may still be disrupted, leading to increased strength but decreased antistatic performance.

[0005] Therefore, the core technical problem that this invention needs to solve is how to suppress the encapsulation and isolation effect of the reinforced polyester matrix on the ionic polyether ester antistatic phase during the reinforcement treatment of polyester fibers containing biocrystal powder, so that the antistatic phase can remain effectively connected inside the fiber, while taking into account the high-temperature processing stability of biocrystal powder, the spinnability and mechanical strength of the fiber, so as to obtain antistatic high-strength functional polyester fibers suitable for sofa fabrics. Summary of the Invention

[0006] The purpose of this invention is to provide an antistatic high-strength polyester fiber containing biocrystal powder for sofa fabric and its preparation method, so as to solve the technical problems mentioned in the background art.

[0007] To achieve the above objectives, the present invention provides the following technical solution: A method for preparing antistatic high-strength polyester fiber containing biocrystal powder for sofa fabric includes the following steps: S1. Dimethyl terephthalate, sodium 5-sulfonate dimethyl isophthalate, and ethylene glycol undergo transesterification in the presence of tetraisopropyl titanate. During the reaction, methanol generated is removed and ethylene glycol is refluxed. Polyethylene glycol 1000, polyethylene glycol 4000, and trimethylolpropane are added, and pre-condensation and compression reduction polymerization are carried out sequentially to obtain an ionic polyether ester antistatic copolyester. S2. Fluorite powder, gypsum powder, and red jasper powder are mixed and ground finely according to the original feed mass ratio of 1:1:1. The resulting mixed powder is hydrolyzed and condensed using tetraethyl orthosilicate, then dehydrated under vacuum with progressively increasing temperature, and then surface-treated with γ-(2,3-epoxypropoxy)propyltrimethoxysilane to obtain surface-modified dehydrated biocrystal powder. The surface-modified dehydrated biocrystal powder, polyethylene terephthalate, and pyromellitic dianhydride are reacted and extruded to obtain reinforced polyester chips. S3. Polyamide 6 and sodium montmorillonite are melt-blended to obtain bridging masterbatch; S4. The reinforced polyester chips, ionic polyether ester antistatic copolyester and bridging masterbatch are dried and then mixed. The mixture is then melt-spun, two-stage drawing, tension heat setting and controlled relaxation to obtain the antistatic high-strength polyester fiber. The composition comprises, based on an initial feed amount of 100 parts by weight of polyethylene terephthalate, ionic polyether ester antistatic copolyester, surface-modified dehydrated biocrystal powder, pyromellitic dianhydride, polyamide 6, and sodium montmorillonite used to prepare the final spinning composition, wherein the ionic polyether ester antistatic copolyester comprises 14-18 parts by weight, the surface-modified dehydrated biocrystal powder comprises 1.0-2.0 parts by weight, the pyromellitic dianhydride comprises 0.08-0.12 parts by weight, the polyamide 6 comprises 1.5-2.5 parts by weight, the sodium montmorillonite comprises 0.15-0.25 parts by weight, and the polyethylene terephthalate comprises the remainder.

[0008] Preferably, the amounts of polyethylene terephthalate, ionic polyether ester antistatic copolyester, surface-modified dehydrated biocrystal powder, pyromellitic dianhydride, polyamide 6, and sodium montmorillonite are 80.20 parts by weight, 16.00 parts by weight, 1.50 parts by weight, 0.10 parts by weight, 2.00 parts by weight, and 0.20 parts by weight, respectively; the mixing mass ratio of reinforced polyester chips, ionic polyether ester antistatic copolyester, and bridging masterbatch calculated from the amounts of the above-mentioned amounts is 81.80:16.00:2.20.

[0009] Preferably, based on a total amount of 1.00 mol of dimethyl terephthalate and sodium isophthalate 5-sulfonate, the amounts of dimethyl terephthalate, sodium isophthalate 5-sulfonate, ethylene glycol, polyethylene glycol 1000, polyethylene glycol 4000, and trimethylolpropane are 0.95 mol, 0.05 mol, 1.50 mol, 0.050 mol, 0.0125 mol, and 0.0008–0.0010 mol, respectively; the amount of tetraisopropyl titanate is 8–12 mg / kg, calculated based on the mass content of titanium relative to the theoretically generated ionic polyether ester antistatic copolyester.

[0010] Preferably, step S1 includes: under nitrogen protection, mixing dimethyl terephthalate, sodium isophthalate 5-sulfonate, ethylene glycol, and tetraisopropyl titanate, reacting at 200°C for 70 min, then raising the temperature to 210°C to continue the reaction, continuously removing methanol and refluxing ethylene glycol until the cumulative amount of methanol distilled off is not less than 90% of the theoretical amount; adding pre-dried polyethylene glycol 1000, polyethylene glycol 4000, and trimethylolpropane, pre-condensing at 230–240°C for 25–30 min until the cumulative amount of methanol distilled off is not less than 95% of the theoretical amount; gradually reducing the absolute pressure of the reaction system to no more than 50 Pa within 25–35 min, and then compressing and condensing at 245–250°C for 90–120 min.

[0011] Preferably, the particle size D50 of the mixed powder after grinding and refining in step S2 is 0.4-0.8 μm, D90 is not greater than 1.5 μm, and D99 is not greater than 3.0 μm. Based on 100 parts by weight of the mixed powder, 3.0 parts by weight of tetraethyl orthosilicate, 12 parts by weight of anhydrous ethanol, 1.2 parts by weight of water, and 0.15 parts by weight of ammonia water with a mass fraction of 25% are prepared into a treatment solution. The treatment solution is sprayed onto the mixed powder in a tumbling state and treated at 40±2℃ for 60 min. Then, the ethanol is removed at 80℃, and the powder is vacuum treated at 110℃ for 1 h, heated to 180℃ for 1 h, and then treated at 240±5℃ and an absolute pressure not exceeding 10 kPa for 2 h. Finally, the powder is cooled under dry nitrogen protection to obtain dehydrated biocrystal powder.

[0012] Preferably, based on 100 parts by weight of the dehydrated biocrystal powder, 1.00 parts by weight of γ-(2,3-epoxypropoxy)propyltrimethoxysilane, 8.0 parts by weight of anhydrous ethanol, 0.23 parts by weight of water, and 0.02 parts by weight of glacial acetic acid are mixed and pre-hydrolyzed at 25°C for 20 min to obtain a silane treatment solution. Under nitrogen protection, the silane treatment solution is sprayed onto the dehydrated biocrystal powder at 60°C in a dynamic mixing state, mixed for 20 min, and kept at that temperature for 30 min. Then, it is dried at 130°C and an absolute pressure not exceeding 10 kPa for 4 h to obtain surface-modified dehydrated biocrystal powder.

