A lightweight tear-resistant fabric and its manufacturing process
By incorporating a grid structure in the fabric, combined with polyaryl filament and softener treatment, the problem of insufficient tear strength in lightweight fabrics is solved, achieving a balance between lightweight and tear resistance.
Patent Information
- Application Number
- CN202611388855.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-08
- Publication Date
- 2026-11-17
AI Technical Summary
Existing fabrics made of nylon fibers have difficulty maintaining stable warp tear strength to meet usage requirements after weight reduction.
The warp yarn A and weft yarn A form a grid body structure, and the warp yarn B and weft yarn B form a grid edge structure. The warp yarn B and weft yarn B are polyaramid filaments. The warp density and weft density are controlled through weaving, dyeing, softening and calendering steps. Softeners and penetrants are used to reduce the coefficient of friction between yarns. The calendering temperature is controlled at 100-110℃.
While reducing the fabric weight, tear resistance is also maintained, with improved warp tear strength, and it meets the requirements for outdoor clothing.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This invention relates to a lightweight tear-resistant fabric and its manufacturing process, belonging to the field of fabrics. Background Technology
[0002] Nylon fiber is widely used in outdoor clothing fabrics due to its excellent abrasion resistance, good elasticity and soft hand feel.
[0003] Lightweighting is an important development direction for outdoor clothing fabrics, but when the weight of existing fabrics using nylon fibers is reduced, the tear strength often decreases, especially the warp tear strength, which is difficult to consistently meet the usage requirements. Summary of the Invention
[0004] To address the shortcomings of existing technologies, the present invention aims to provide a lightweight tear-resistant fabric and its manufacturing process, in order to solve the problem that the tear strength of existing fabrics using nylon fibers often decreases as the basis weight is reduced, especially the warp tear strength, which is difficult to consistently meet the usage requirements.
[0005] To achieve the above objectives, the present invention is implemented through the following technical solution: a lightweight tear-resistant fabric, which is processed by weaving, dyeing, softening and calendering of warp and weft yarns; the warp yarns consist of warp yarn A and warp yarn B, which are arranged radially in a cyclic manner with one warp yarn B following every several consecutive warp yarns A; the weft yarns consist of weft yarn A and weft yarn B, which are arranged radially in a cyclic manner with one weft yarn B following every several consecutive weft yarns A; the interlacing area of warp yarn A and weft yarn A forms a grid structure, and the interlacing point of warp yarn B and weft yarn B forms a grid edge structure.
[0006] Furthermore, both the warp yarn A and the weft yarn A are nylon filaments.
[0007] Furthermore, both the warp yarn B and the weft yarn are polyaramid filaments.
[0008] A manufacturing process for a lightweight tear-resistant fabric includes the following steps: Step S1: Weave the warp and weft yarns to obtain the greige fabric; Step S2: Dye the greige fabric from step S1 to obtain dyed greige fabric; Step S3: Apply softener and penetrant to the dyed fabric from step S2 in the same bath to perform softening finishing. Step S4 involves calendering the dyed fabric after the softening process in step S3 to obtain a lightweight, tear-resistant fabric.
[0009] Furthermore, step S1 also includes controlling the warp density and weft density of the fabric, wherein the warp density is 165-175 threads / inch and the weft density is 155-170 threads / inch.
[0010] Furthermore, the dyeing in step S2 is specifically a conventional acid dyeing process for nylon fabric, with a dyeing temperature of 98-110℃.
[0011] Furthermore, step S2 also includes heat preservation and dye bath work for the dyed fabric, with a heat preservation time of 30-60 minutes and a dye bath pH value of 4-6.
[0012] Furthermore, the calendering temperature in step S4 is 100-110℃.
[0013] The beneficial effects of this invention are: by using polyarylate fiber filaments arranged in a spaced manner to form a lattice skeleton to provide limiting resistance, by using a lower warp and weft density to provide space for yarn slippage, by using a softener to reduce the coefficient of friction between yarns to promote slippage, and by using a synergistic matching of calendering temperature and softener dosage to avoid excessive compression of yarns, it is possible to achieve both lightweight and tear resistance under conditions of reduced fabric weight and no film layer or fluorinated finishing agent. Detailed Implementation
[0014] To make the technical means, creative features, objectives and effects of this invention easier to understand, the invention will be further described below in conjunction with specific embodiments.
[0015] This invention provides a lightweight tear-resistant fabric and its manufacturing process: The lightweight tear-resistant fabric is processed by weaving, dyeing, softening, and calendering warp and weft yarns; the warp yarns consist of warp A and warp B, arranged radially in a cyclic manner with one warp B following every several consecutive warp A yarns; the weft yarns consist of weft A and weft B, arranged radially in a cyclic manner with one weft B following every several consecutive weft A yarns; the interlacing areas of warp A and weft A form a grid structure, and the interlacing points of warp B and weft B form a grid edge structure; both warp A and weft A are nylon filaments; both warp B and weft B are polyaramid filaments.
