A glass fiber electronic cloth and its preparation method

By constructing a hydrophobic modified CNF nanofiber coating on the surface of glass fiber base cloth, the dielectric drift problem of glass fiber electronic cloth in humid and hot environments is solved, achieving low dielectric loss and high resistance to humid and hot conditions, making it suitable for 5G/6G high-frequency communication and automotive high-frequency electronic devices.

CN123108949APending Publication Date: 2026-11-17JIANGSU JIESI NEW ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611076777.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-20
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Traditional fiberglass electronic cloth suffers severe dielectric property drift in humid and hot environments, failing to meet the stability requirements of 5G/6G high-frequency and high-speed communication. Conventional modification methods cannot effectively eliminate microscopic pore defects and moisture absorption problems.

Method used

A dense, hydrophobic nanofiber low dielectric functional coating is constructed on the surface of a glass fiber substrate by combining hydrophobic modified CNF nanofibers with a silane coupling agent and employing processes such as gradient step feeding, vacuum degassing, and explosion-proof curing to seal pores and reduce dielectric loss.

Benefits of technology

The glass fiber electronic cloth achieves low dielectric constant and low dielectric loss at high frequencies, improving its resistance to damp heat and dimensional stability. The dielectric constant is 3.0 to 3.2, the dielectric loss is ≤0.008, the moisture content is ≤0.3%, the heat deformation rate is ≤0.08%, and the dielectric performance decay rate is ≤3%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108949A_ABST
    Figure CN123108949A_ABST
Patent Text Reader

Abstract

This application discloses a glass fiber electronic cloth and its preparation method. The glass fiber electronic cloth comprises a glass fiber base cloth and a nanofiber low-dielectric functional coating. The nanofiber low-dielectric functional coating is composited on one or both sides of the glass fiber base cloth. The nanofiber low-dielectric functional coating comprises the following raw materials in the indicated mass percentages: hydrophobically modified CNF nanofibers: 1.5wt%–3.0wt%; silane coupling agent: 0.8wt%–1.5wt%; crosslinking aid: 0.3wt%–0.6wt%; organic solvent: 94.9wt%–97.wt%. The hydrophobically modified CNF nanofibers are obtained by hydrophobically modifying wood-based CNF nanofibers. This application can eliminate microscopic pore defects caused by the weaving process, solve the dielectric drift problem, and reduce the overall dielectric constant and high-frequency dielectric loss of the composite material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the fields of new electronic insulation materials, high-frequency copper-clad laminate substrates, and precision electronic composite materials. Specifically, it relates to a glass fiber electronic cloth and its preparation method, which is suitable for the large-scale production and high-end application scenarios of 5G / 6G high-frequency high-speed communication copper-clad laminates, automotive high-frequency electronic devices, precision electronic insulation components, and high-end signal transmission substrates. Background Technology

[0002] Fiberglass electronic cloth is a core substrate for the fabrication of high-frequency copper-clad laminates and electronic insulating devices, and is widely used in communication equipment, automotive intelligent electronics, precision industrial control, and new energy electronics. With the rapid iteration of 5G high-frequency high-speed communication and millimeter-wave signal transmission technologies, terminal devices have increasingly higher requirements for the high-frequency dielectric stability, low-loss characteristics, moisture and heat resistance, and batch consistency of insulating substrates. Traditional modified fiberglass electronic cloth can no longer meet the application standards of high-end high-frequency electronics.

[0003] Low-dielectric glass fiber modification technologies in related fields typically focus on modifying the glass fiber yarn itself, improving the inherent dielectric parameters of the yarn by adjusting the glass composition, doping with metal oxides, and optimizing the drawing process. However, this approach can only optimize the initial dielectric properties of the substrate and cannot eliminate the micropores formed after glass fiber weaving. These micropores easily absorb ambient moisture, causing significant drift in the dielectric constant and dielectric loss of the product under humid and hot conditions, a substantial decrease in the stability of high-frequency signal transmission, and performance degradation after humid and hot aging.

[0004] To improve porosity defects, related technologies also employ post-processing modification methods such as inorganic filler doping, ordinary sol impregnation, and hydrophilic nanofiber blending. However, conventional hydrophilic nanocellulose contains a large number of hydrophilic groups, and doping will further increase the hygroscopicity of the substrate, which will exacerbate high-frequency dielectric loss.

[0005] Therefore, it is of particular importance to provide a glass fiber electronic cloth and its preparation method to solve the moisture absorption defect of glass fiber substrate, thereby solving the problem of damp heat dielectric drift defect. Summary of the Invention

[0006] To address the aforementioned technical problems, this application proposes a glass fiber electronic cloth and its preparation method.

[0007] On the one hand, embodiments of this application provide a fiberglass electronic cloth, which includes a fiberglass base cloth and a nanofiber low-dielectric functional coating, wherein the nanofiber low-dielectric functional coating is composited on one or both sides of the surface of the fiberglass base cloth; The nanofiber low-dielectric functional coating comprises the following raw materials by mass percentage: Hydrophobically modified CNF nanofibers: 1.5wt%~3.0wt%; Silane coupling agent: 0.8wt%~1.5wt%; Crosslinking aid: 0.3wt%~0.6wt% Organic solvents: 94.9 wt% to 97 wt%; The hydrophobically modified CNF nanofibers are obtained by using lignin-based CNF nanofibers as raw materials and then performing hydrophobic modification treatment.

[0008] In an optional embodiment, the fiberglass base fabric is an alkali-free fiberglass cloth with a thickness ranging from 0.08 mm to 0.20 mm, and the organic solvent is electronic-grade anhydrous ethanol.

[0009] In an optional embodiment, the thickness of the nanofiber low-dielectric functional coating is 3 × 10⁻⁶. -6 m~8×10 -6 m.

[0010] On the other hand, embodiments of this application also provide a method for preparing glass fiber electronic cloth, the method comprising: S1. Provide fiberglass base fabric; S2. The hydrophobically modified CNF nanofibers, silane coupling agent, crosslinking aid, and organic solvent are dispersed and vacuum degassed according to the mass ratio to obtain a low dielectric functional coating of nanofibers. S3. The nanofiber low dielectric functional coating is uniformly coated on one or both sides of the glass fiber base cloth to obtain the coated glass fiber cloth. S4. The coated glass fiber cloth is subjected to explosion-proof curing treatment to obtain explosion-proof cured glass fiber cloth; S5. In the modified liquid, the glass fiber cloth after the explosion-proof curing treatment is subjected to silane interface hydrophobic crosslinking modification treatment to obtain glass fiber electronic cloth.