[0013] Preferably, the reactive extrusion in step S2 is carried out using a twin-screw extruder, wherein the temperatures of each temperature zone of the twin-screw extruder are 245℃, 260℃, 270℃, 275℃, 278℃, 275℃ and 270℃ respectively, the screw speed is 180~220r / min, the material residence time is 60~90s, and the absolute pressure of the vacuum exhaust port is not higher than 10kPa.

[0014] Preferably, in step S3, the mass ratio of polyamide 6 to sodium montmorillonite is 10:1, the particle size D90 of the sodium montmorillonite agglomerates is not greater than 1.0 μm, the melt blending temperature is 235–245 °C, the screw speed is 220–260 r / min, and the material residence time is 60–90 s.

[0015] Preferably, step S4 includes: drying the reinforced polyester chips at 145–150°C for 6 hours, drying the ionic polyether ester antistatic copolyester at 75°C for 12 hours, and drying the bridging masterbatch at 80°C for 12 hours, so that the total moisture content of the mixture entering the spinning equipment is not higher than 80 mg / kg; the maximum temperature of the spinning melt during melt spinning is 272–278°C, the residence time of the melt in the equipment is 60–90 s, and the melt is filtered using a melt filter with a filtration accuracy of 15–25 μm; the resulting nascent fiber is first drawn at 85°C with a first stage of 2.7–2.9 times, then drawn at 125°C with a second stage of 1.30–1.40 times, with a total draw ratio of 3.6–4.0 times, and then subjected to tension heat setting at 155°C for 15–30 s, with the relaxation rate controlled at 1%–2%.

[0016] A sofa fabric made of antistatic high-strength polyester fiber containing biocrystal powder is prepared by the method described above.

[0017] Compared with the prior art, the beneficial effects of the present invention are: 1. Regarding antistatic properties, the sodium sulfonate groups in the ionic polyether ester provide relatively stable ionic interaction sites, while the polyethylene glycol segments possess certain hygroscopic capacity and good segment mobility. They can utilize the trace amounts of moisture adsorbed by the fiber to promote ion migration, allowing the charge generated by friction to gradually diffuse from the local high-potential region to the surrounding area. The shorter molecular chains of polyethylene glycol 1000 result in a more uniform distribution within the copolyester, which is beneficial for increasing the number of hydrophilic sites. The longer flexible segments of polyethylene glycol 4000 can expand the effective connection range between adjacent ionic microregions. The combination of these two polyethylene glycols with different chain lengths ensures that the antistatic component does not easily form excessively large soft phase regions, while simultaneously forming relatively continuous charge conduction pathways within the fiber. This antistatic component exists within the fiber in copolyester form, independent of any migratory coating on the fiber surface, thus maintaining good charge dissipation capabilities even after friction, cleaning, and long-term use.

[0018] 2. In terms of mechanical properties, after particle size control, the number of large particles and hard agglomerates in the biocrystal powder is significantly reduced, which can lower the risk of cracking due to local stress concentration during fiber drawing. The siliceous transition layer formed by tetraethyl orthosilicate treatment can improve the differences in surface properties of different mineral particles, and the subsequent silane surface treatment further reduces the interfacial repulsion between inorganic powder and polyester melt, making the biocrystal powder more uniformly dispersed in polyester. The staged dehydration treatment removes the water of crystallization contained in the gypsum, which can reduce the polyester viscosity reduction, bubbles, and internal voids in the fiber caused by water release during high-temperature spinning. The reinforced polyester obtained by reactive extrusion has high melt strength and molecular chain entanglement. The uniformly dispersed mineral particles can transfer load through a stable interface and reduce stress concentration around the particles. Combined with two-stage drawing and tension heat setting, the polyester molecular chains are fully oriented along the fiber axis and form a more stable crystalline structure, thereby improving the fiber's breaking strength and dimensional stability, and providing a structural basis for the stable performance of the far-infrared function of the biocrystal powder.

[0019] 3. With improved melt elasticity and interfacial constraint of the reinforced polyester, the rheological differences between the ionic polyether ester and the reinforced polyester become more pronounced. During melt mixing and drawing, the antistatic phase, originally distributed in a slender morphology, is prone to shrinkage and aggregation, and is encapsulated by the reinforced polyester matrix into mutually separated micro-regions. This leads to increased fiber strength but also the disruption of internal ion conduction pathways. While increasing the amount of ionic polyether ester alone can partially compensate for antistatic properties, it easily reduces fiber strength and spinning stability. To resolve this performance conflict, this solution pre-melt blends fiber-grade polyamide 6 and sodium-based montmorillonite at a mass ratio of 10:1, adding both as bridging components involved in the fiber phase structure construction. Polyamide 6 contains polar amide groups, exhibiting good affinity for the polar surfaces of polyester matrices, ionic polyether esters, and sodium montmorillonite. This improves the wetting state between different polymer phases, reduces interfacial tension, and refines the antistatic phase in the melt, stretching it along the spinning direction. However, when used alone, polyamide 6's flexible phase may still retract during shearing and stretching processes, making it difficult to maintain the elongated morphology of the antistatic phase in the long term. Sodium montmorillonite has a high aspect ratio layered structure. During premixing with polyamide 6, polyamide 6 can wet the surface of sodium montmorillonite and penetrate some of the interlamellar gaps, promoting the dispersion of montmorillonite in thinner lamellar units and preventing the formation of hard agglomerates after direct addition to polyester. The dispersed montmorillonite lamellars can also spatially constrain the polyamide 6 segments and form physical anchoring points at the polymer phase interface, limiting the retraction and aggregation of the antistatic phase. Thus, polyamide 6 plays a flexible wetting and interphase bonding role, while sodium montmorillonite plays a rigid support and interface anchoring role. The two form a synergistic structure of "flexible bridging and lamellar fixation", which enables the refined antistatic phase to maintain a high degree of mutual overlap in the reinforced polyester matrix. While maintaining load transfer and fiber strength, it restores a continuous charge dissipation path, thereby solving the technical problem of the antistatic phase being isolated and the antistatic performance decreasing due to the reinforcement treatment. Attached Figure Description

[0020] Figure 1 This is a SEM image of the antistatic high-strength polyester fiber prepared in Example 1 of the present invention. Detailed Implementation

[0021] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0022] In the following examples, polyethylene terephthalate and polyamide 6 were both fiber-grade products; sodium 5-sulfonate dimethyl isophthalate was anhydrous; anhydrous ethylene glycol had a purity of not less than 99.80%, anhydrous ethanol had a purity of not less than 99.70%, and tetraethyl orthosilicate, γ-(2,3-epoxypropoxy)propyltrimethoxysilane, and pyromellitic dianhydride all had a purity of not less than 98.00%. All vacuum levels were expressed as absolute pressure. Particle size was determined by laser diffraction, using anhydrous ethanol as the dispersion medium, and tested after ultrasonic dispersion for 5 minutes; the moisture content of the material was determined by Karl Fischer method.