[0016] Among them, polyarylate fiber has higher strength than conventional nylon fiber. The warp and weft yarns B are distributed in an alternating manner among the warp and weft yarns A to form a grid-like skeleton. When the fabric is subjected to tearing force, the warp and weft yarns A located at the tear first slip and gradually gather in the activity space provided by the low-density weaving to form a yarn cluster to resist the external force. When the slip displacement continues to increase and reaches the grid edge, the high-modulus polyarylate warp and weft yarns B, as a rigid skeleton, use their high strength characteristics to bear the final tear resistance and prevent the tear from expanding further. The breaking elongation of polyarylate fiber is much lower than that of conventional nylon, which is common knowledge. Its function is not to absorb stress through its own elongation, but to distribute the concentrated load to the surrounding multiple nylon yarns by limiting the excessive slippage of the nylon yarns, thereby reducing the breakage of a single nylon yarn due to stress concentration, and also preventing the polyarylate yarn from breaking directly without slip buffer.
[0017] A manufacturing process for a lightweight tear-resistant fabric includes the following steps: Step S1: Weave the warp and weft yarns to obtain the greige fabric, and control the warp density and weft density of the greige fabric, wherein the warp density is 165-175 threads / inch and the weft density is 155-170 threads / inch. Step S2: The greige fabric from step S1 is dyed using a conventional acid dyeing process for nylon fabrics to obtain dyed greige fabric. The dyeing temperature is 98-110℃, the holding time is 30-60min, and the pH value of the dye bath is 4-6. Step S3: Apply softener and penetrant to the dyed fabric from step S2 in the same bath to perform softening finishing. The softener is Depo Chemical's Finishing Softener 400 Concentrate, used at a concentration of 5–20 g / L; the penetrant is Depo Chemical's Penetrant JFC, used at a concentration of 2–5 g / L. The softener adheres to the yarn surface, reducing the coefficient of friction between yarns, making it easier for the yarns to slip when torn. The penetrant reduces the surface tension of the working fluid, helping the softener penetrate into the yarn, resulting in a more uniform finishing effect. If the amount of softener is too low, the coefficient of friction between yarns will still be relatively high, hindering slippage; if the amount is too high, the yarns will be too slippery, making it easy for the yarns to be pulled out of the fabric when torn, and the amount of seam slippage may exceed the requirements of garment processing.
[0018] Step S4 involves calendering the dyed fabric after the softening treatment in step S3 to obtain a lightweight, tear-resistant fabric. The calendering temperature is 100-110℃. Calendering makes the yarns on the fabric surface smoother, increases the contact area between the yarns, and improves the overall strength of the fabric. When the calendering temperature exceeds 110℃, the nylon yarn cross-section is crushed under the combined action of high temperature and roller pressure, and the contact area increases rapidly. Even if a softener is used to reduce the surface friction coefficient of the yarn, the physical slip space of the yarn will still be greatly compressed, causing the yarn to be unable to slip smoothly when tearing, and the tear strength will decrease accordingly. The calendering temperature of 110℃ is lower than the conventional temperature resistance limit of polyarylate fiber (180℃). Therefore, the effect of calendering on this fiber in this process can be ignored. However, this temperature is close to the critical range for significant thermoplastic deformation of 20D fine denier nylon yarn, so it should not be increased further.
[0019] Among them, the finished lightweight tear-resistant fabric has a warp density of 180-200 threads / inch, a weft density of 170-190 threads / inch, and a weight of ≤40g / ㎡. Example 1
[0020] For the sake of brevity, the parts that are the same as those in other embodiments will not be repeated. The main focus is on the structure that differs from other embodiments of the present invention. The warp yarns A and B are arranged radially in a cyclic pattern, with one warp yarn B following every eighteen consecutive warp yarns A. The weft yarns consist of weft yarns A and B, arranged radially in a cyclic pattern, with one weft yarn B following every seventeen consecutive weft yarns A. Both warp yarns A and weft yarns A are 20D nylon filaments, and both warp yarns B and weft yarns B are 25D polyaramid fiber filaments, wherein the mass percentage of 25D polyaramid fiber filaments is 3.0%. The warp density and weft density of the fabric obtained by weaving the warp and weft yarns are 165 threads / inch and 155 threads / inch, respectively. In the softening process, the amount of softener used is 5 g / L, and the amount of penetrant used is 2 g / L. In the calendering process, the calendering temperature is 100°C. Example 2
[0021] For the sake of brevity, the parts that are the same as those in other embodiments will not be repeated. The main focus is on the structure that differs from other embodiments of the present invention. The warp yarns A and B are arranged radially in a cyclic pattern, with one warp yarn B following every eighteen consecutive warp yarns A. The weft yarns consist of weft yarns A and B, arranged radially in a cyclic pattern, with one weft yarn B following every seventeen consecutive weft yarns A. Both warp yarns A and weft yarns A are 20D nylon filaments, and both warp yarns B and weft yarns B are 25D polyaramid fiber filaments, wherein the mass percentage of 25D polyaramid fiber filaments is 3.5%. The warp density and weft density of the fabric obtained by weaving the warp and weft yarns are 175 ends / inch and 170 ends / inch, respectively. In the softening process, the amount of softener used is 20 g / L, and the amount of penetrant used is 5 g / L. In the calendering process, the calendering temperature is 110°C.
