A rime-like structure of hydrogenated titanium oxide-coated porous carbon nanofiber composite material, its preparation method and application

By constructing a haze-like structure of hydrogenated titanium oxide coating on the surface of porous carbon nanofibers, the problems of high preparation temperature, simple loss mechanism and lack of dielectric control layer in electromagnetic wave absorption of existing silicon carbide-based and titanium dioxide-based nanofibers are solved, achieving lightweight and broadband electromagnetic wave absorption performance improvement.

CN123108927APending Publication Date: 2026-11-17SHAANXI UNIV OF SCI & TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611368507.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-04
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing silicon carbide-based and titanium dioxide-based nanofibers suffer from insufficient absorption performance in electromagnetic wave absorption applications due to their high preparation temperature, lack of porous structure, simple loss mechanism, and lack of structured dielectric control layer.

Method used

A hydrothermal self-assembly and Ar/H2 mixed atmosphere treatment method was used to construct a haze-like structure of hydrogenated titanium oxide coating on the surface of porous carbon nanofibers. The coating thickness of TiO2 nanosheets was precisely controlled by the glycerol confinement effect, which introduced abundant heterostructures and oxygen vacancies to enhance polarization loss.

Benefits of technology

It achieves lightweight and wide-band electromagnetic wave absorption performance improvement, covering Ku, X, C and S bands, and solves the problems of high preparation temperature, single loss mechanism and lack of dielectric control layer in existing technologies. It has good application flexibility and industrialization prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108927A_ABST
    Figure CN123108927A_ABST
Patent Text Reader

Abstract

This invention discloses a haze-like structure hydrogenated titanium oxide-coated porous carbon nanofiber composite material, its preparation method, and its application, belonging to the field of electromagnetic wave absorbing material preparation technology. The method includes: using porous carbon nanofibers as a structural template, TiO2-F127 single micelles as a precursor, and glycerol as a confinement solvent, constructing a haze-like structure TiO2 nanosheet coating layer on the surface of porous carbon nanofibers via a hydrothermal self-assembly process, followed by hydrogenation treatment to obtain the haze-like structure hydrogenated titanium oxide-coated porous carbon nanofiber composite material. The thickness of the hydrogenated titanium oxide coating layer is precisely controlled by the glycerol confinement effect, and oxygen vacancies and TiO2 nanosheets are introduced through hydrogenation treatment. 3+ The defects are transformed into a mixed anatase and rutile crystal phase, achieving multiple synergistic effects of dipole polarization, interface polarization, and conductivity loss. It exhibits strong broadband absorption performance in the X-band and Ku-band, and has low density and small filling ratio, showing broad application prospects in the field of electromagnetic wave absorption.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of electromagnetic wave absorbing material preparation technology, specifically relating to a hydrogenated titanium oxide-coated porous carbon nanofiber composite material with a rime-like structure, its preparation method, and its application. Background Technology

[0002] With the rapid development of modern electronic communication technology, the large-scale application of electromagnetic devices has brought about increasingly serious electromagnetic pollution problems, which not only affect the normal operation of electronic equipment but also pose a potential threat to human health. While electromagnetic shielding materials can provide some protection, they suffer from secondary pollution. In contrast, wave-absorbing materials can effectively dissipate electromagnetic wave energy by converting it into heat or other forms of energy, fundamentally avoiding electromagnetic wave hazards. One-dimensional carbon nanofibers, due to their high aspect ratio, low density, and anisotropy, show significant potential in enhancing conductivity and polarization losses. However, the inherent impedance mismatch problem of carbon materials and their excessively high dielectric constant lead to a large amount of electromagnetic wave reflection on the material surface, severely limiting their wave-absorbing performance. How to optimize impedance matching and enhance loss capacity while achieving lightweighting through reasonable component control and microstructure design has become a research hotspot in the field of electromagnetic wave absorbing materials.

[0003] To address the aforementioned issues, researchers have already conducted relevant explorations. For example, Chinese patent CN113737314B discloses a flexible SiC / C nanocomposite fiber and its preparation method. Using polysilane as the silicon carbide source, Mo-SiC / C composite nanofibers were prepared through electrospinning and high-temperature pyrolysis, and then applied to electromagnetic wave absorption. This patent introduces molybdenum acetylacetonate doping, generating uniformly dispersed Mo2C grains within the fiber. These grains synergistically interact with the SiC / C matrix, effectively broadening the effective absorption width of the composite fiber, achieving complete coverage of the Ku and X-bands at different thicknesses. However, in this technical solution, the formation of SiC requires high-temperature sintering at 1000~1300°C. The excessively high preparation temperature leads to complex processes and high energy consumption, limiting its application on flexible substrates. The prepared nanofibers are solid structures, lacking porous design, which is not conducive to achieving lightweight absorption and cannot utilize the multiple reflection and scattering mechanisms of the porous-air interface to enhance dissipation. The fiber surface is smooth, without a core-shell structure or structured coating layer, lacking abundant heterogeneous interfaces to provide sufficient interfacial polarization loss. Furthermore, Chinese patent CN112886013B discloses a method for preparing multi-level TiO2 / C nanofibers. Using tetrabutyl titanate as the titanium source and tetraethyl orthosilicate as the template agent, multi-level TiO2 / C nanofibers with a mixed crystalline phase of anatase and TiO2(B) are prepared through electrospinning and alkaline etching processes. This patent utilizes a one-dimensional structure to shorten the ion transport path and a mesoporous structure to increase the specific surface area, and is mainly applied to sodium-ion battery anode materials. However, this technical solution has significant limitations when applied to the field of electromagnetic wave absorption: the material contains only two components, TiO2 and carbon, and the loss mechanism is mainly conductive loss, lacking a multi-component synergistic polarization loss mechanism, making it difficult to achieve broadband strong absorption; TiO2 is distributed in the fiber in particulate form, without constructing a dielectric modulation layer with a specific morphology on the carbon fiber surface, making it impossible to effectively adjust impedance matching characteristics; calcination is carried out in a pure Ar atmosphere, without introducing a reducing atmosphere to hydrogenate TiO2, thus lacking oxygen vacancies and Ti... 3+ The enhanced dipole polarization effect caused by the defect limits the dielectric loss capability.