[0023] Under dry nitrogen protection, 0.10 g of tetraisopropyl titanate (based on purity) was added to 9.90 g of anhydrous ethylene glycol and mixed thoroughly to prepare a 1.00% tetraisopropyl titanate ethylene glycol solution, which was used on the same day it was prepared.

[0024] Example 1

[0025] A method for preparing antistatic high-strength polyester fiber containing biocrystal powder for sofa fabric includes the following steps: (1) Preparation of ionic polyether ester antistatic copolyester 138.36 g of dimethyl terephthalate, 11.11 g of anhydrous sodium 5-sulfonate dimethyl isophthalate, 68.79 g of anhydrous ethylene glycol, and 1.05 g of a 1.00% (w / w) tetraisopropyl titanate ethylene glycol solution were added to a 1 L polymerization reactor equipped with mechanical stirring, an ethylene glycol reflux fractionation column, a methanol receiver, and a vacuum system. The catalyst solution contained 1.04 g of ethylene glycol, the total ethylene glycol feed was 69.83 g, and the titanium element dosage was 8.00 mg / kg based on the theoretical copolyester mass.

[0026] Dry nitrogen gas with a purity of not less than 99.99% was introduced at a flow rate of 0.20 L / min, and the mixture was stirred and heated to 200 °C for 70 min. The temperature was then raised to 210 °C to continue the transesterification process. Ethylene glycol was refluxed through a fractionating column and methanol was collected. The ethylene glycol in the distillate was determined by gas chromatography and the amount of methanol in the distillate was subtracted. After a total of 43.25 g of methanol was distilled off, 37.50 g of polyethylene glycol 1000, 37.50 g of polyethylene glycol 4000, and 0.08 g of trimethylolpropane, which had been dried for 4 h at 80 °C and an absolute pressure not exceeding 10 kPa, were added.

[0027] The reaction temperature was adjusted to 230℃, and pre-polymerization was carried out for 30 minutes until a total of 45.66g of methanol was distilled off. The absolute pressure was gradually reduced to 30Pa over 35 minutes, and decompression polymerization was carried out at 245℃ for 120 minutes. Dry nitrogen was introduced to release the vacuum, and the product was discharged, cooled, and pelletized to obtain ionic polyether ester antistatic copolyester.

[0028] (2) Preparation of surface-modified dehydrated biocrystal powder 40.00g of fluorite powder, 40.00g of selenite powder, and 40.00g of red jasper powder were mixed in an initial mass ratio of 1:1:1. The mixed powder was loaded into a zirconia-lined planetary ball mill jar, and 600.00g of zirconia balls with a diameter of 3.00mm were added. Dry ball milling was carried out at 300r / min, with a 10min stop and sample taken every 1 hour of ball milling. After ball milling until the D50 of the mixed powder was 0.40μm, D90 was 1.20μm, and D99 was 2.50μm, the zirconia balls were separated.

[0029] 3.60 g of tetraethyl orthosilicate was mixed with 14.40 g of anhydrous ethanol to obtain the first liquid; 1.44 g of deionized water was mixed with 0.18 g of 25.00% ammonia solution to obtain the second liquid. The second liquid was added to the first liquid, stirred for 5 min, and then immediately sprayed onto the mixed powder in a tumbling state. The mixture was then further tumbling at 38 °C for 60 min.

[0030] Ethanol was removed at 80℃, and then the mixture was treated sequentially at 110℃ for 1 h, 180℃ for 1 h, and 235℃ for 2 h under an absolute pressure of 10 kPa. The mixture was then cooled under dry nitrogen protection to obtain dehydrated biocrystal powder.

[0031] Weigh 100.00 g of dehydrated biocrystal powder. Mix 1.00 g of γ-(2,3-epoxypropoxy)propyltrimethoxysilane, 8.00 g of anhydrous ethanol, 0.23 g of deionized water and 0.02 g of glacial acetic acid, and pre-hydrolyze at 25 °C for 20 min. Under dry nitrogen protection, spray the resulting silane treatment solution onto the dehydrated biocrystal powder at 60 °C in a dynamic mixing state, mix for 20 min and keep at this temperature for 30 min, then dry at 130 °C and 10 kPa for 4 h to obtain surface-modified dehydrated biocrystal powder.

[0032] (3) Preparation of reinforced polyester chips To account for material loss at the beginning and end of the extrusion, the feed was set at 1.20 times the final required composition of reinforced polyester chips. 999.24g of fiber-grade polyethylene terephthalate chips were vacuum-dried at 150℃ for 6 hours, 12.00g of surface-modified dehydrated biocrystal powder was vacuum-dried at 130℃ for 4 hours, and 0.96g of pyromellitic dianhydride was vacuum-dried at 100℃ for 3 hours.

[0033] 50.00g of the polyethylene terephthalate (PET) chips were taken and mixed with 0.96g of pyromellitic dianhydride, then mixed with the remaining PET chips and 12.00g of surface-modified dehydrated biocrystal powder. Reactive extrusion was performed using a co-rotating twin-screw extruder with a diameter of 20mm and an aspect ratio of 40:1. The temperatures in each zone were 245℃, 260℃, 270℃, 275℃, 278℃, 275℃, and 270℃, respectively. The screw speed was 180r / min, the average residence time was 90s, and the absolute pressure at the vacuum exhaust port was 10kPa. The material from the stabilized extrusion section was cooled, pelletized, and dried at 145℃ for 6 hours. 843.50g of reinforced polyester chips were weighed for later use.

[0034] (4) Preparation of bridging masterbatch 60.00 g of fiber-grade polyamide 6 was vacuum-dried at 80 °C for 12 h, and 6.00 g of sodium montmorillonite was vacuum-dried at 110 °C for 4 h. The particle size D90 of the sodium montmorillonite agglomerates after air-flow depolymerization was 0.80 μm. The two materials were dry-mixed for 10 min and then added to a laboratory micro twin-screw mixer. The mixture was melt-blended at 235 °C and 220 r / min for 90 s, cooled, pelletized, and then dried at 80 °C for 12 h. 16.50 g of bridging masterbatch was weighed out for later use.

[0035] (5) Melt spinning and post-processing The obtained ionic polyether ester antistatic copolyester was dried at 75℃ for 12 hours, and 140.00g of ionic polyether ester antistatic copolyester, 843.50g of reinforced polyester chips, and 16.50g of bridging masterbatch were weighed. The total of the three materials was 1000.00g, and the corresponding main raw material composition was 832.70g of polyethylene terephthalate, 140.00g of ionic polyether ester antistatic copolyester, 10.00g of surface-modified dehydrated biocrystal powder, 0.80g of pyromellitic dianhydride, 15.00g of polyamide 6, and 1.50g of sodium montmorillonite.