[0011] In an optional embodiment, in step S2, an organic solvent, hydrophobically modified CNF nanofibers, silane coupling agent and crosslinking aid are sequentially added using a gradient step feeding process. The dispersion speed of the slurry in the dispersion treatment is 800 r / min to 1200 r / min, and the dispersion time is 1500 s to 2100 s; The vacuum degassing negative pressure during the vacuum degassing process is -8×10⁻⁸. 4 Pa ~ -9×10 4 Pa, degassing time is 900s to 1200s.

[0012] In an optional embodiment, in step S3, the coating speed is 5 m / min to 8 m / min, the coating constant tension is 20 N to 25 N, and the coating thickness deviation is ≤ ±0.5 × 10⁻⁶.-6 m.

[0013] In an optional embodiment, the explosion-proof curing treatment in step S4 is a three-stage gradient explosion-proof curing treatment, which includes a pre-baking stage, a curing stage, and a ripening stage. The temperature of the pre-baking stage is 353.15K to 363.15K, and the pre-baking time is 40s to 60s; The curing stage has a temperature of 393.15K to 403.15K and a curing time of 80s to 100s. The temperature during the curing stage is 423.15K to 433.15K, and the curing time is 100s to 120s.

[0014] In an optional embodiment, in step S5, the modified liquid is a fluorinated silane anhydrous ethanol solution, the mass concentration of the modified liquid is 2.0% to 3.5%, the immersion temperature is 318.15K to 328.15K, and the immersion time is 30s to 50s.

[0015] In an optional embodiment, after the explosion-proof cured glass fiber cloth undergoes silane interfacial hydrophobic crosslinking modification treatment, the method further includes: A constant tension slitting and winding machine was used to slit and rewind the cross-linked modified glass fiber cloth under constant tension. The constant tension slitting and winding machine has a fabric feeding speed of 6m / min to 10m / min, a slitting tension of 18N to 20N for thin coatings, a slitting tension of 22N to 24N for thick coatings, and a slitting accuracy of ±0.1×10⁻⁶. - ³m, with a winding pressure of 0.3MPa~0.5MPa.

[0016] In an optional embodiment, the preparation method is carried out in a dust-free environment with an ambient temperature of 295.15K to 299.15K and a relative humidity of 45% to 60%.

[0017] Based on the above technical solution, the embodiments of this application have at least the following beneficial effects: This application proposes a glass fiber electronic cloth and its preparation method. This application abandons the traditional approach of modifying hydrophilic nanofibers, instead using a glass fiber substrate as the base and hydrophobically modified CNF nanofibers as the core functional filler, combined with a silane coupling agent crosslinking system. A dense, hydrophobic, low-dielectric functional coating of nanofibers is constructed on the surface of the glass fiber substrate. The hydrophobically modified CNF nanofibers are obtained from wood-based CNF nanofibers after hydrophobic modification. The mass ratio of each raw material is as follows: hydrophobically modified CNF nanofibers: 1.5wt%–3.0wt%; silane coupling agent: 0.8wt%–1.5wt%; crosslinking aid: 0.3wt%–0.6wt%; organic solvent: 94.9wt%–97.wt%.

[0018] After the fiberglass substrate is woven, a large number of micron- and submicron-sized interconnected pores naturally exist on the surface and inside the substrate. These pore structures easily trap air and adsorb environmental moisture. Air has a dielectric constant of approximately 1.0, while water molecules have a dielectric constant as high as 80. These two factors are the core causes of high-frequency polarization loss and unstable dielectric parameters in fiberglass electronic fabrics. Related technologies only focus on optimizing the fiberglass yarn formulation, which can only improve the inherent properties of the glass itself and cannot eliminate the microscopic pore defects introduced by the weaving process, thus failing to fundamentally solve the dielectric drift problem. This application uses hydrophobically modified CNF nanofibers. With their nanoscale ultrafine size and ultra-high aspect ratio, these nanofibers can precisely penetrate, fill, and seal the micropores of the fiberglass substrate, completely replacing the original air and moisture adsorption sites within the pores. By combining physical pore sealing with chemical hydrophobic modification, the high-loss "glass fiber-pore-air-water vapor" microstructure in related technologies is reconstructed into a dense, low-polarization, and highly stable nanofiber composite structure, which significantly reduces the overall dielectric constant and high-frequency dielectric loss of the composite material from the physical structure level.

[0019] As can be seen, this application uses fiberglass base fabric as the matrix and hydrophobically modified CNF nanofibers as the core functional filler. The hydrophobically modified CNF nanofibers can seal pores, suppress moisture, and reduce dielectric loss. The silane coupling agent can perform interfacial crosslinking, enhancing the bonding force between the coating and the fiberglass and sealing the hydrophilic groups of the base fabric. The crosslinking aid can improve the crosslinking density, structural stability, and weather resistance of the coating. The organic solvent can disperse the medium, ensuring no impurity contamination and guaranteeing low dielectric insulation performance. Therefore, by using the above formulation, the hydrophilic groups of the fibers can be eliminated, the micropores of the fiberglass can be precisely filled, and the surface polarity of the matrix can be reduced. This fundamentally suppresses water vapor adsorption and high-frequency polarization loss, solving the core defect of damp heat dielectric drift in related technologies, and achieving a comprehensive performance improvement of fiberglass electronic cloth with low loss, high damp heat resistance, and high dimensional stability. Attached Figure Description

[0020] To more clearly illustrate the technical solutions and advantages in the embodiments of this application or related technologies, the drawings used in the description of the embodiments or related technologies will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0021] Figure 1 This is a schematic flowchart illustrating an exemplary embodiment of the preparation method of a fiberglass-free electronic cloth. Detailed Implementation

[0022] The technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of this application.

[0023] This application provides a fiberglass electronic cloth, which includes a fiberglass base cloth and a nanofiber low-dielectric functional coating, wherein the nanofiber low-dielectric functional coating is laminated on one or both sides of the surface of the fiberglass base cloth. The nanofiber low-dielectric functional coating comprises the following raw materials by mass percentage: Hydrophobically modified CNF nanofibers: 1.5wt%~3.0wt%; Silane coupling agent: 0.8wt%~1.5wt%; Crosslinking aid: 0.3wt%~0.6wt% Organic solvents: 94.9 wt% to 97 wt%; The hydrophobically modified CNF nanofibers are obtained by using lignin-based CNF nanofibers as raw materials and then performing hydrophobic modification treatment.