[0004] In summary, existing silicon carbide-based and titanium dioxide-based nanofibers are limited in electromagnetic wave absorption applications by problems such as excessively high preparation temperatures, lack of porous structures, simplistic loss mechanisms, and lack of structured dielectric control layers. How to construct a controllable dielectric coating layer on the surface of carbon nanofibers using a mild preparation process, while simultaneously introducing porous structures to achieve lightweighting and enhancing polarization loss through defect engineering, has become a key technical challenge that urgently needs to be overcome in this field. Summary of the Invention

[0005] In order to overcome the shortcomings of the prior art, the present invention aims to provide a haze-like structure hydrogenated titanium oxide-coated porous carbon nanofiber composite material, its preparation method and application, so as to solve the technical problems of high preparation temperature, simple loss mechanism, lack of structured dielectric control layer and poor low-frequency electromagnetic wave absorption performance of existing silicon carbide-based and titanium dioxide-based nanofiber microwave absorbing materials.

[0006] To achieve the above objectives, the present invention employs the following technical solution: This invention discloses a method for preparing a porous carbon nanofiber composite material with hydrogenated titanium oxide coated with a rime-like structure, comprising: Porous carbon nanofibers were dispersed in anhydrous ethanol and glycerol to obtain solution A; TiO2-F127 single micelles were dispersed in anhydrous ethanol to obtain solution B; Solution A and solution B were mixed and stirred, and then subjected to a hydrothermal reaction. After centrifugation and drying, TiO2-coated porous carbon nanofibers were obtained. TiO2-coated porous carbon nanofibers were calcined in a mixed atmosphere of Ar and H2 to obtain a rime-like structure of hydrogenated titanium oxide-coated porous carbon nanofiber composite material.

[0007] Preferably, in solution A, the ratio of porous carbon nanofibers, anhydrous ethanol and glycerol is 200 mg: 10 mL: (5~10) mL; in solution B, the ratio of TiO2-F127 single micelles to anhydrous ethanol is (1.0~2.0) g: 5 mL.

[0008] Preferably, solutions A and B are stirred for 0.5 to 1.0 h until homogeneous.

[0009] Preferably, the mixing and stirring time for solution A and solution B is 6 to 12 hours.

[0010] Preferably, the hydrothermal reaction temperature is 80~120°C and the time is 8~12h.

[0011] Preferably, the calcination process involves a heating rate of 2-4°C / min, a temperature of 600-800°C, and a time of 2-4 hours.

[0012] The present invention also discloses a rime-like structure hydrogenated titanium oxide coated porous carbon nanofiber composite material, which is prepared by the above-mentioned preparation method of the rime-like structure hydrogenated titanium oxide coated porous carbon nanofiber composite material.

[0013] Preferably, the frost-like structure is a frost-like morphology structure formed by uniformly coating TiO2 nanosheets onto the surface of porous carbon nanofibers, with the TiO2 nanosheets overlapping each other to form a continuous and dense coating layer.

[0014] Preferably, in the rime-like structure of hydrogenated titanium oxide-coated porous carbon nanofiber composite material, hydrogenated titanium oxide is uniformly coated on the surface of porous carbon nanofiber in the form of nanosheets, the thickness of the hydrogenated titanium oxide coating layer is controlled by the amount of glycerol added, and the hydrogenated titanium oxide is a mixed crystal phase of anatase and rutile.

[0015] The present invention also discloses the application of the above-mentioned haze-like structure hydrogenated titanium oxide coated porous carbon nanofiber composite material in low-frequency electromagnetic wave absorption.

[0016] Compared with the prior art, the present invention has the following beneficial effects: This invention discloses a method for preparing a hydrogenated titanium dioxide-coated porous carbon nanofiber composite material with a frost-like structure. Glycerol is used as a confining solvent, and its addition amount precisely controls the coating thickness of the TiO2 nanosheets. Figure 2 As shown, the coating thickness of TiO2 nanosheets gradually decreased with increasing glycerol addition from 5 mL to 10 mL. The most regular and uniformly coated frost-like structure was obtained when the glycerol addition was 7.5 mL. The hydrothermal self-assembly process enabled TiO2 nanosheets to uniformly coat the surface of porous carbon nanofibers in a frost-like morphology. The nanosheets overlapped to form a continuous and dense coating layer. This frost-like structure introduced abundant PC / TiO2 heterointerfaces, such as... Figure 3 As shown, the real and imaginary parts of the dielectric constant of the sample were significantly improved after hydrogenation treatment, confirming the enhancement of interfacial polarization loss; the calcination treatment in an Ar / H2 mixed atmosphere introduced oxygen vacancies and TiO2 atoms into the TiO2 lattice through hydrogenation. 3+ Defects simultaneously form a mixed anatase and rutile crystal phase. The generation of defect dipoles significantly enhances dipole polarization loss, thereby enabling the composite material to achieve broadband strong absorption in electromagnetic wave absorption performance, such as... Figure 4 As shown, the sample with 7.5 mL of added glycerol exhibits a significantly improved effective absorption width, completely covering the Ku and X bands, and achieving substantial coverage of the C and S bands at different thicknesses. The preparation method of this invention, through the synergistic effect of the glycerol confinement effect, the frost-like structured design, and hydrogenation treatment, solves the technical problems of excessively high preparation temperatures, a single loss mechanism, lack of a structured dielectric control layer, and poor low-frequency absorption performance in existing microwave absorbing materials.