[0036] The three materials were mixed for 10 minutes, and the total moisture content was confirmed to be no higher than 80 mg / kg by the Karl Fischer method before being fed into a laboratory melt spinning machine. A single-screw extruder with a diameter of 12 mm and a 24-hole spinneret with an orifice diameter of 0.30 mm were used. The melt flow rate per orifice was 0.50 g / min, the side-blown air temperature was 22℃, the air velocity was 0.40 m / s, and the initial filament winding speed was 800 m / min. The highest temperature of the spinning melt was 272℃, the average residence time was 90 s, and the melt filtration accuracy was 25 μm.

[0037] The nascent fibers were stretched to 2.70 times at 85℃ and then stretched to 1.40 times at 125℃, for a total stretching ratio of 3.78 times. Subsequently, they were subjected to tension heat setting at 155℃ for 15 seconds, with the relaxation rate controlled at 1.00%, to obtain antistatic high-strength polyester fibers containing biocrystal powder.

[0038] Example 2

[0039] A method for preparing antistatic high-strength polyester fiber containing biocrystal powder for sofa fabric includes the following steps: (1) Preparation of ionic polyether ester antistatic copolyester 138.36 g of dimethyl terephthalate, 11.11 g of anhydrous sodium 5-sulfonate dimethyl isophthalate, 68.53 g of anhydrous ethylene glycol, and 1.31 g of a 1.00% (w / w) tetraisopropyl titanate ethylene glycol solution were added to the 1 L polymerization reactor. The catalyst solution contained 1.30 g of ethylene glycol, and the total amount of ethylene glycol added was 69.83 g. The amount of titanium used was 10.00 mg / kg based on the theoretical copolyester mass.

[0040] Under dry nitrogen protection, the mixture was heated to 200℃ and reacted for 70 min, then heated to 210℃ to reflux the ethylene glycol while continuously collecting methanol. After a cumulative methanol distillation of 43.25 g, 37.50 g of pre-dried polyethylene glycol 1000, 37.50 g of polyethylene glycol 4000, and 0.09 g of trimethylolpropane were added, and pre-polymerization was carried out at 235℃ for 28 min until a cumulative methanol distillation of 45.66 g was achieved. The absolute pressure was gradually reduced to 40 Pa over 30 min, and decompression polymerization was carried out at 248℃ for 105 min. Dry nitrogen was introduced to release the vacuum, and the mixture was discharged, cooled, and pelletized to obtain an ionic polyether ester antistatic copolyester.

[0041] (2) Preparation of surface-modified dehydrated biocrystal powder Mix 40.00g of fluorite powder, 40.00g of selenite powder and 40.00g of red jasper powder, and process them by ball milling according to Example 1 until D50 is 0.60μm, D90 is 1.35μm and D99 is 2.80μm.

[0042] The treatment solution was prepared by mixing 3.60 g of tetraethyl orthosilicate, 14.40 g of anhydrous ethanol, 1.44 g of deionized water, and 0.18 g of ammonia solution with a mass fraction of 25.00% according to the solution preparation order in Example 1. This solution was then sprayed onto the tumbling mixed powder within 5 minutes and treated at 40°C for 60 minutes. The ethanol was removed at 80°C, and the powder was then treated sequentially at 110°C for 1 hour, 180°C for 1 hour, and 240°C for 2 hours under an absolute pressure of 8 kPa, followed by cooling under dry nitrogen protection.

[0043] Weigh 100.00g of the obtained dehydrated biocrystal powder, mix 1.00g of γ-(2,3-epoxypropoxy)propyltrimethoxysilane, 8.00g of anhydrous ethanol, 0.23g of deionized water and 0.02g of glacial acetic acid, and pre-hydrolyze at 25℃ for 20min; spray the obtained silane treatment solution onto the dehydrated biocrystal powder at 60℃, dynamically mix under dry nitrogen protection for 20min and keep warm for 30min, and then dry at 130℃ and 8kPa absolute pressure for 4h to obtain surface-modified dehydrated biocrystal powder.

[0044] (3) Preparation of reinforced polyester chips 962.40g of fiber-grade polyethylene terephthalate (PET) chips were vacuum-dried at 150℃ for 6 hours. 18.00g of surface-modified dehydrated biocrystal powder was vacuum-dried at 130℃ for 4 hours. 1.20g of pyromellitic dianhydride was vacuum-dried at 100℃ for 3 hours. First, 1.20g of pyromellitic dianhydride was mixed with 50.00g of chips taken from the PET chips. Then, the remaining chips and 18.00g of surface-modified dehydrated biocrystal powder were added and mixed thoroughly.

[0045] Reactive extrusion was performed using the twin-screw extruder described in Example 1. The temperatures in each zone were 245℃, 260℃, 270℃, 275℃, 278℃, 275℃, and 270℃, respectively. The screw speed was 200 r / min, the average residence time was 75 s, and the absolute pressure at the vacuum exhaust port was 8 kPa. The material from the stabilized extrusion section was cooled, pelletized, and dried at 148℃ for 6 hours. 818.00 g of reinforced polyester chips were weighed out for later use.

[0046] (4) Preparation of bridging masterbatch 60.00 g of fiber-grade polyamide 6 was vacuum-dried at 80 °C for 12 h, and 6.00 g of sodium montmorillonite with an aggregate particle size D90 of 0.90 μm was vacuum-dried at 110 °C for 4 h. The two materials were dry-mixed for 10 min, then melt-blended at 240 °C and 240 r / min for 75 s, cooled, pelletized, and dried at 80 °C for 12 h. 22.00 g of bridging masterbatch was weighed out for later use.

[0047] (5) Melt spinning and post-processing Ionic polyether ester antistatic copolyester was dried at 75℃ for 12 hours, and 160.00g of ionic polyether ester antistatic copolyester was weighed; 818.00g of reinforced polyester chips and 22.00g of bridging masterbatch were also weighed. The total of the three materials was 1000.00g, and the corresponding main raw material composition was 802.00g polyethylene terephthalate, 160.00g ionic polyether ester antistatic copolyester, 15.00g surface-modified dehydrated biocrystal powder, 1.00g pyromellitic dianhydride, 20.00g polyamide 6 and 2.00g sodium montmorillonite.

[0048] The total moisture content of the mixture was controlled to be no higher than 80 mg / kg, and spinning was performed using the melt spinning equipment described in Example 1. The maximum temperature of the spinning melt was 275°C, the average residence time was 75 s, and the melt filtration accuracy was 20 μm. The spinneret, melt flow rate, side blowing conditions, and nascent filament winding speed were the same as in Example 1.