[0024] It should be noted that "CNF nanofibers" refers to cellulose nanofibers. Hydrophobically modified CNF nanofibers refer to hydrophobically modified cellulose nanofibers.

[0025] In an exemplary embodiment, the hydrophobically modified CNF nanofibers are hydrophobically modified high-purity wood-based CNF nanofibers. The preparation process of the hydrophobically modified CNF nanofibers may include: providing high-purity electronic-grade refined wood pulp board; purifying the high-purity electronic-grade refined wood pulp board to obtain purified pulp; dissociating the purified pulp to obtain wood-based CNF aqueous filter cake; using electronic-grade anhydrous ethanol as a solvent replacement medium to replace the wood-based CNF aqueous filter cake to eliminate free water inside the fiber and hydrophilic residual groups on the surface, to obtain wood-based CNF ethanol gel; hydrolyzing and activating an alkylsilane modifier to obtain a modifier; adding the modifier to the wood-based CNF ethanol gel, and uniformly grafting hydrophobic alkyl functional groups onto the surface of the cellulose fiber through a controllable covalent grafting reaction to completely eliminate the fiber's native hydrophilic hydroxyl groups, to obtain hydrophobically modified nanofibers; and purifying the hydrophobically modified nanofibers to obtain hydrophobically modified CNF nanofibers.

[0026] Specifically, it includes the following steps: Step 1: Standardized preparation of electronic-grade lignocellulosic CNF hydrogels Supporting equipment: raw material dispersing and purification machine, high-pressure homogenizing nano-dissociation machine, precision vacuum filter cake forming machine.

[0027] Operating Procedures and Precise Parameters: High-purity electronic-grade refined wood pulp board is selected as the base raw material. It is fed into a raw material dispersing and purification machine to complete multi-stage wet purification, thoroughly removing residual lignin, hemicellulose, and solid mechanical impurities from the raw material. The purified uniform pulp is sent to a high-pressure homogenizing nano-dissociation machine, with a constant dissociation pressure of 80MPa~100MPa, and continuous dissociation is performed 3~5 times. After dissociation, a wood-based CNF aqueous filter cake with uniform texture, no lumps, and no coarse fiber defects is prepared by a precision vacuum filter cake forming machine. The fiber aspect ratio of the finished product is stably controlled at 500~800, and the parameter deviation of a single batch of products is ≤±5%, ensuring the consistency of raw material batches.

[0028] Step 2: Multi-stage negative pressure anhydrous solvent replacement for water removal Supporting equipment: constant temperature negative pressure displacement reactor, precision material lifting and impregnation machine.

[0029] Operating procedures and precise parameters: Electronic-grade anhydrous ethanol is used as the solvent replacement medium. The prepared CNF aqueous filter cake is placed in a constant-temperature negative-pressure replacement reactor. The entire process is carried out in a closed negative-pressure environment with a constant negative pressure parameter of -0.06MPa to -0.08MPa. The soaking time for each immersion is fixed at 20min to 50min, and 3 to 5 replacement processes are completed continuously to completely eliminate free water inside the fiber and hydrophilic residual groups on the surface. Through multi-stage precise solvent replacement, a highly dispersible lignocellulosic CNF ethanol gel without hydrophilic residue is prepared, which provides a core guarantee for the uniformity and stability of the subsequent hydrophobic grafting reaction.

[0030] Step 3: Isothermal covalent hydrophobic grafting modification Supporting equipment: intelligent constant temperature stirring reactor, precise micro-feeding machine for additives, and integrated ultrasonic activation machine.

[0031] Operating Procedures and Precise Parameters: The alkylsilane modifier is pre-activated using an integrated ultrasonic activation machine for a fixed activation time of 20-50 minutes. The modifier is then quantitatively added using a precise micro-feeder, with the amount added being 8%-12% of the CNF dry basis mass. The reaction vessel system is kept at a constant temperature of 323.15K-333.15K, with a constant mechanical stirring speed of 300-500 rpm, and the reaction is continued at this constant temperature for 120-180 minutes. Through a controlled covalent grafting reaction, hydrophobic alkyl functional groups are uniformly grafted onto the surface of the cellulose fibers, completely eliminating the fiber's native hydrophilic hydroxyl groups and solving the problem of moisture adsorption in the substrate from the source.

[0032] Step 4: High-speed centrifugal washing and purification and preparation of dual-form finished products Supporting equipment: high-speed refrigerated centrifuge, vacuum low-temperature drying oven, and dust-free material dispensing equipment.

[0033] Operating Procedures and Precise Parameters: After the hydrophobic modification reaction is completed, electronic-grade anhydrous ethanol is used as the washing medium. Multi-stage centrifugation purification is carried out using a high-speed refrigerated centrifuge at a constant speed of 8000 r / min to 10000 r / min, with each centrifugation lasting 10 to 20 minutes. This centrifugation and washing process is repeated 2 to 5 times to completely remove unreacted modifiers and reaction byproducts, eliminating trace impurities. Two standardized finished product preparation paths are established after purification: one is a liquid product, directly packaged in a dust-free environment to obtain a hydrophobic modified CNF ethanol dispersion, which can be directly used for coating slurry preparation; the other is a powder product, where the purified CNF ethanol gel is placed in a vacuum low-temperature drying oven, set to a drying temperature of 313.15 K and a vacuum degree of -0.09 MPa, and dried at a constant temperature until the material reaches constant weight, yielding high-purity hydrophobic modified CNF nanofiber powder. The entire process is completed in a Class 10,000 cleanroom environment, effectively avoiding dust and moisture contamination and ensuring product performance stability.

[0034] After hydrophobic modification, the hydrophobically modified CNF nanofibers possess the following properties: 1) The modification process can completely eliminate the hydrophilic active groups on the surface of cellulose fibers, breaking through the industry's technical prejudice that "CNF materials are not suitable for modifying low-dielectric glass fibers," and effectively avoiding the inherent technical defects of conventional hydrophilic fillers that are prone to moisture absorption and cause increased dielectric loss; 2) The CNF nanofibers after the process have excellent dispersion uniformity, without agglomeration or sedimentation problems, and can be precisely adapted to the precision coating mass production process of gradient step feeding and high-speed dispersion in this application, ensuring uniform and stable performance of batch slurry systems; 3) The modified CNF fibers have nano-ultrafine particle size and ultra-high aspect ratio structural characteristics, which can accurately fill the micropores of glass fiber substrates, simultaneously achieving the dual technical effects of physical pore sealing and chemical interface hydrophobic modification, which is the core support for the product's low dielectric and high resistance to humid heat performance.