[0022] Comparative Example 1 of Example 1 For the sake of brevity, the parts that are the same as those in other embodiments will not be described again. The main focus is on the structure that is different from other embodiments of the present invention. The warp yarns A and B are arranged in a radial loop, with one warp yarn B placed after every twenty consecutive warp yarns A. The weft yarns are composed of weft yarns A and weft yarns B, which are arranged in a radial loop, with one weft yarn B placed after every nineteen consecutive weft yarns A. The mass percentage of 25D polyaramid fiber filaments is 2.5%.
[0023] Comparative Example 2 of Example 1 For the sake of brevity, the parts that are the same as those in other embodiments will not be described again. The main focus here is on the structure that is different from other embodiments of the present invention, where the warp density and weft density of the fabric obtained by weaving the warp and weft yarns are 160 threads / inch and 150 threads / inch, respectively.
[0024] Comparative Example 3 of Example 1 For the sake of brevity, the parts that are the same as those in other embodiments will not be described again. The main focus here is on the structure that is different from other embodiments of the present invention, where the warp density and weft density of the fabric obtained by weaving the warp and weft yarns are 180 threads / inch and 170 threads / inch, respectively.
[0025] Comparative Example 4 of Example 1 For the sake of brevity, the parts that are the same as those in other embodiments will not be described again. The main focus here is on the structure that is different from other embodiments of the present invention. In the softening process, the amount of softener used is 25 g / L and the amount of penetrant used is 5 g / L.
[0026] Comparative Example 5 of Example 1 For the sake of brevity, the parts that are the same as those in other embodiments will not be described again. The main focus here is on the structure that is different from other embodiments of the present invention, in which the calendering temperature is 95°C during the calendering process.
[0027] Comparative Example 6 of Example 1 For the sake of brevity, the parts that are the same as those in other embodiments will not be described again. The main focus here is on the structure that is different from other embodiments of the present invention, in which the calendering temperature is 120°C during the calendering process.
[0028] Test methods for lightweight tear-resistant fabrics Cut the fabric into rectangles, make a cut of a specified length at the center of the short side to form a "tongue", clamp the two "tongues" into the upper and lower clamps of the constant speed elongation type electronic fabric strength tester, stretch the sample at a constant speed until it is completely torn, record the force value during the tearing process and calculate the average tear strength.
[0029] The effects of different polyaramid fiber filament contents on warp tear strength are shown in Table 1; the effects of different fabric warp densities on warp tear strength are shown in Table 2; the effects of different additive dosages on warp tear strength are shown in Table 3; and the effects of different calendering temperatures on warp tear strength are shown in Table 4. Given that down jackets, windbreakers, and other outdoor clothing are primarily stressed in the warp direction and secondarily in the weft direction during wear, warp tear strength is typically the weakest direction in terms of fabric strength. Therefore, Tables 1 to 4 use warp tear strength as a key evaluation indicator. In the tests of each embodiment, weft tear strength was also tested simultaneously, and the results were all no less than 90% of the corresponding warp tear strength. Furthermore, seam slippage and down-proof properties simultaneously met the requirements of this standard; therefore, weft data are not listed individually.
[0030] Table 1
[0031] As shown in Table 1, the mass percentage of polyaryl filament affects the density of the lattice skeleton. When the proportion of polyaryl filament is too low, the number of lattice edges is insufficient, and the nylon yarn lacks the limiting resistance provided by the LCP lattice edges after sliding into place. When the proportion of polyaryl filament is 3.0-3.5%, the lattice edge density is moderate, which can provide effective limiting resistance after the nylon yarn slides into place, without causing the hand feel to be too hard and the cost to increase due to too much polyaryl filament. Therefore, the preferred mass percentage of polyaryl filament in this invention is 3.0-3.5%.
[0032] Table 2
[0033] As shown in Table 2, with a polyarylate fiber filament mass ratio of 3.0-3.5%, the strength decreases when the warp density is below 165 threads / inch and also shows a decreasing trend when it is above 175 threads / inch. This indicates that there is an optimal balance between slip space and interlacing holding force. Therefore, this invention selects a warp density of 165-175 threads / inch and a weft density of 155-170 threads / inch for the fabric.