[0049] The nascent fibers were stretched 2.77 times at 85℃ and then stretched 1.30 times at 125℃, for a total stretching ratio of 3.60 times. Subsequently, they were subjected to tension heat setting at 155℃ for 22 seconds, with the relaxation rate controlled at 1.50%, to obtain antistatic high-strength polyester fibers containing biocrystal powder.

[0050] Example 3

[0051] A method for preparing antistatic high-strength polyester fiber containing biocrystal powder for sofa fabric includes the following steps: (1) Preparation of ionic polyether ester antistatic copolyester 138.36 g of dimethyl terephthalate, 11.11 g of anhydrous sodium 5-sulfonate dimethyl isophthalate, 68.28 g of anhydrous ethylene glycol, and 1.57 g of a 1.00% (w / w) tetraisopropyl titanate ethylene glycol solution were added to the 1 L polymerization reactor. The catalyst solution contained 1.55 g of ethylene glycol, the total ethylene glycol feed was 69.83 g, and the titanium element dosage was 12.00 mg / kg based on the theoretical copolyester mass.

[0052] Under dry nitrogen protection, the mixture was heated to 200℃ and reacted for 70 min, then heated to 210℃ to reflux the ethylene glycol while continuously collecting methanol. After a cumulative methanol distillation of 43.25 g, 37.50 g of pre-dried polyethylene glycol 1000, 37.50 g of polyethylene glycol 4000, and 0.10 g of trimethylolpropane were added, and pre-polymerization was carried out at 240℃ for 25 min until a cumulative methanol distillation of 45.66 g was achieved. The absolute pressure was gradually reduced to 50 Pa over 25 min, and decompression polymerization was carried out at 250℃ for 90 min. Dry nitrogen was introduced to release the vacuum, and the mixture was discharged, cooled, and pelletized to obtain an ionic polyether ester antistatic copolyester.

[0053] (2) Preparation of surface-modified dehydrated biocrystal powder Mix 40.00g of fluorite powder, 40.00g of selenite powder and 40.00g of red jasper powder, and process them by ball milling according to Example 1 until D50 is 0.80μm, D90 is 1.50μm and D99 is 3.00μm.

[0054] The treatment solution was prepared by mixing 3.60 g of tetraethyl orthosilicate, 14.40 g of anhydrous ethanol, 1.44 g of deionized water, and 0.18 g of ammonia solution with a mass fraction of 25.00% according to the solution preparation order in Example 1. This solution was then sprayed onto the tumbling mixed powder within 5 minutes and treated at 42°C for 60 minutes. The ethanol was removed at 80°C, and the powder was then treated sequentially at 110°C for 1 hour, 180°C for 1 hour, and 245°C for 2 hours under an absolute pressure of 6 kPa, followed by cooling under dry nitrogen protection.

[0055] Weigh 100.00g of the obtained dehydrated biocrystal powder, mix 1.00g of γ-(2,3-epoxypropoxy)propyltrimethoxysilane, 8.00g of anhydrous ethanol, 0.23g of deionized water and 0.02g of glacial acetic acid, and pre-hydrolyze at 25℃ for 20min; spray the obtained silane treatment solution onto the dehydrated biocrystal powder at 60℃, dynamically mix under dry nitrogen protection for 20min and keep warm for 30min, and then dry at 130℃ and 6kPa absolute pressure for 4h to obtain surface-modified dehydrated biocrystal powder.

[0056] (3) Preparation of reinforced polyester chips 925.56g of fiber-grade polyethylene terephthalate (PET) chips were vacuum-dried at 150℃ for 6 hours. 24.00g of surface-modified dehydrated biocrystal powder was vacuum-dried at 130℃ for 4 hours. 1.44g of pyromellitic dianhydride was vacuum-dried at 100℃ for 3 hours. First, 1.44g of pyromellitic dianhydride was mixed with 50.00g of chips taken from the PET chips. Then, the remaining chips and 24.00g of surface-modified dehydrated biocrystal powder were added and mixed thoroughly.

[0057] Reactive extrusion was performed using the twin-screw extruder described in Example 1. The temperatures in each zone were 245℃, 260℃, 270℃, 275℃, 278℃, 275℃, and 270℃, respectively. The screw speed was 220 r / min, the average residence time was 60 s, and the absolute pressure at the vacuum exhaust port was 6 kPa. The material from the stabilized extrusion section was cooled, pelletized, and dried at 150℃ for 6 hours. 792.50 g of reinforced polyester chips were weighed out for later use.

[0058] (4) Preparation of bridging masterbatch 60.00 g of fiber-grade polyamide 6 was vacuum-dried at 80 °C for 12 h, and 6.00 g of sodium montmorillonite with an aggregate particle size D90 of 1.00 μm was vacuum-dried at 110 °C for 4 h. The two materials were dry-mixed for 10 min, then melt-blended at 245 °C and 260 r / min for 60 s, cooled, pelletized, and dried at 80 °C for 12 h. 27.50 g of bridging masterbatch was weighed out for later use.

[0059] (5) Melt spinning and post-processing Ionic polyether ester antistatic copolyester was dried at 75℃ for 12 hours, and 180.00g of ionic polyether ester antistatic copolyester was weighed; 792.50g of reinforced polyester chips and 27.50g of bridging masterbatch were also weighed. The total of the three materials was 1000.00g, and the corresponding main raw material composition was 771.30g polyethylene terephthalate, 180.00g ionic polyether ester antistatic copolyester, 20.00g surface-modified dehydrated biocrystal powder, 1.20g pyromellitic dianhydride, 25.00g polyamide 6 and 2.50g sodium montmorillonite.

[0060] The total moisture content of the mixture was controlled to be no higher than 80 mg / kg, and spinning was performed using the melt spinning equipment described in Example 1. The highest temperature of the spinning melt was 278°C, the average residence time was 60 s, and the melt filtration accuracy was 15 μm. The spinneret, melt flow rate, side blowing conditions, and nascent filament winding speed were the same as in Example 1.

[0061] The nascent fibers were first stretched at 85℃ for 2.90 times, and then stretched at 125℃ for 1.37 times, for a total stretching ratio of 3.97 times. Subsequently, they were subjected to tension heat setting at 155℃ for 30 seconds, and the relaxation rate was controlled at 2.00% to obtain antistatic high-strength polyester fibers containing biocrystal powder.

[0062] Comparative Example 1: Compared with Example 1, only 140.00g of ionic polyether ester antistatic copolyester was replaced with 140.00g of fiber-grade polyethylene terephthalate chips. All other raw materials, amounts and preparation conditions were the same as in Example 1.

[0063] Comparative Example 2: Compared with Example 1, only 10.00g of surface-modified dehydrated biocrystal powder was replaced with 10.00g of biocrystal powder composed of fluorite powder, selenite powder and red jasper powder in the original feed mass ratio of 1:1:1 and with the same particle size, but without tetraethyl orthosilicate treatment, graded dehydration and KH-560 surface treatment. All other conditions were the same as in Example 1.