[0035] This application uses high-purity specialty dissolved wood pulp as the sole raw material. This raw material is a benchmark high-purity substrate in the international high-end electronic insulation, optoelectronic display, and precision functional composite material fields. It meets high-end electronic-grade exclusive quality control standards, including ultra-high cellulose purity of up to 98%, ultra-low ash impurities of ≤0.5%, controllable uniform polymerization degree of DP300~1200, and trace metal ion residues. It can suppress ion conduction loss and dipole relaxation loss from the source, and completely avoid the high-frequency dielectric performance degradation problems caused by impurity enrichment and high hydrophilic residues in ordinary industrial wood pulp and textile-grade dissolved pulp. This application is equipped with multi-stage impurity removal and purification, precise temperature-controlled covalent grafting, and dust-free closed purification and drying processes, which are refined and controllable exclusive processes. It can stably prepare high-purity, highly hydrophobic, and highly dispersible modified CNF functional fillers in batches, breaking through the long-standing technical prejudice and bottleneck in the industry that "conventional CNF is hydrophilic and hygroscopic, rich in impurities, and easily causes increased dielectric loss, making it unsuitable for high-end low-dielectric glass fiber modification." Studies have shown that by precisely controlling the surface functional groups of CNFs through covalent hydrophobic grafting modification, eliminating hydrophilic active sites, and optimizing interfacial fiber interactions, the dielectric constant and dielectric loss in the 10–40 GHz ultra-high frequency band can be significantly reduced, and dielectric parameter drift under humid and hot environments can be greatly mitigated. It is evident that this exclusive high-end raw material selection and customized complete process are deeply coupled and synergistically enhanced. From the raw material end, it completely eliminates dielectric polarization interference and high-frequency signal attenuation caused by impurities; from the process end, it eradicates the inherent hydrophilic and hygroscopic defects of cellulose. This dual closed-loop system ensures the product's core performance characteristics of low dielectric constant, low loss, high resistance to humid heat, and high dimensional stability.

[0036] After the fiberglass substrate is woven, a large number of micron- and submicron-sized interconnected pores naturally exist on the surface and inside the substrate. These pore structures easily trap air and adsorb environmental moisture. Air has a dielectric constant of approximately 1.0, while water molecules have a dielectric constant as high as 80. These two factors are the core causes of high-frequency polarization loss and unstable dielectric parameters in fiberglass electronic fabrics. Related technologies only focus on optimizing the fiberglass yarn formulation, which can only improve the inherent properties of the glass itself and cannot eliminate the microscopic pore defects introduced by the weaving process, thus failing to fundamentally solve the dielectric drift problem. This application uses hydrophobically modified CNF nanofibers. With their nanoscale ultrafine size and ultra-high aspect ratio, these nanofibers can precisely penetrate, fill, and seal the micropores of the fiberglass substrate, completely replacing the original air and moisture adsorption sites within the pores. Through a combination of physical pore sealing and chemical hydrophobic modification, the high-loss "glass fiber-pore-air-water vapor" microstructure in related technologies is reconstructed into a dense, low-polarization, and highly stable nanofiber composite structure. This significantly reduces the overall dielectric constant and high-frequency dielectric loss of the composite material at the physical structural level. Specifically, this application uses glass fiber substrate as the matrix and hydrophobically modified CNF nanofibers as the core functional filler. The hydrophobically modified CNF nanofibers can seal pores, suppress moisture, and reduce dielectric loss. The silane coupling agent can perform interfacial crosslinking, enhancing the bonding force between the coating and the glass fiber and sealing the hydrophilic groups of the substrate. The crosslinking aid can improve the crosslinking density, structural stability, and weather resistance of the coating. The organic solvent can disperse the medium, ensuring no impurity contamination and guaranteeing low dielectric insulation performance. Therefore, the above formulation can eliminate hydrophilic groups in the fibers, precisely fill the micropores of the glass fiber, reduce the surface polarity of the matrix, and fundamentally suppress water vapor adsorption and high-frequency polarization loss. This solves the core defect of damp heat dielectric drift in related technologies, achieving a comprehensive performance improvement in glass fiber electronic cloth, characterized by low loss, high resistance to damp heat, and high dimensional stability. Experimental verification shows that this glass fiber electronic cloth possesses low dielectric constant, low loss, and high resistance to damp heat, with a dielectric constant of 3.0–3.2, dielectric loss ≤0.008, moisture content ≤0.3%, overall dimensional thermal deformation rate ≤0.08%, dielectric performance degradation rate ≤3% under high and low temperature alternating damp heat environment, and insulation resistance ≥1×10¹. 4 Ω exhibits excellent high-frequency electrical stability and weather resistance.

[0037] In one optional embodiment, the fiberglass base fabric is an alkali-free fiberglass cloth. More specifically, the alkali-free fiberglass cloth is an E6 alkali-free fiberglass base fabric. This E6 alkali-free fiberglass base fabric is an electronic-grade precision plain weave base fabric, with a smooth, undamaged, stain-free, and crease-free surface. The base fabric undergoes high-temperature desizing pretreatment to remove surface sizing and oil impurities, with a residual sizing content ≤0.1%. The fabric surface tension is uniform and stable, providing a clean and smooth substrate interface for the uniform lamination of nano-functional coatings.

[0038] Optionally, the thickness of the fiberglass base fabric ranges from 0.08mm to 0.20mm. Preferred mass-production specifications are standard electronic-grade fiberglass fabrics of 0.10mm, 0.14mm, and 0.17mm. This thickness range perfectly balances the mechanical support performance of the substrate, the uniformity of the coating layer, and the stability of high-frequency signal transmission: too low a thickness can easily lead to fabric surface tension deformation and reduced forming flatness; too high a thickness can easily cause residual micropores inside the matrix, which cannot be completely sealed, thus affecting the dielectric uniformity and high-frequency stability of the product.

[0039] In an optional embodiment, the organic solvent is electronic-grade anhydrous ethanol. Using electronic-grade anhydrous ethanol as the dispersion medium results in low levels of moisture, metal ions, and evaporation residue. This not only stably disperses the hydrophobically modified lignin-based CNF and prevents nanofiber aggregation, but also prevents the introduction of conductive impurities, ensuring the coating's low dielectric constant, low dielectric loss, and insulating properties. Furthermore, the absence of residue defects after curing improves the coating's film uniformity and long-term humid heat stability.