[0017] This invention discloses a haze-like structure of hydrogenated titanium oxide-coated porous carbon nanofiber composite material. Through a glycerol-confined hydrothermal self-assembly and hydrogenation process, a unique haze-like core-shell structure is formed. The porous carbon nanofibers provide a conductive loss network and lightweight support for the core, while the hydrogenated titanium oxide nanosheets provide dielectric regulation and polarization loss functions for the outer shell. Figure 2As shown, TiO2 nanosheets with a frost-like structure are uniformly coated on the surface of porous carbon nanofibers, with a fiber diameter of approximately 500 nm and uniform size. The internal conductive network constructed by the interlacing of one-dimensional carbon nanofibers facilitates electron migration within the fibers and transitions between fibers, effectively enhancing conductivity loss. The porous structure not only reduces the effective dielectric constant of the material, thereby improving impedance matching, but also enhances the multiple reflections and scattering of electromagnetic waves through the porous-air interface. The frost-like structure of TiO2... 2-x Nanosheet coating provides PC / TiO 2-x Heterogeneous interfaces and anatase / rutile two-phase interfaces, combined with oxygen vacancies and Ti introduced by hydrogenation treatment. 3+ The defects were overcome, resulting in a significant enhancement of interface polarization and dipole polarization. For example... Figure 4 As shown, PC@TiO 2-x -7.5 nanofibers exhibit strong reflection loss and wide effective absorption bandwidth at different matching thicknesses, and can completely cover the Ku and X bands. At different thicknesses, they can achieve most of the coverage of the C and S bands, realizing strong broadband absorption from high frequency to low frequency. At the same time, the introduction of porous carbon fiber matrix reduces the material density and achieves lightweight absorption.

[0018] This invention discloses the application of a hydrogenated titanium oxide-coated porous carbon nanofiber composite material with a frost-like structure in low-frequency electromagnetic wave absorption. Based on the synergistic effect of the composite material's multi-level loss mechanism and structural advantages, traditional absorbing materials often struggle to achieve effective absorption in the low-frequency band (S-band and C-band) due to thickness limitations and impedance matching difficulties. However, this invention's composite material improves impedance matching by reducing the effective dielectric constant through porous carbon fibers, provides abundant heterogeneous interfaces to enhance interfacial polarization through a frost-like structure, and introduces oxygen vacancies and Ti atoms through hydrogenation treatment. 3+ The triple cooperative mechanism of defect-enhanced dipole polarization relaxation loss, such as Figure 4 As shown, the composite nanofibers with an added glycerol content of 7.5 mL exhibit a significantly enhanced effective absorption width, completely covering the Ku and X bands, and achieving substantial coverage of the C and S bands at varying thicknesses, successfully extending the absorption performance to the low-frequency S and C bands. Furthermore, this composite material, using porous carbon nanofibers as a matrix and incorporating a porous structure design, boasts advantages such as low density and low filler ratio, meeting the lightweight development requirements of modern microwave absorbing materials. Its preparation process is mild and controllable, allowing for precise adjustment of the coating layer thickness by regulating the glycerol addition amount to optimize absorption performance across different frequency bands. This demonstrates excellent application flexibility and industrialization prospects, providing a highly efficient low-frequency electromagnetic wave absorbing material solution for the fields of electromagnetic compatibility and electromagnetic protection. Attached Figure Description

[0019] Figure 1Here are SEM images (a) and TEM images (b) of the PC nanofibers disclosed in this invention. Figure 2 The PC@TiO3 with a frost-like structure prepared in Examples 1, 2 and 3 of this invention 2-x SEM images of nanofibers, where (a) is PC@TiO 2-x -5 nanofibers represent an addition of 5 mL of glycerol; (b) represents PC@TiO 2-x -7.5 nanofibers represent an addition of 7.5 mL of glycerol; (c) represents PC@TiO 2-x -10 nanofibers represent an addition of 10 mL of glycerin; Figure 3 PC@TiO2-7.5 nanofibers (a) and PC@TiO2 nanofibers prepared in Example 2 of this invention 2-x Plot of the real and imaginary parts of the dielectric constant of -7.5 nanofibers (b); Figure 4 PC@TiO prepared in Example 2 of this invention 2-x - 7.5 nanofibers as microwave absorbing materials: three-dimensional reflection loss diagram (a) and effective absorption bandwidth diagram (b) at different thicknesses. Detailed Implementation

[0020] The technical solution of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0021] Unless otherwise specified, all embodiments and preferred embodiments mentioned herein can be combined to form new technical solutions.

[0022] Unless otherwise specified, all the technical features and preferred features mentioned herein can be combined to form new technical solutions.

[0023] In this invention, unless otherwise specified, percentage (%) or parts refer to weight percentage or parts relative to the composition.

[0024] Unless otherwise specified, the components or preferred components involved in this invention can be combined with each other to form new technical solutions.