[0064] Comparative Example 3: Compared with Example 1, 0.80g of pyromellitic dianhydride was not added during the preparation of the reinforced polyester chips, and 0.80g of fiber-grade polyethylene terephthalate chips were used as an equal substitute. The remaining raw materials, amounts and preparation conditions were the same as in Example 1.

[0065] Comparative Example 4: Compared with Example 1, 16.50g of bridging masterbatch consisting of 15.00g of fiber-grade polyamide 6 and 1.50g of sodium montmorillonite was not added, and 16.50g of fiber-grade polyethylene terephthalate chips were used as an equal substitute. All other raw materials, amounts and preparation conditions were the same as in Example 1.

[0066] Comparative Example 5: Compared with Example 1, only 15.00g of fiber-grade polyamide 6 was retained without adding 1.50g of sodium montmorillonite, and 1.50g of fiber-grade polyethylene terephthalate chips were used as an equal substitute. The polyamide 6 was dried and then directly mixed with the reinforced polyester chips and the antistatic copolyester. All other conditions were the same as in Example 1.

[0067] Comparative Example 6: Compared with Example 1, only 1.50g of sodium montmorillonite was retained instead of 15.00g of fiber-grade polyamide 6, and 15.00g of fiber-grade polyethylene terephthalate chips were used as an equal substitute. The sodium montmorillonite was directly added to the final spinning composition after drying and airflow depolymerization. All other conditions were the same as in Example 1.

[0068] Comparative Example 7: Compared with Example 1, 15.00g of fiber-grade polyamide 6 and 1.50g of sodium montmorillonite were dried and directly added to the final spinning composition. The two were not pre-melted and blended to prepare bridging masterbatch. The other raw materials, dosages and preparation conditions were the same as in Example 1.

[0069] Performance testing 1.1 Sample Conditioning and Parallel Test Setup For each group of filaments, equal samples were taken from no fewer than three rolls, with 100m of the surface filament removed from each roll. Unless otherwise specified, all samples were conditioned for 24 hours in standard atmosphere at (20±2)℃ and (65±4)% relative humidity. The filaments used for electrostatic half-life testing were fabricated into plain knitted fabric using the same equipment and process parameters, with a surface density controlled at (180±5) g / m². 2 The samples were not subjected to antistatic finishing; the filaments used for far-infrared testing were directly combed into uniform, fluffy fiber samples. Random samples were taken for each test, and the results in the table are the arithmetic mean of the specified number of parallel determinations.

[0070] 1.2 Fracture strength and elongation at break The tensile properties of chemical fiber filaments were tested using an electronic single-yarn tensile tester with constant-speed elongation, in accordance with GB / T 14344—2022 "Test Method for Tensile Properties of Chemical Fiber Filaments". Each conditioned filament was clamped individually at a distance of (500±1) mm, with a pre-tension of (0.05±0.005) cN / dtex and a tensile speed of 500 mm / min, continuously stretched until the specimen broke. Specimens that broke or slipped at the clamping point were discarded, and 20 valid values ​​were obtained for each group. The breaking strength was calculated based on the breaking load and the measured linear density, and the breaking elongation was recorded simultaneously. The arithmetic mean of the 20 valid values ​​was taken as the test result.

[0071] 1.3 Volume resistivity The volume resistivity of synthetic fiber filaments was determined according to FZ / T 50035—2016 "Test Method for Resistance of Synthetic Fiber Filaments". To eliminate the influence of spinning oil, each group of filaments was first treated in a neutral soap solution at (72±2)℃ for 60 min at a bath ratio of not less than 1:25, then washed twice with grade III water at (82±2)℃ for 5 min each time, air-dried naturally, then dried at 50℃ for 30 min, and finally conditioned at (20±2)℃ and (35±5)% relative humidity for 2 h. Three sections of sample were cut from each roll, spaced several meters apart. The filaments were straightened and fixed in copper clamps with a clamping distance of (100±1) mm. Conductive adhesive was applied to the contact area between the clamping surface and the sample. A DC voltage of (100±5) V was applied, and the resistance R was read after 60 s. v =R×D×10 -6 / (L×ρ f Calculate the volume resistivity, where D is the measured linear density in dtex, L is the clamping distance in cm, and ρ is the volume resistivity. f At 1.38 g / cm 3 Calculation: The arithmetic mean of 9 valid measurements for each group is taken, and the unit is Ω·cm.

[0072] 1.4 Static Voltage Half-Life The electrostatic properties of textiles were tested according to GB / T 12703.1—2021, "Test Methods for Electrostatic Properties of Textiles—Part 1: Corona Charging Method". Five 45mm × 45mm samples were cut from each group of weft-knitted fabrics and conditioned for 24 hours at (20±2)℃, (40±4)% relative humidity, and an air velocity not exceeding 0.1m / s. The samples were then fixed on a rotating platform with a rotation speed not less than 1000r / min. The distance between the discharge needle tip and the sample surface was set to 20mm, and the distance between the induction electrode and the sample surface was set to 15mm. Corona charging was performed at -10kV for 30s. After the high voltage was cut off, the time required for the peak induced electrostatic voltage to decay to half its value was recorded. The arithmetic mean of the measured values ​​from the five samples was taken as the electrostatic voltage half-life.

[0073] 1.5 Far-infrared emissivity and far-infrared radiation temperature rise The far-infrared emissivity was determined according to GB / T 30127—2013 "Testing and Evaluation of Far-Infrared Properties of Textiles", with three parallel samples set up for each group. When determining the far-infrared emissivity, 0.50g of loose fiber was weighed and evenly filled into an open cylindrical metal sample dish with an inner diameter of 60mm and a height of 30mm, ensuring the sample surface was flat and not additionally compacted. The test hot plate was stabilized at (34.0±0.1)℃, and the far-infrared radiation intensity was calibrated using a standard blackbody plate with an emissivity of not less than 0.95. After the reading stabilized within the detection band of 5μm to 14μm, the far-infrared radiation intensity of the sample was measured, and the emissivity was calculated. When measuring the temperature rise of far-infrared radiation, the fibers were combed into uniform flakes approximately 30 mm thick and greater than 60 mm in diameter. The sample surface was kept 500 mm away from a far-infrared external source with a dominant wavelength of 5 μm to 14 μm and a radiation power of 150 W. The temperature sensor was fixed at the center of the irradiated surface, and the initial temperature T0 and the surface temperature T1 after 30 seconds of irradiation were recorded. T1-T0 was taken as the temperature rise value. Both indicators were taken as the arithmetic mean of three parallel measurements. The fiber sample test results are only used as a basis for raw material selection and inter-group comparison, and are not used to determine physiological or medical efficacy.