[0040] In an optional embodiment, the thickness of the nanofiber low-dielectric functional coating is 3 × 10⁻⁶. -6 m~8×10 -6 m, coating thickness uniformity deviation ≤ ±0.5×10 -6 m. By controlling the thickness and uniformity deviation of the low dielectric functional coating of the nanofiber, the prepared glass fiber electronic cloth is free of pinholes, bubbles, and particle agglomeration defects, and the coating is tightly bonded to the glass fiber substrate without delamination.

[0041] This application also provides a method for preparing glass fiber electronic cloth. Figure 1 This is a schematic flowchart illustrating an exemplary embodiment of the preparation method of a fiberglass-free electronic cloth, as shown in this application. Figure 1 As shown, the preparation method of this glass fiber electronic cloth includes: S1. Provide fiberglass base fabric.

[0042] Optionally, the fiberglass base fabric is alkali-free fiberglass cloth. More specifically, the alkali-free fiberglass cloth is E6 alkali-free fiberglass base fabric. The thickness of the fiberglass base fabric ranges from 0.08 mm to 0.20 mm. Preferably, mass-produced specifications are standard electronic-grade fiberglass cloths of 0.10 mm, 0.14 mm, and 0.17 mm.

[0043] Optionally, the fiberglass base fabric can be pre-treated before dispersion and vacuum degassing. Pre-treatment may include: using a pneumatic shaftless unwinder to unwind the E6 alkali-free fiberglass base fabric at a uniform speed, removing the slurry and oil impurities on the surface of the base fabric through a two-stage high-temperature desizing oven to complete the clean activation of the base fabric, and then transferring it in a dust-free and sealed manner for later use after cooling.

[0044] S2. The hydrophobically modified CNF nanofibers, silane coupling agent, crosslinking aid, and organic solvent are dispersed and vacuum degassed according to the mass ratio to obtain a low dielectric functional coating of nanofibers.

[0045] Optionally, in step S2, under a Class 10,000 cleanroom environment with constant temperature and humidity, an organic solvent, hydrophobically modified CNF nanofibers, silane coupling agent, and crosslinking aid can be added sequentially using a gradient step-by-step feeding process. After high-speed dispersion and vacuum degassing, a uniform, stable, non-agglomerated, and bubble-free low-dielectric functional coating slurry is obtained. The dispersion speed in the dispersion process is 800 r / min to 1200 r / min, and the dispersion time is 1500 s to 2100 s. The vacuum degassing negative pressure in the vacuum degassing process is -8 × 10⁻⁸. 4 Pa ~ -9×10 4 Pa, degassing time is 900s to 1200s.

[0046] The gradient step feeding process used in this application can effectively avoid the problems of CNF nanofiber agglomeration and premature failure of additives, and ensure uniform dispersion and stable storage of slurry.

[0047] S3. The nanofiber low dielectric functional coating is uniformly coated on one or both sides of the glass fiber base cloth to obtain the coated glass fiber cloth.

[0048] In this embodiment, a precision micro-groove coating machine with a width of 0.6m to 1.0m can be used, matched with a servo constant tension control system, to complete the uniform coating of the base fabric on one or both sides under uniform speed. The coating forming accuracy is ensured by air knife dust removal and online thickness measurement.

[0049] In an optional embodiment, in step S3, the coating speed of the coating machine is 5 m / min to 8 m / min, the coating constant tension is 20 N to 25 N, and the coating thickness deviation is ≤ ±0.5 × 10⁻⁶. -6 m. By controlling the coating speed, constant coating tension, and coating thickness deviation, the uniformity of coating formation and batch consistency can be ensured.

[0050] S4. The coated glass fiber cloth is subjected to explosion-proof curing treatment to obtain explosion-proof cured glass fiber cloth.

[0051] The embodiments of this application can adopt a three-stage gradient explosion-proof curing process, in which the coated semi-finished product is conveyed in a sealed manner to three independent temperature-controlled gradient explosion-proof ovens, and the low-temperature pre-baking, medium-temperature curing and high-temperature curing stages are completed in sequence. This completely eliminates the thermal stress generated by a single high-temperature curing, avoids coating pinholes, cracks and aging defects, and greatly improves the density of the coating and the stability of the interface bonding.

[0052] In one optional embodiment, the three-stage gradient explosion-proof curing process includes a pre-baking stage, a curing stage, and a ripening stage. The temperature of the pre-baking stage is 353.15K to 363.15K, and the pre-baking time is 40s to 60s; The curing stage has a temperature of 393.15K to 403.15K and a curing time of 80s to 100s. The temperature during the curing stage is 423.15K to 433.15K, and the curing time is 100s to 120s.

[0053] The total curing time for this three-stage gradient explosion-proof curing treatment is 220s to 280s.

[0054] S5. In the modified liquid, the glass fiber cloth after the explosion-proof curing treatment is subjected to silane interface hydrophobic crosslinking modification treatment to obtain glass fiber electronic cloth.

[0055] In this embodiment, during the silane interface hydrophobic crosslinking modification stage, the cured and shaped composite electronic cloth can be immersed in the modification liquid for treatment, and the hydrophobic crosslinking structure can be locked by hot air shaping, thereby strengthening the bonding force between the coating and the base cloth interface, sealing the micropores of the material, and reducing the moisture absorption rate of the product.

[0056] In an optional embodiment, the modifying liquid is a fluorinated silane anhydrous ethanol solution with a mass concentration of 2.0% to 3.5%, an impregnation temperature of 318.15K to 328.15K, an impregnation time of 30s to 50s, and hot air setting at 373.15K for 20s.

[0057] Because the surface of the glass fiber matrix is ​​covered with a large number of polar hydrophilic active groups of silanol groups (Si-OH), these groups have a strong water vapor adsorption capacity. The adsorbed water molecules undergo severe dipole polarization under the action of a high-frequency electric field, which is a key factor leading to the increase in dielectric loss and significant performance drift after the product undergoes humid heat aging. This application achieves long-term interface modification through the synergistic crosslinking reaction of silane coupling agent and hydrophobically modified CNF: on the one hand, the silane coupling agent can chemically bond with the silanol groups on the glass fiber surface to form stable Si-O-Si covalent bonds, completely sealing the hydrophilic active sites of the glass fiber matrix; on the other hand, the hydrophobically modified CNF nanofibers used in this application have had a large number of hydrophilic groups removed in advance. Combined with the interface hydrophobic shaping process, a continuous, dense, low-polarity hydrophobic protective interface can be constructed on the surface of the glass fiber cloth, which inhibits water vapor adsorption from a chemical level, effectively solving the defect of dielectric performance decay under humid heat conditions in related technologies, and significantly improving the product's humid heat resistance stability.