[0025] In this invention, unless otherwise specified, the numerical range "a~b" is an abbreviation for any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "6~22" indicates that all real numbers between "6~22" have been listed in this document, and "6~22" is simply an abbreviation for these numerical combinations.

[0026] The "scope" disclosed in this invention can be in the form of a lower limit and an upper limit, and can be one or more lower limits and one or more upper limits, respectively.

[0027] The term “and / or” as used in this invention refers to any combination of one or more of the associated listed items, as well as all possible combinations, and includes such combinations.

[0028] Unless otherwise stated, the technical and scientific terms used herein have the same meanings as those familiar to those skilled in the art. Furthermore, any methods or materials similar to or equivalent to those described herein may also be used in this invention.

[0029] This invention provides a method for preparing a frost-like structure of hydrogenated titanium oxide-coated porous carbon nanofiber composite material. Porous carbon nanofibers (PC) and glycerol are dissolved in anhydrous ethanol solvent in a certain proportion, and TiO2-F127 single micelles are dissolved in anhydrous ethanol solvent to prepare homogeneous solutions. The two solutions are mixed and stirred for a sufficient time to achieve homogeneity. The resulting homogeneous solution undergoes hydrothermal self-assembly to obtain TiO2-coated porous carbon nanofibers (PC@TiO2 nanofibers). The PC@TiO2 nanofibers are then pyrolyzed at high temperature under an Ar / H2 atmosphere to obtain a frost-like structure of hydrogenated titanium oxide-coated porous carbon nanofiber composite material (frost-like structure PC@TiO2). 2-x Nanofibers); Frost-like PC@TiO 2-x A dielectric sample was prepared by mixing nanofibers and paraffin in a certain proportion, and its electromagnetic wave absorption performance was tested; TiO2 2-x The addition of [component name] not only effectively improves the impedance mismatch problem of PC nanofibers and broadens the effective absorption width of composite fibers, but also the porous structure design can effectively reduce the filling ratio of the material.

[0030] This invention provides a method for preparing a porous carbon nanofiber composite material with a haze-like structure coated with hydrogenated titanium oxide, comprising the following steps: S1. Place PC nanofibers and anhydrous ethanol into a polytetrafluoroethylene liner, and add glycerol in a certain proportion to obtain solution A; place TiO2-F127 single micelles in a weighing bottle, add anhydrous ethanol to obtain solution B, and stir the obtained solutions A and B separately with a magnetic stirrer for 0.5~1.0 h until they are homogeneous solutions. The preparation method of PC nanofibers is as follows: 0.9 g of polyacrylonitrile (PAN) and 0.3 g of polystyrene (PS) were dissolved in 9.1 g and 1.4 g of N,N-dimethylformamide (DMF), respectively. The two solutions were then mixed and stirred at room temperature for 12 h to obtain a homogeneous precursor solution for electrospinning. The precursor solution was then loaded into a 5 mL syringe, and electrospinning was performed at a receiving distance of 20 cm, a voltage of 18 kV, and a feed rate of 0.2 mm / min for 2 h to obtain PAN-PS composite fibers. The collected fibers were treated in an 80℃ forced-air drying oven for 4 h, followed by pre-oxidation at 200℃ for 2 h. Under argon protection, the temperature was increased to 800℃ at a heating rate of 2℃ / min and calcined for 2 h to finally obtain PC nanofibers.

[0031] The preparation method of TiO2-F127 single micelles includes: First, 1.5 g of triblock copolymer Pluronic F127 is added to 30.0 mL of tetrahydrofuran (THF) solution and stirred until completely dissolved; then, 2.4 mL of acetic acid (HOAc) and 3.2 mL of hydrochloric acid (HCl) are slowly added dropwise to the above mixed solution, and stirred continuously for 10 min to prepare a homogeneous and transparent mixed solution; then, 3.0 mL of tetrabutyl titanate (TBOT) is added dropwise to it, and stirred rapidly for 10 min to obtain a yellowish-white mixed solution; finally, the obtained solution is transferred to two volumetric flasks, placed in a sealed drying oven, and evaporated at 45℃ for 30 h to finally obtain TiO2-F127 single micelles.

[0032] The mass / volume ratio of porous carbon nanofibers: anhydrous ethanol: glycerol is 200mg: 10mL: (5~10)mL; the mass / volume ratio of TiO2-F127: anhydrous ethanol is (1.0~2.0)g: 5mL.

[0033] S2. Slowly add the homogeneous solution B obtained in step S1 to solution A under magnetic stirring, and then stir for 6-12 hours to ensure that the two solutions are fully mixed. S3. Place the mixed solution obtained in step S2 into a reaction vessel and carry out a hydrothermal reaction in an oven at 80~120℃ for 8~12h. After centrifugation and drying, the obtained product is used to obtain TiO2-coated porous carbon nanofibers (PC@TiO2 nanofibers). S4. The PC@TiO2 nanofibers obtained in step S3 are sintered in an Ar / H2 atmosphere (Ar / H2 volume ratio 9:1), heated to 600-800°C at a rate of 2-4°C / min, and annealed for 2-4 h to obtain a haze-like structured hydrogenated titanium oxide-coated porous carbon nanofiber composite material (haze-like structured PC@TiO2).2-x Nanocomposite fibers).