[0034] Table 3
[0035] As shown in Table 3, as the softener dosage increased from 5 g / L to 25 g / L, the warp tear strength continuously increased from 13.5 N to 17.0 N. This indicates that the softener's effect on reducing the coefficient of friction between yarns and promoting slippage increased with increasing dosage. Simultaneously, the seam slippage increased from 1.8 mm to 4.5 mm. According to the GB / T 13772.2-2018 standard method (100 N constant load method), and based on the standard requirements for conventional outdoor clothing fabrics in this field, the acceptable seam slippage criterion is ≤4 mm. With a softener dosage of 20 g / L, the seam slippage was 3.2 mm, and with 25 g / L, it reached 4.5 mm. Therefore, although the tear strength continuously increases with the softener dosage, the softener dosage cannot be increased indefinitely due to the acceptable seam slippage standard. A reasonable dosage range is 5-20 g / L, with a tear strength of 13.5-16.5 N and a seam slippage of 1.8-3.2 mm.
[0036] Table 4
[0037] As shown in Table 4, although the tear strength reaches 17.5N at a calendering temperature of 95℃, the down-proof performance is 18 threads, exceeding the acceptable standard of ≤15 threads. When the calendering temperature is increased to 100℃, the down-proof performance improves to 12 threads, while the warp tear strength remains at 16.8N. This demonstrates better process stability in balancing tear strength and down-proof performance. As the calendering temperature continues to rise to 110℃ and 120℃, the yarn cross-section gradually flattens under pressure, and the slippage space continues to narrow. The warp tear strength decreases from 16.8N to 16.4N and 15.3N respectively, with the rate of decrease gradually increasing. Although the down-proof performance decreases from 12 threads to 8 threads, the rate of decrease in tear strength gradually increases with increasing temperature. Considering both down-proof performance and tear strength maintenance, a calendering temperature of 100-110℃ is the optimal range.
[0038] The foregoing has shown and described the basic principles, main features, and advantages of the present invention. It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the invention can be implemented in other specific forms without departing from its spirit or essential characteristics. Therefore, the embodiments should be considered illustrative and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description. Thus, all variations falling within the meaning and scope of equivalents of the claims are intended to be included within the present invention. No reference numerals in the claims should be construed as limiting the scope of the claims.
[0039] Furthermore, it should be understood that although this specification describes embodiments, not every embodiment contains only one independent technical solution. This narrative style is merely for clarity. Those skilled in the art should consider the specification as a whole, and the technical solutions in each embodiment can also be appropriately combined to form other embodiments that can be understood by those skilled in the art.
Claims
1. A lightweight, tear-resistant fabric, characterized by: The fabric is processed by weaving, dyeing, softening and calendering the warp and weft yarns. The warp yarns consist of warp yarns A and warp yarns B, which are arranged radially in a circular manner, with one warp yarn B placed after every several consecutive warp yarns A. The weft yarn consists of weft yarn A and weft yarn B, which are arranged radially in a circular manner, with one weft yarn B placed after every several consecutive weft yarns A. The interlacing area of warp yarn A and weft yarn A forms a grid structure, and the interlacing point of warp yarn B and weft yarn B forms a grid edge structure.
2. The lightweight tear-resistant fabric of claim 1, wherein: Both warp yarn A and weft yarn A are nylon filaments.
3. The lightweight tear-resistant fabric of claim 1, wherein: Both the warp yarn B and the weft yarn are polyaramid filaments.
4. A process for producing the lightweight tear-resistant fabric according to claim 1, characterized by, Includes the following steps: Step S1: Weave the warp and weft yarns to obtain the greige fabric; Step S2: Dye the greige fabric from step S1 to obtain dyed greige fabric; Step S3: Apply softener and penetrant to the dyed fabric from step S2 in the same bath to perform softening finishing. Step S4 involves calendering the dyed fabric after the softening process in step S3 to obtain a lightweight, tear-resistant fabric.
5. The process for producing a lightweight tear-resistant fabric according to claim 4, characterized in that: Step S1 further includes controlling the warp density and weft density of the fabric, wherein the warp density is 165-175 threads / inch and the weft density is 155-170 threads / inch.
6. The process for producing a lightweight tear resistant fabric as claimed in claim 4, wherein: The dyeing process in step S2 is specifically a conventional acid dyeing process for nylon fabrics, with a dyeing temperature of 98-110℃.
7. The process for producing a lightweight tear-resistant fabric according to claim 6, characterized in that: Step S2 also includes heat preservation of the dyed fabric and dye bath operation, with heat preservation time of 30-60 minutes and dye bath pH value of 4-6.
8. The process for producing a lightweight tear resistant fabric as claimed in claim 4, wherein: The calendering temperature in step S4 is 100-110℃.