[0058] In an optional embodiment, after the explosion-proof cured glass fiber cloth undergoes silane interfacial hydrophobic crosslinking modification treatment, the method further includes: A constant tension slitting and winding machine is used to precisely slit and rewind the cross-linked modified glass fiber cloth. The constant tension slitting and winding machine has a fabric feeding speed of 6m / min to 10m / min, a slitting tension of 18N to 20N for thin coatings, a slitting tension of 22N to 24N for thick coatings, and a slitting accuracy of ±0.1×10⁻⁶. - ³m, with a winding pressure of 0.3MPa~0.5MPa.

[0059] The embodiments of this application, through precise slitting and winding processes, can avoid defects such as fabric deformation, wrinkles, and loose winding.

[0060] In an optional embodiment, after step S5, the method may further include: We conduct comprehensive performance testing and closed-loop quality control on finished products, implementing a three-tiered quality closed-loop control system of IQC / IPQC / FQC. Qualified products are packaged and stored, while unqualified products are isolated and disposed of, achieving closed-loop quality control throughout the entire process. This enables controllable process parameters, traceable quality issues, and compliant production processes, breaking through the industry bottleneck of traditional processes' inability to achieve stable mass production.

[0061] The IQC / IPQC / FQC may include: IQC (Incoming Quality Control) conducts comprehensive inspections on all raw and auxiliary materials, including E6 alkali-free fiberglass base fabric, modified CNF nanofibers, silane coupling agents, and crosslinking aids, upon receipt. This includes verifying the residual slurry rate, flatness, and tensile stability of the base fabric; testing the aspect ratio, dispersibility, and hydrophobic properties of CNF fibers; and checking the purity and moisture content of the additives. Non-conforming materials are directly returned, while conforming materials are documented and traced back to their source, thus preventing product performance issues caused by raw material defects from the outset.

[0062] IPQC process quality control: Online dynamic sampling inspection is implemented throughout the entire production process. The pretreatment process verifies the removal effect of residual slurry on the base fabric. The solution preparation process tests the uniformity and bubble-free state of the slurry. The coating process records film thickness data in real time. The curing process monitors the temperature of the temperature zone, the fabric feeding speed, and the equipment tension parameters. The modification and slitting processes sample the interface bonding status and fabric flatness. Deviations in process parameters are corrected in real time to achieve zero-defect dynamic control of the production process.

[0063] FQC Finished Product Quality Control: Each batch of finished products undergoes comprehensive performance testing, covering core indicators such as dielectric parameters, insulation performance, dimensional thermal stability, damp heat decay rate, moisture content, and film thickness uniformity. Test data is linked to the product batch traceability code. Qualified products are stored in a constant temperature and humidity warehouse after being vacuum-packed with anti-static agents. Unqualified products are included in the abnormal review process, achieving a closed-loop quality control across the entire chain.

[0064] In an optional embodiment, this application also provides a three-level hierarchical anomaly review mechanism: Level 1 Minor Anomaly: Slight deviation in production parameters that does not affect the core performance indicators of the product. Adjust process parameters immediately, register the anomaly in the logbook, and do not require shutdown. Continuously monitor the performance status of the subsequent products.

[0065] Level 2 General Abnormality: If local coating defects or small-scale product non-conformity occur, immediately stop the machine to investigate the cause of the fault, isolate the non-conforming products, and only resume production after rectification and verification. At the same time, update the process parameter standard library.

[0066] Level 3 Major Anomaly: The core dielectric, insulation, and weather resistance properties of the product fail to meet the standards, resulting in the entire batch being unqualified. A joint review will be conducted, the entire production line will be shut down to trace the source of the problem throughout the entire process, a special rectification plan and prevention mechanism will be issued, and mass production can only be restarted after acceptance. The abnormal data will be archived to prevent the recurrence of similar problems.

[0067] In one optional embodiment, the entire production process is equipped with standardized waste treatment technology, ensuring that waste gas, wastewater, and solid waste are treated in a compliant manner and that pollutants are discharged in compliance with standards, meeting the environmental compliance requirements for industrialization. For example, this compliant treatment includes: organic waste gas generated from coating and drying ovens, and dust-containing waste gas generated from the liquid preparation process, are collected by a gas collection system, pre-filtered, and purified by activated carbon adsorption before being discharged in compliance with standards; production wastewater is treated by sedimentation filtration and advanced oxidation processes, with some of the clean water being reused and the remainder being discharged in compliance with standards; production solid waste is strictly classified and stored, and then transferred and disposed of by compliant units. The entire process fully complies with the environmental emission standards of the electronics industry, meeting the requirements for industrialization environmental impact assessment and green production.

[0068] In an optional embodiment, the preparation method is carried out in a dust-free environment, for example, the entire production process is arranged in a Class 10,000 cleanroom with an ambient temperature of 295.15K to 299.15K and a relative humidity of 45% to 60%, which isolates the product from dust and water vapor pollution throughout the process and ensures stable product performance.

[0069] The purpose, principle, and beneficial effects of the embodiments of this application are explained below: I. Purpose of the Invention The purpose of this application is to overcome the technical shortcomings of related technologies, such as the inability of modified fiberglass electronic cloth yarn to solve problems like dielectric drift due to moisture and heat, deterioration of moisture absorption due to conventional nano-modification, poor coating density of traditional molding processes, and weak mass production stability. This application provides a fiberglass electronic cloth and its preparation method. Breaking through existing industry technical understanding, this application adopts a post-processing modification route of hydrophobic modified CNF nanofibers to seal pores, fundamentally solving the moisture absorption problem of the substrate. Matched with a segmented gradient curing precision molding process, it achieves a comprehensive performance improvement in electronic cloth, including low dielectric constant, low loss, high resistance to moisture and heat, and high dimensional stability. Simultaneously, it constructs a full-process quality control and environmentally friendly mass production system, realizing the standardized and large-scale industrial mass production of high-end low-dielectric fiberglass electronic cloth.