[0034] The PC@TiO3 with a frost-like structure prepared by this invention 2-x Nanocomposite fibers not only possess the high aspect ratio and high electrical conductivity of carbon nanofibers, but also introduce rich interfacial polarization and multiple reflections and scatterings through their unique frost-like structure (a frost-like structure refers to TiO2 nanosheets uniformly and densely coating the surface of porous carbon nanofibers in a frost-like morphology, with the nanosheets overlapping to form a continuous network-like coating layer). Furthermore, they utilize the combination of PC nanofibers and TiO2... 2-x The heterogeneous interface between them enhances dielectric loss, thus exhibiting excellent impedance matching characteristics and broadband strong absorption capability in electromagnetic wave absorption.

[0035] Pure porous carbon nanofibers have relatively high real and imaginary dielectric values, and are mainly characterized by dielectric loss with low loss capacity. With the addition of TiO2-F127 single micelles, uniformly coated TiO2 nanosheets are generated on the surface of PC nanofibers. They work synergistically with PC nanofibers to significantly improve the effective absorption width and optimal reflection loss.

[0036] This invention uses PC nanofibers and TiO2-F127 single micelles as raw materials, glycerol as a confinement solvent, and anhydrous ethanol as a solvent. A hoarfrost-like PC@TiO2 structure is prepared by hydrothermal self-assembly and high-temperature treatment under an Ar / H2 atmosphere. 2-x Composite nanofibers. The thickness of TiO2 was precisely controlled by adjusting the glycerol content in the solution. As the glycerol content increased, the thickness of TiO2 gradually decreased, resulting in improved electromagnetic wave absorption performance. This invention features a simple process and produces fibers with a unique morphology. TiO2 nanosheets are uniformly coated on the surface of PC nanofibers, creating a frost-like structure of PC@TiO2. 2-x Nanocomposite fibers exhibit excellent electromagnetic wave absorption properties.

[0037] This invention provides a method for preparing a porous carbon nanofiber composite material with hydrogenated titanium oxide coated with a frost-like structure. The method mainly employs a simple hydrothermal self-assembly method and a high-temperature pyrolysis process to obtain PC@TiO₂ with a porous, frost-like nanofiber morphology and excellent electromagnetic wave absorption properties. 2-x Nanofibers are an electromagnetic wave absorbing material with promising application prospects. Their preparation conditions are easy to achieve, the operation is simple, the morphology is uniform and easy to control, and the specific surface area is large.

[0038] This invention provides a PC@TiO3 structure resembling frost. 2-x Preparation method of nanocomposite fibers, PC@TiO 2-xNanofibers possess the structural advantage of easily establishing an internal conductive network through their interwoven one-dimensional structure, facilitating electron migration within the fiber and transitions between fibers, effectively enhancing electrical conductivity. Rutile-anatase two-phase TiO₂ 2-x The introduction of nanosheets and their composite with PC nanofibers to achieve a frost-like structure effectively enhances dipole polarization and interfacial polarization. Furthermore, the presence of a porous structure effectively increases the interfacial area of ​​the system, thereby significantly improving its electromagnetic wave absorption performance. In this invention, TiO2 nanosheets are prepared using PC nanofibers as a structural template and TiO2-F127 single micelles as a precursor, and glycerol is introduced as a confinement solvent to regulate the TiO2 nanosheets. 2-x The thickness of the layer, through hydrothermal self-assembly process and subsequent high-temperature treatment in Ar / H2 atmosphere, yields a hoarfrost-like structure with excellent microwave absorption properties, PC@TiO2. 2-x Composite nanofibers.

[0039] Furthermore, with a mass / volume ratio of PC nanofibers: anhydrous ethanol: glycerol of 200 mg: 10 mL: (5-10) mL, the addition of glycerol not only precisely controlled the thickness of the TiO2 nanosheets, but also slowed down the hydrolysis and condensation rate of the titanium oligomers.

[0040] Furthermore, the mass / volume ratio of TiO2-F127 to anhydrous ethanol is (1.0~2.0) g: 5 mL, which ensures complete dissolution of TiO2-F127 and avoids the aggregation of TiO2-F127 single micelles.

[0041] Furthermore, in order to ensure that PC is uniformly dispersed and TiO2-F127 is fully dissolved, they are first dissolved in anhydrous ethanol / glycerol and anhydrous ethanol. Sufficient stirring time is required to ensure that they are uniformly dispersed, which is beneficial for the thorough mixing of the solution in the next step.

[0042] Furthermore, since the solute and solvent diffuse in the mixed solution, it is essential to ensure that the PC nanofibers and TiO2-F127 single micelles are completely encapsulated by the glycerol solvent to prevent the self-assembly of the single micelles at room temperature. Therefore, sufficient stirring time is necessary.

[0043] Furthermore, the mixed solution requires sufficient hydrothermal temperature and time to ensure that TiO2-F127 has enough time and driving force to grow TiO2 nanosheets on the PC nanofiber surface; the hydrothermal temperature should not be too low or too high to ensure sufficient driving force for the diffusion of glycerol solvent; the hydrothermal time should not be too short to ensure sufficient time for the solution to diffuse.

[0044] Furthermore, the prepared fibers were calcined at a specific temperature under an Ar / H2 atmosphere. Hydrogen, acting as a reducing agent, could create oxygen vacancies in the material and reduce high-valence metal ions to low-valence states, which was beneficial for the generation of dipole polarization. Simultaneously, the heating rate for the prepared composite fibers had to be within a certain range; if the heating was too rapid, the frost-like morphology of the fibers would be difficult to maintain.

[0045] The present invention provides a hydrogenated titanium oxide-coated porous carbon nanofiber composite material with a frost-like structure as a microwave absorbing material. It can construct an internal conductive network, and the porous structure effectively increases the internal interface area, thereby reducing both the real and imaginary parts of the dielectric constant, enhancing reflection loss, and significantly improving the effective absorption width.