[0074] 1.6 Boiling water shrinkage rate The heat shrinkage rate of chemical fiber filaments was determined according to the twisting method in GB / T 6505—2017 "Test Method for Heat Shrinkage Rate of Chemical Fiber Filaments (After Treatment)". The filaments were twisted according to the number of sampling turns specified in the standard. The twisted filaments were conditioned for 4 hours at (20±2)℃ and (65±5)% relative humidity in a standard atmosphere. After being loaded with the pre-tension specified in the standard for (30±3) seconds, the length L0 before treatment was measured. The twisted filaments were then completely immersed in Grade III water conforming to GB / T 6682 in a relaxed state and boiled continuously for 30 minutes. After dripping for 10 minutes, the filaments were placed in an oven at (55±5)℃ for approximately 60 minutes to dry. They were then conditioned for 4 hours in the same standard atmosphere and the length L1 after treatment was measured under the same pre-tension. The boiling water shrinkage rate was calculated as (L0-L1) / L0×100%. Three parallel samples were measured for each group, and the arithmetic mean was taken.

[0075] Table 1:

[0076] Table 1 shows that the breaking strengths of Examples 1, 2, and 3 were 4.68 cN / dtex, 4.86 cN / dtex, and 4.75 cN / dtex, respectively, all maintaining a high level for functional polyester filaments. Example 2 simultaneously achieved a breaking strength of 4.86 cN / dtex and an elongation at break of 26.20%, indicating that under moderate amounts of functional components, a good balance was achieved in interfacial load transfer, molecular chain orientation, and stretchability. In Example 3, after further increasing the content of antistatic copolyester and biocrystal powder, the strength decreased slightly compared to Example 2, but was still higher than that of Example 1. In Comparative Example 1, the strength increased to 4.91 cN / dtex after supplementing the antistatic copolyester with PET, but the antistatic properties were not maintained, indicating that an increase in individual strength cannot replace comprehensive performance. The fracture strength and elongation at break of Comparative Example 2 decreased to 3.42 cN / dtex and 14.90%, respectively, indicating that undehydrated and untreated powders are prone to uneven dispersion and local stress concentration. The strength of Comparative Example 3 decreased to 4.16 cN / dtex after removing pyromellitic dianhydride, reflecting a decrease in the degree of molecular chain connection and interfacial stress transfer ability.

[0077] The volume resistivity and electrostatic voltage half-life of Example 1 are 7.60 × 10⁻⁶. 8 The Ω·cm and 0.84s values ​​decreased further in Example 3 to 1.40 × 10⁻⁶ Ω·cm and 0.84s, respectively, with increasing antistatic copolyester content. 8 Ω·cm and 0.23s. Comparative Example 1, without the addition of antistatic copolyester, saw its two properties increase to 4.90 × 10⁻⁶. 12 The values ​​of Ω·cm and 118.70 s indicate that the ionic hydrophilic phase is the basis for rapid migration and charge dissipation. It is noteworthy that Comparative Example 3, after removing pyromellitic dianhydride, has a volume resistivity of 5.80 × 10⁻⁶. 8 With a half-life of 0.63 s and Ω·cm, the antistatic properties did not deteriorate, but the strength decreased significantly. This indicates that matrix reinforcement causes the antistatic phase to tend to shrink and separate during stretching, creating a contradiction between strength and conductivity pathways. Fiber-grade polyamide 6 can wet the interface between PET and the hydrophilic antistatic phase, forming a transition region with polarity and a certain degree of toughness. Sodium-based montmorillonite sheets provide multi-point physical anchoring within this transition region, limiting the shrinkage of polyamide 6 and the antistatic phase during stretching and cooling, and extending the continuous retention time of the interfacial charge transfer path. In Comparative Example 4, after removing both, the volume resistivity increased to 7.10 × 10⁻⁶. 9 Ω·cm; Comparative Example 5, with only polyamide 6 retained, lacked the effect of lamellar fixation; Comparative Example 6, with only sodium montmorillonite retained, was more prone to agglomeration due to the lack of wetting and dispersion of polyamide 6; Comparative Example 7, although both were added, was not pre-melted and blended, and its volume resistivity and half-life were still 5.20 × 10 Ω·cm; 9Ω·cm and 5.47s. The above differences indicate that the flexible interfacial bridging of polyamide 6 and the lamellar anchoring of sodium montmorillonite work together, and the stable structure is formed through pre-dispersion, which can alleviate the interruption of conductive pathways caused by matrix reinforcement.

[0078] The far-infrared emissivity of Examples 1 to 3 was 89.10%, 90.20%, and 91.30%, respectively, and the far-infrared temperature rise was 1.62℃, 1.91℃, and 2.18℃, respectively, steadily increasing with the increase of biocrystal powder addition. Other samples using the same amount of powder showed only slight fluctuations, indicating that the main influencing factors on the far-infrared indicators are the powder content and its dispersion state. Comparative Example 2 used powder without dehydration and surface treatment, and its emissivity and temperature rise were 88.10% and 1.44℃, respectively, lower than Example 1, indicating that uniform dispersion is beneficial to increasing the effective radiation area. The boiling water shrinkage rates of Examples 1 to 3 were 5.36%, 4.87%, and 4.31%, respectively, while those of Comparative Examples 2 and 3 increased to 7.62% and 6.18%, respectively. Combined with the mechanical data, it can be seen that after powder pretreatment, interface synergistic regulation, and matching stretching and heat setting, the fiber maintained good dimensional stability while obtaining antistatic and far-infrared properties.

[0079] Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art can still modify the technical solutions described in the foregoing embodiments or make equivalent substitutions for some of the technical features. Any modifications, equivalent substitutions, improvements, etc., made within the essence and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A method for preparing antistatic high-strength polyester fiber containing biocrystal powder for sofa fabric, characterized in that, Includes the following steps: S1. Dimethyl terephthalate, sodium 5-sulfonate dimethyl isophthalate, and ethylene glycol undergo transesterification in the presence of tetraisopropyl titanate. During the reaction, methanol generated is removed and ethylene glycol is refluxed. Polyethylene glycol 1000, polyethylene glycol 4000, and trimethylolpropane are added, and pre-condensation and compression reduction polymerization are carried out sequentially to obtain an ionic polyether ester antistatic copolyester. S2. Fluorite powder, gypsum powder, and red jasper powder are mixed and ground finely according to the original feed mass ratio of 1:1:

1. The resulting mixed powder is hydrolyzed and condensed using tetraethyl orthosilicate, then dehydrated under vacuum with progressively increasing temperature, and then surface-treated with γ-(2,3-epoxypropoxy)propyltrimethoxysilane to obtain surface-modified dehydrated biocrystal powder. The surface-modified dehydrated biocrystal powder, polyethylene terephthalate, and pyromellitic dianhydride are reacted and extruded to obtain reinforced polyester chips. S3. Polyamide 6 and sodium montmorillonite are melt-blended to obtain bridging masterbatch; S4. The reinforced polyester chips, ionic polyether ester antistatic copolyester and bridging masterbatch are dried and then mixed. The mixture is then melt-spun, two-stage drawing, tension heat setting and controlled relaxation to obtain the antistatic high-strength polyester fiber. The composition comprises, based on an initial feed amount of 100 parts by weight of polyethylene terephthalate, ionic polyether ester antistatic copolyester, surface-modified dehydrated biocrystal powder, pyromellitic dianhydride, polyamide 6, and sodium montmorillonite used to prepare the final spinning composition, wherein the ionic polyether ester antistatic copolyester comprises 14-18 parts by weight, the surface-modified dehydrated biocrystal powder comprises 1.0-2.0 parts by weight, the pyromellitic dianhydride comprises 0.08-0.12 parts by weight, the polyamide 6 comprises 1.5-2.5 parts by weight, the sodium montmorillonite comprises 0.15-0.25 parts by weight, and the polyethylene terephthalate comprises the remainder.

2. The preparation method according to claim 1, characterized in that, The feed amounts of polyethylene terephthalate, ionic polyether ester antistatic copolyester, surface-modified dehydrated biocrystal powder, pyromellitic dianhydride, polyamide 6, and sodium montmorillonite are 80.20 parts by weight, 16.00 parts by weight, 1.50 parts by weight, 0.10 parts by weight, 2.00 parts by weight, and 0.20 parts by weight, respectively. The mixing mass ratio of reinforced polyester chips, ionic polyether ester antistatic copolyester, and bridging masterbatch, calculated from the feed amounts, is 81.80:16.00:2.

20.

3. The preparation method according to claim 1, characterized in that, Based on a total amount of 1.00 mol of dimethyl terephthalate and sodium isophthalate 5-sulfonate, the amounts of dimethyl terephthalate, sodium isophthalate 5-sulfonate, ethylene glycol, polyethylene glycol 1000, polyethylene glycol 4000, and trimethylolpropane are 0.95 mol, 0.05 mol, 1.50 mol, 0.050 mol, 0.0125 mol, and 0.0008–0.0010 mol, respectively; the amount of tetraisopropyl titanate is 8–12 mg / kg, calculated based on the mass content of titanium relative to the theoretically generated ionic polyether ester antistatic copolyester.

4. The preparation method according to claim 3, characterized in that, Step S1 includes: under nitrogen protection, mixing dimethyl terephthalate, sodium isophthalate 5-sulfonate, ethylene glycol, and tetraisopropyl titanate, reacting at 200°C for 70 min, then raising the temperature to 210°C to continue the reaction, continuously removing methanol and refluxing ethylene glycol until the cumulative amount of methanol distilled off is not less than 90% of the theoretical amount; adding pre-dried polyethylene glycol 1000, polyethylene glycol 4000, and trimethylolpropane, pre-condensing at 230–240°C for 25–30 min until the cumulative amount of methanol distilled off is not less than 95% of the theoretical amount; gradually reducing the absolute pressure of the reaction system to no more than 50 Pa within 25–35 min, and then compressing and condensing at 245–250°C for 90–120 min.

5. The preparation method according to claim 1, characterized in that, In step S2, the particle size of the refined mixed powder is D50 of 0.4-0.8 μm, D90 of no more than 1.5 μm, and D99 of no more than 3.0 μm. Based on 100 parts by weight of the mixed powder, 3.0 parts by weight of tetraethyl orthosilicate, 12 parts by weight of anhydrous ethanol, 1.2 parts by weight of water, and 0.15 parts by weight of ammonia water with a mass fraction of 25% are prepared into a treatment solution. The treatment solution is sprayed onto the mixed powder in a tumbling state and treated at 40±2℃ for 60 min. Then, the ethanol is removed at 80℃, and the powder is vacuum treated at 110℃ for 1 h, heated to 180℃ for 1 h, and then treated at 240±5℃ and an absolute pressure of no more than 10 kPa for 2 h. Finally, the powder is cooled under dry nitrogen protection to obtain dehydrated biocrystal powder.

6. The preparation method according to claim 5, characterized in that, Based on 100 parts by weight of the dehydrated biocrystal powder, 1.00 parts by weight of γ-(2,3-epoxypropoxy)propyltrimethoxysilane, 8.0 parts by weight of anhydrous ethanol, 0.23 parts by weight of water and 0.02 parts by weight of glacial acetic acid were mixed and pre-hydrolyzed at 25°C for 20 min to obtain a silane treatment solution. Under nitrogen protection, the silane treatment solution was sprayed onto the dehydrated biocrystal powder at 60°C in a dynamic mixing state, mixed for 20 min and kept at that temperature for 30 min, and then dried at 130°C and an absolute pressure not exceeding 10 kPa for 4 h to obtain surface-modified dehydrated biocrystal powder.

7. The preparation method according to claim 1, characterized in that, The reactive extrusion in step S2 is carried out using a twin-screw extruder. The temperatures of each temperature zone of the twin-screw extruder are 245℃, 260℃, 270℃, 275℃, 278℃, 275℃ and 270℃ respectively. The screw speed is 180~220r / min, the material residence time is 60~90s, and the absolute pressure of the vacuum exhaust port is not higher than 10kPa.

8. The preparation method according to claim 1, characterized in that, In step S3, the mass ratio of polyamide 6 to sodium montmorillonite is 10:1, and the particle size D90 of the sodium montmorillonite agglomerates is not greater than 1.0 μm; the melt blending temperature is 235-245℃, the screw speed is 220-260 r / min, and the material residence time is 60-90 s.

9. The preparation method according to claim 1, characterized in that, Step S4 includes: drying reinforced polyester chips at 145–150°C for 6 hours, drying ionic polyether ester antistatic copolyester at 75°C for 12 hours, and drying bridging masterbatch at 80°C for 12 hours, so that the total moisture content of the mixture entering the spinning equipment is not higher than 80 mg / kg; the maximum temperature of the spinning melt during melt spinning is 272–278°C, the residence time of the melt in the equipment is 60–90 s, and the melt is filtered using a melt filter with a filtration accuracy of 15–25 μm; the resulting nascent fiber is first drawn at 85°C with a first stage of 2.7–2.9 times, then drawn at 125°C with a second stage of 1.30–1.40 times, with a total draw ratio of 3.6–4.0 times, and then subjected to tension heat setting at 155°C for 15–30 s, with the relaxation rate controlled at 1%–2%.

10. A sofa fabric made of antistatic high-strength polyester fiber containing biocrystal powder, characterized in that, It is prepared by the method described in any one of claims 1 to 9 above.