[0070] II. The embodiments of this application do not optimize the glass fiber matrix formulation. The principle and reaction mechanism of preparing highly uniform, low dielectric, low loss, high insulation, and highly resistant to damp heat modified glass fiber electronic cloth based on the original process are as follows: This application does not modify the fiberglass raw yarn matrix composition, nor does it rely on the development of new chemical raw materials. Instead, it utilizes a unique integrated finishing process involving microscopic pore reconstruction, interfacial chemical modification, gradient crosslinking film formation, and dust-free precision molding. Without altering the fiberglass raw yarn formulation, this process systematically reshapes the microscopic physical structure and interfacial chemical state of the fiberglass base fabric, fundamentally overcoming inherent defects in related technologies such as high dielectric constant, high high-frequency loss, performance drift in humid and hot environments, and poor product uniformity. The specific mechanism of action is as follows: 1) Microscopic pore sealing mechanism to achieve optimization of core performance with low dielectric and low loss.

[0071] After weaving, fiberglass electronic fabrics (such as E6 alkali-free fiberglass base fabric) naturally contain a large number of micron- and submicron-sized interconnected pores on the surface and inside the matrix. These pore structures easily trap air and absorb ambient moisture. Air has a dielectric constant of approximately 1.0, while water molecules have a dielectric constant as high as 80. These two factors are the core causes of high-frequency polarization loss and unstable dielectric parameters in fiberglass electronic fabrics. Related technologies only focus on optimizing the fiberglass yarn formulation, which can only improve the inherent properties of the glass itself and cannot eliminate the microscopic pore defects introduced by the weaving process, thus failing to fundamentally solve the dielectric drift problem.

[0072] This application employs hydrophobically modified CNF nanofibers (e.g., hydrophobically modified high-purity wood-based CNF nanofibers). Leveraging their nanoscale ultrafine size and ultra-high aspect ratio, these nanofibers can precisely penetrate, fill, and seal the micropores of the glass fiber substrate, completely replacing the original air and water vapor adsorption sites within the pores. This reconstructs the traditional high-loss "glass fiber-pore-air-water vapor" microstructure into a dense, low-polarization, and highly stable nanofiber composite structure, significantly reducing the overall dielectric constant and high-frequency dielectric loss of the composite material at the physical structure level.

[0073] 2) The hydrophobic modification mechanism at the interface fundamentally inhibits the drift of dielectric properties in humid and hot environments.

[0074] The surface of the glass fiber matrix is ​​covered with a large number of silanol (Si-OH) polar hydrophilic active groups. These groups have a strong water vapor adsorption capacity. The adsorbed water molecules undergo violent dipole polarization under the action of a high-frequency electric field, which is a key factor leading to the increase in dielectric loss and significant performance drift after the product has been aging in damp heat.

[0075] This application embodiment achieves long-term interface modification through the synergistic crosslinking reaction of silane coupling agent and hydrophobically modified CNF: on the one hand, the silane coupling agent can chemically bond with the silanol groups on the glass fiber surface to form stable Si-O-Si covalent bonds, completely sealing the hydrophilic active sites of the glass fiber matrix; on the other hand, the hydrophobically modified CNF nanofibers used in this application embodiment have had a large number of hydrophilic groups removed in advance, and with the interface hydrophobic shaping process, a continuous, dense, low-polarity hydrophobic protective interface can be constructed on the surface of the glass fiber cloth, inhibiting water vapor adsorption from a chemical level, effectively solving the industry pain point of dielectric performance degradation under humid and hot conditions in related technologies, and significantly improving the product's resistance to humid and hot conditions.

[0076] As can be seen, the embodiments of this application break the industry's inherent R&D thinking of "only improving the original yarn without repairing the interface pores" and create a unique dual modification mechanism of "precise sealing of nanoscale micropores + low polarity hydrophobic reconstruction of the interface". From the dual dimensions of physical structure repair and chemical interface modification, it fundamentally solves the long-standing industry technical problems of easy moisture absorption, high frequency dielectric drift and high dielectric loss of glass fiber substrate.

[0077] 3) The three-stage gradient curing and progressive cross-linking mechanism improves the product's density, uniformity, and insulation.

[0078] The relevant technologies generally adopt a single-temperature zone constant temperature curing process. The instantaneous and rapid evaporation of solvents can easily cause microscopic defects such as pinholes, micro-gaps, and internal stress concentration in the functional coating. This results in a loose coating structure, uneven cross-linking density, and weak interfacial bonding, ultimately manifesting as large fluctuations in the dielectric parameters of the product, poor structural stability, and insufficient resistance to damp heat.

[0079] This application abandons the traditional crude process of impregnation coating and single-temperature constant-temperature curing, and instead features a unique three-stage gradient explosion-proof curing process. It employs a zoned, progressive temperature-controlled molding mechanism: a low-temperature pre-baking zone slowly removes the coating solvent, avoiding pinholes and cracks caused by instantaneous evaporation; a medium-temperature constant-temperature zone precisely triggers the cross-linking reaction between nanofibers and silane coupling agents, ensuring uniform interfacial bonding; and a high-temperature curing zone completes the coating's densification and reinforcement, eliminating internal stress during molding. This process achieves highly consistent cross-linking density across the entire coating area, effectively improving coating density, interfacial bonding strength, product dimensional stability, and insulation performance.

[0080] 4) Precision micro-gravure coating combined with dust-free molding process ensures the uniformity of the entire product and batch consistency.

[0081] Traditional coarse coating processes such as dipping, spraying, and brushing generally suffer from uneven coating thickness, localized missed coatings, and material accumulation, resulting in poor overall product uniformity and large batch-to-batch dispersion. This application employs a precision micro-recessed coating process, enabling accurate, controllable, and uniform forming of micron-level ultrathin coatings. Simultaneously, it utilizes a Class 10,000 cleanroom environment with constant temperature and humidity to completely eliminate performance deviations caused by dust contamination, moisture intrusion, and temperature and humidity fluctuations, effectively ensuring the uniform performance of the modified fiberglass electronic cloth across its entire width and the stability of mass production batches.

[0082] In summary, the embodiments of this application differ from the single technical approach of optimizing only the glass fiber raw yarn in related technologies. By constructing a brand-new glass fiber finishing and modification technology system through micropore reconstruction, interface polarity modification, gradient cross-linking and densification molding, and dust-free precision mass production process, a leapfrog improvement in the performance of commercial raw materials is achieved without changing the glass fiber raw yarn formula.