[0046] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some, not all, of the embodiments of the present invention. The components of the embodiments of the present invention described and shown in the accompanying drawings can generally be arranged and designed in various different configurations. Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the claimed invention, but merely to illustrate selected embodiments of the invention. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without inventive effort are within the scope of protection of the present invention.

[0047] Example 1 Weigh 200 mg of PC nanofibers and disperse them in 10 mL of anhydrous ethanol. Then add 5 mL of glycerol and stir the solution under magnetic stirring for 0.5 h to obtain a homogeneous solution A. Meanwhile, 1.5g of TiO2-F127 was weighed and dissolved in 5mL of anhydrous ethanol. This solution was stirred under magnetic stirring for 0.5h to obtain a homogeneous solution B. Under magnetic stirring, solution B was slowly added to solution A, and the mixture was stirred magnetically for 6 hours until a homogeneous and stable mixed solution C was formed. The resulting mixed solution was subjected to a hydrothermal reaction in an oven at 100°C for 12 hours. The resulting nanofibers were then sintered in an Ar / H2 atmosphere, with the temperature increased at 2°C / min, and annealed at 700°C for 4 hours to obtain PC@TiO. 2-x Nanofibers.

[0048] The composite nanofibers maintain one-dimensional morphological characteristics, with TiO2 nanosheets uniformly coated on the fiber surface. The TiO2 nanosheets overlap each other to form an interconnected and dense network morphology.

[0049] Example 2 Weigh 200 mg of PC nanofibers and disperse them in 10 mL of anhydrous ethanol. Then add 7.5 mL of glycerol and stir the solution under magnetic stirring for 0.5 h to obtain a homogeneous solution A. Meanwhile, 1.5g of TiO2-F127 was weighed and dissolved in 5mL of anhydrous ethanol. This solution was stirred under magnetic stirring for 0.5h to obtain a homogeneous solution B. Under magnetic stirring, solution B was slowly added to solution A, and the mixture was stirred magnetically for 6 hours until a homogeneous and stable mixed solution C was formed. The resulting mixed solution was subjected to a hydrothermal reaction in an oven at 100°C for 12 hours. The resulting nanofibers were then sintered in an Ar / H2 atmosphere, with the temperature increased at 2°C / min, and annealed at 700°C for 4 hours to obtain PC@TiO. 2-x Nanofibers.

[0050] The fiber surface is coated with dense, fine, and uniform TiO2 nanosheets, which are tightly bonded to the PC fiber matrix without significant agglomeration or detachment. Simultaneously, the thickness of the TiO2 shell is significantly reduced. This is because the confinement effect is enhanced with increasing glycerol content, leading to a gradual decrease in the thickness of the TiO2 nanosheet layer.

[0051] Example 3 Weigh 200 mg of PC nanofibers and disperse them in 10 mL of anhydrous ethanol. Then add 10 mL of glycerol and stir the solution under magnetic stirring for 0.5 h to obtain a homogeneous solution A. Meanwhile, 1.5g of TiO2-F127 was weighed and dissolved in 5mL of anhydrous ethanol. This solution was stirred under magnetic stirring for 0.5h to obtain a homogeneous solution B. Under magnetic stirring, solution B was slowly added to solution A, and the mixture was stirred magnetically for 6 hours until a homogeneous and stable mixed solution C was formed. The resulting mixed solution was subjected to a hydrothermal reaction in an oven at 100°C for 12 hours. The resulting nanofibers were then sintered in an Ar / H2 atmosphere, with the temperature increased at 2°C / min, and annealed at 700°C for 4 hours to obtain PC@TiO. 2-x Nanofibers.

[0052] The TiO2 loading on the fiber surface of this sample is mainly composed of nanoparticles, with only a small number of TiO2 nanosheets scattered around. The overall loading is low and the distribution is relatively sparse, and no continuous and dense coating layer is formed. The fiber body still maintains a relatively smooth morphology.

[0053] Example 4 Weigh 200 mg of PC nanofibers and disperse them in 10 mL of anhydrous ethanol. Then add 7.5 mL of glycerol and stir the solution under magnetic stirring for 0.5 h to obtain a homogeneous solution A. Meanwhile, 2.0 g of TiO2-F127 was weighed and dissolved in 5 mL of anhydrous ethanol. This solution was stirred under magnetic stirring for 0.5 h to obtain a homogeneous solution B. Under magnetic stirring, solution B was slowly added to solution A, and the mixture was stirred magnetically for 6 hours until a homogeneous and stable mixed solution C was formed. The resulting mixed solution was subjected to a hydrothermal reaction in an oven at 100°C for 12 hours. The resulting nanofibers were then sintered in an Ar / H2 atmosphere, with the temperature increased at 2°C / min, and annealed at 700°C for 4 hours to obtain PC@TiO. 2-x Nanofibers.

[0054] Example 5 Weigh 200 mg of PC nanofibers and disperse them in 10 mL of anhydrous ethanol. Then add 7.5 mL of glycerol and stir the solution under magnetic stirring for 0.5 h to obtain a homogeneous solution A. Meanwhile, 1.5g of TiO2-F127 was weighed and dissolved in 5mL of anhydrous ethanol. This solution was stirred under magnetic stirring for 0.5h to obtain a homogeneous solution B. Under magnetic stirring, solution B was slowly added to solution A, and the mixture was stirred magnetically for 6 hours until a homogeneous and stable mixed solution C was formed. The resulting mixed solution was subjected to a hydrothermal reaction in an oven at 120°C for 12 h, and then the resulting nanofibers were sintered in an Ar / H2 atmosphere, with the temperature increased at 2°C / min, and annealed at 700°C for 4 h to obtain PC@TiO. 2-x Nanofibers.

[0055] Example 6 Weigh 200 mg of porous carbon nanofibers and disperse them in 10 mL of anhydrous ethanol. Then add 7.5 mL of glycerol and stir the solution under magnetic stirring for 1.0 h to obtain a homogeneous solution A. Meanwhile, 1.0 g of TiO2-F127 was weighed and dissolved in 5 mL of anhydrous ethanol. This solution was stirred under magnetic stirring for 1.0 h to obtain a homogeneous solution B. Under magnetic stirring, solution B was slowly added to solution A, and the mixture was stirred magnetically for 12 hours until a homogeneous and stable mixed solution C was formed. The resulting mixed solution was subjected to a hydrothermal reaction in an oven at 80°C for 8 hours. The resulting nanofibers were then sintered in an Ar / H2 atmosphere, with the temperature increased at 4°C / min, and annealed at 600°C for 2 hours to obtain PC@TiO.2-x Nanofibers.

[0056] Example 7 Weigh 200 mg of porous carbon nanofibers and disperse them in 10 mL of anhydrous ethanol. Then add 7.5 mL of glycerol and stir the solution under magnetic stirring for 1.0 h to obtain a homogeneous solution A. Meanwhile, 1.0 g of TiO2-F127 was weighed and dissolved in 5 mL of anhydrous ethanol. This solution was stirred under magnetic stirring for 1.0 h to obtain a homogeneous solution B. Under magnetic stirring, solution B was slowly added to solution A, and the mixture was stirred magnetically for 12 hours until a homogeneous and stable mixed solution C was formed. The resulting mixed solution was subjected to a hydrothermal reaction in an oven at 80°C for 8 hours. The resulting nanofibers were then sintered in an Ar / H2 atmosphere, with the temperature increased at 3°C / min, and annealed at 800°C for 3 hours to obtain PC@TiO. 2-x Nanofibers.

[0057] Example 8 Weigh 200 mg of porous carbon nanofibers and disperse them in 10 mL of anhydrous ethanol. Then add 7.5 mL of glycerol and stir the solution under magnetic stirring for 1.0 h to obtain a homogeneous solution A. Meanwhile, 1.0 g of TiO2-F127 was weighed and dissolved in 5 mL of anhydrous ethanol. This solution was stirred under magnetic stirring for 1.0 h to obtain a homogeneous solution B. Under magnetic stirring, solution B was slowly added to solution A, and the mixture was stirred magnetically for 12 hours until a homogeneous and stable mixed solution C was formed. The resulting mixed solution was subjected to a hydrothermal reaction in an oven at 120°C for 12 h, and then the resulting nanofibers were sintered in an Ar / H2 atmosphere, with the temperature increased at 4°C / min, and annealed at 700°C for 4 h to obtain PC@TiO. 2-x Nanofibers.

[0058] Example 9 Weigh 200 mg of porous carbon nanofibers and disperse them in 10 mL of anhydrous ethanol. Then add 7.5 mL of glycerol and stir the solution under magnetic stirring for 1.0 h to obtain a homogeneous solution A. Meanwhile, 1.0 g of TiO2-F127 was weighed and dissolved in 5 mL of anhydrous ethanol. This solution was stirred under magnetic stirring for 1.0 h to obtain a homogeneous solution B. Under magnetic stirring, solution B was slowly added to solution A, and the mixture was stirred magnetically for 12 hours until a homogeneous and stable mixed solution C was formed. The resulting mixed solution was subjected to a hydrothermal reaction in an oven at 80°C for 12 hours. The resulting nanofibers were then sintered in an Ar / H2 atmosphere, with the temperature increased at 4°C / min, and annealed at 600°C for 2 hours to obtain PC@TiO. 2-x Nanofibers.

[0059] Figure 1 The images show SEM (a) and TEM (b) images of the PC nanofibers disclosed in this invention. The SEM images reveal that the PC nanofibers exhibit a typical one-dimensional fiber morphology with relatively uniform fiber diameter and a smooth surface. The fibers interlock to form a three-dimensional network structure, which facilitates axial migration of electrons within the fibers and hopping conduction between fibers, laying the structural foundation for the subsequent construction of a conductive loss network. The TEM images further confirm the presence of a distinct porous structure (light-colored area) within the PC nanofibers, with a relatively uniform pore distribution. The introduction of this porous structure reduces the effective dielectric constant of the material, which helps to improve the inherent impedance mismatch problem of carbon materials. Furthermore, the presence of the porous-air interface provides a structural basis for multiple reflections and scattering of electromagnetic waves, contributing to enhanced electromagnetic energy dissipation.

[0060] Figure 2 The PC@TiO3 with a frost-like structure prepared in Examples 1, 2 and 3 of this invention 2-x SEM images of nanofibers, where (a) is PC@TiO 2-x -5 nanofibers represent an addition of 5 mL of glycerol; (b) represents PC@TiO 2-x -7.5 nanofibers represent an addition of 7.5 mL of glycerol; (c) represents PC@TiO 2-x -10 nanofibers represent an addition of 10 mL of glycerol. As shown in the figure, the amount of glycerol added precisely controls the coating thickness and density of the TiO2 nanosheets, with an optimal value (7.5 mL) at which the frost-like structure is most complete and uniform. When the coating thickness is moderate, it retains the conductivity loss capability of the carbon core while introducing abundant interfacial polarization loss, achieving synergistic enhancement.

[0061] Figure 3 PC@TiO2-7.5 nanofibers (a) and PC@TiO2 nanofibers prepared in Example 2 of this invention 2-x -7.5 nm fiber (b) dielectric constant real and imaginary parts plot; as can be seen from the figure, the untreated sample relies solely on the heterostructure between TiO2 and PC for limited interfacial polarization, while hydrogenation introduces oxygen vacancies and Ti... 3+ The mixed crystalline phase significantly improves dielectric loss capability and is a key triggering step for the synergistic effect of multi-level loss mechanisms.

[0062] Figure 4 PC@TiO prepared in Example 2 of this invention 2-x - Three-dimensional reflection loss diagram (a) and effective absorption bandwidth diagram (b) of 7.5 nanofibers as microwave absorbing material; it can be seen from the figure that the composite nanofibers with 7.5 mL of glycerol addition have significantly improved effective absorption bandwidth, which can completely cover the Ku band and X band, and can achieve most of the coverage of the C band and S band at different thicknesses.

[0063] In summary, this invention discloses a haze-like structure of hydrogenated titanium oxide-coated porous carbon nanofiber composite material, its preparation method, and its application. Using PC as a structural template, TiO2-F127 single micelles are added to improve the microwave absorption properties of the nanofibers, generating TiO2 nanosheets uniformly distributed on the surface of the PC fibers, thus preparing a haze-like PC@TiO2 composite material. 2-x Nanofibers enhance both the real and imaginary parts of the dielectric constant and introduce a multiple loss mechanism to achieve optimal impedance matching and minimum reflection loss. One-dimensional frost-like PC@TiO₂ was prepared using a simple hydrothermal self-assembly method. 2-x Nanocomposite fibers combine the advantages of both the hazy morphology and porous structure of materials, enabling the prepared materials to exhibit excellent electromagnetic wave absorption performance.

[0064] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a porous carbon nanofiber composite material with hydrogenated titanium oxide coated with a rime-like structure, characterized in that, include: Porous carbon nanofibers were dispersed in anhydrous ethanol and glycerol to obtain solution A; TiO2-F127 single micelles were dispersed in anhydrous ethanol to obtain solution B; Solution A and solution B were mixed and stirred, and then subjected to a hydrothermal reaction. After centrifugation and drying, TiO2-coated porous carbon nanofibers were obtained. The TiO2-coated porous carbon nanofibers were calcined in a mixed atmosphere of Ar and H2 to obtain a rime-like structure of hydrogenated titanium oxide-coated porous carbon nanofiber composite material.

2. The method for preparing the hydrogenated titanium oxide-coated porous carbon nanofiber composite material with a rime-like structure according to claim 1, characterized in that, In solution A, the ratio of porous carbon nanofibers, anhydrous ethanol, and glycerol is 200 mg: 10 mL: (5~10) mL; in solution B, the ratio of TiO2-F127 single micelles to anhydrous ethanol is (1.0~2.0) g: 5 mL.

3. The method for preparing the hydrogenated titanium oxide-coated porous carbon nanofiber composite material with a rime-like structure according to claim 1, characterized in that, Solution A and solution B are stirred for 0.5 to 1.0 hours until homogeneous.

4. The method for preparing the hydrogenated titanium oxide-coated porous carbon nanofiber composite material with a frost-like structure according to claim 1, characterized in that, The mixing and stirring time for solution A and solution B is 6~12 hours.

5. The method for preparing the hydrogenated titanium oxide-coated porous carbon nanofiber composite material with a rime-like structure according to claim 1, characterized in that, The hydrothermal reaction is carried out at a temperature of 80-120°C for 8-12 hours.

6. The method for preparing the hydrogenated titanium oxide-coated porous carbon nanofiber composite material with a rime-like structure according to claim 1, characterized in that, The calcination process involves a heating rate of 2-4°C / min, a temperature of 600-800°C, and a time of 2-4 hours.

7. A hydrogenated titanium oxide-coated porous carbon nanofiber composite material with a rime-like structure, characterized in that, The composite material is prepared by the method described in any one of claims 1-6, which is a hydrogenated titanium oxide-coated porous carbon nanofiber composite material with a rime-like structure.

8. The method for preparing the hydrogenated titanium oxide-coated porous carbon nanofiber composite material with a frost-like structure according to claim 7, characterized in that, The frost-like structure is a frost-like morphology structure formed by uniformly coating TiO2 nanosheets on the surface of porous carbon nanofibers, wherein the TiO2 nanosheets overlap each other to form a continuous and dense coating layer.

9. The method for preparing the hydrogenated titanium oxide-coated porous carbon nanofiber composite material with a frost-like structure according to claim 7, characterized in that, In the aforementioned haze-like structure of hydrogenated titanium oxide-coated porous carbon nanofiber composite material, hydrogenated titanium oxide is uniformly coated on the surface of porous carbon nanofibers in the form of nanosheets. The thickness of the hydrogenated titanium oxide coating layer is controlled by the amount of glycerol added. The hydrogenated titanium oxide is a mixed crystal phase of anatase and rutile.

10. The application of the hydrogenated titanium oxide-coated porous carbon nanofiber composite material with a frost-like structure as described in any one of claims 7-9 in the absorption of low-frequency electromagnetic waves.

Citation Information

Patent Citations

  • A method for preparing a multi-level structured titanium dioxide / carbon nanofiber anode material

    CN112886013B

  • A flexible SiC / C nanocomposite fiber, its preparation method and application

    CN113737314B