[0083] III. Current Technological Advantages of Related Technologies 1) Originality in raw material application: Breaking through inherent technological biases in the industry It is widely known in the industry that hydrophilic CNFs have strong hygroscopic properties, which significantly deteriorate the high-frequency dielectric properties of glass fibers. Therefore, related technologies have developed a technical bias that "CNFs are not suitable for modifying low-dielectric glass fibers," completely rejecting the application of such materials in high-frequency dielectric substrates. This application's embodiments uniquely employ hydrophobically modified high-purity wood-based CNFs. Through a proprietary hydrophobic modification process, the hydrophilic defects are eliminated, while retaining the core advantages of nanofibers—ultra-high aspect ratio and precise pore sealing. This transforms a material generally considered unsuitable for chemical modification into a core functional raw material for low-dielectric modification, overcoming the cognitive limitations of related technologies.

[0084] 2) Originality of coating process: Solves the industry's defects in uniform forming of high-end electronic cloth. This application abandons the traditional rough forming processes such as dipping, spraying, and brushing, and pioneers a micro-concave ultra-thin precision coating process, which can accurately control the forming of 3μm to 8μm ultra-thin functional coatings with a full-width thickness deviation of ≤±0.5μm. It achieves high-precision uniform film formation without pinholes, agglomeration, or uneven thickness, effectively solving the industry problem of large-area uniform forming of high-end low-dielectric electronic cloth.

[0085] 3) Originality of curing process: The unique gradient molding mechanism eliminates microscopic defects in the molding process. This application presents a unique segmented gradient temperature-controlled curing mechanism that combines low-temperature pre-baking and solvent removal, mid-temperature precise cross-linking, and high-temperature curing and densification, distinguishing it from the single constant-temperature curing mode of related technologies. This mechanism avoids the defects of incomplete cross-linking and loose structure associated with low-temperature curing, while overcoming the problems of thermal stress concentration, coating cracking, and numerous pinholes caused by high-temperature instantaneous curing. It achieves highly cross-linked and dense coatings, strong interfacial bonding, and zero dimensional deformation of the product. The process mechanism is unique and innovative.

[0086] 4) Originality of the complete system: Integrated innovation, not just the superposition of individual processes. This application integrates a proprietary hydrophobic CNF modification system, precision micro-grooving coating, gradient explosion-proof curing, dust-free interface modification, and constant-tension continuous molding to form an integrated, complete industrial technology solution, rather than a simple superposition of individual processes. The overall technical architecture, modification logic, and molding system are all different from related technologies.

[0087] 5) Technical advantages of "customized formulation system for modified nanofibers + industrialized process for dust-free precision coating gradient molding": This application's embodiments achieve systematic technological innovation from both material formulation and production process dimensions through the synergistic adaptation of a customized nanofiber-specific formulation system with a dust-free precision gradient molding industrial process. This effectively solves the related technical performance shortcomings and mass production bottlenecks. The specific innovation logic and technological advantages are as follows: Innovation Logic of Modified Nanofiber Custom Formulation System: This application's embodiments are tailored to the specific needs of high-frequency, low-dielectric, high-humidity and heat-resistant, and high-insulation high-end electronic substrates, employing a customized, differentiated compound system that is completely distinct from general composite material formulations. It uses hydrophobically modified CNF nanofibers as the core functional phase, specifically responsible for sealing micropores, reducing high-frequency losses, and inhibiting moisture adsorption. A silane coupling agent serves as the interfacial crosslinking phase, achieving a high-strength bond between the coating and the glass fiber matrix while simultaneously sealing the matrix's hydrophilic active sites. A trace amount of crosslinking aid acts as a dense reinforcing phase, improving the coating's crosslinking density, structural stability, and weather resistance. Combined with an electronic-grade anhydrous ethanol high-purity solvent system, free of impurities and harmful fillers, it perfectly meets the stringent requirements of high-frequency precision electronic substrates. The precise synergy of each component, targeted to high-frequency operating conditions, effectively solves the defects of conventional formulations, such as high moisture absorption, weak crosslinking strength, and unstable dielectric properties.

[0088] The innovative logic of dust-free precision coating gradient molding industrial process: First, the Class 10,000 cleanroom environment with constant temperature and humidity completely eliminates microscopic performance defects caused by dust adsorption, moisture intrusion, and temperature and humidity fluctuations during production, ensuring the purity of the functional coating and the long-term stability of product performance. Second, servo constant tension closed-loop control combined with micro-concave precision coating technology achieves smooth fabrication and precise control of film thickness, enabling large-area, continuous preparation of uniform ultra-thin functional coatings, suitable for stable industrial mass production. Third, the three-stage gradient progressive cross-linking molding mode achieves slow solvent removal and gradual cross-linking and densification of the coating through segmented precise temperature control, maximizing the elimination of microscopic defects in molding and significantly improving coating density, interfacial bonding strength, and product dimensional stability.

[0089] Summary of overall technical advantages: The customized nano-formulation system in this application addresses the performance shortcomings of traditional modified materials, such as high moisture absorption, high loss, and poor stability. The dust-free precision gradient molding process overcomes the industrialization shortcomings of traditional mass production processes, such as poor uniformity, high defect rate, and large batch dispersion. The synergistic effect of these two technologies achieves comprehensive technical effects that are unattainable by related technologies, including low dielectric constant, low loss, high resistance to damp heat, high uniformity, and high mass production consistency.

[0090] IV. The embodiments of this application can achieve the following beneficial effects The modified route is differentiated, breaking through the industry's technical understanding and fundamentally solving the problem of dielectric drift under humid heat: The embodiments of this application use hydrophobically modified CNF nanofibers to replace the industry's conventional hydrophilic modified materials and original yarn modification schemes. Through the dual effects of physical pore sealing and chemical hydrophobic modification, the hydrophilic groups of the fiber are eliminated, the micropores of the glass fiber are precisely filled, the polarity of the matrix surface is reduced, and the core pain point of moisture adsorption and high-frequency polarization loss is suppressed from the root. This solves the core pain point of dielectric drift under humid heat in related technologies, effectively solves the moisture absorption defects of glass fiber substrates, effectively suppresses high-frequency polarization loss, and the dielectric constant of the finished product is stably controlled at 3.0~3.2, the dielectric loss is ≤0.008, the performance degradation rate after humid heat aging is significantly reduced, and the high-frequency electrical stability is significantly better than existing products.

[0091] Gradient curing process eliminates molding defects and improves product structural stability: The three-stage gradient independent temperature-controlled curing process, through the segmented temperature control mechanism of low-temperature desolventizing, medium-temperature crosslinking, and high-temperature curing, achieves slow solvent evaporation and gradual crosslinking and densification of the coating, completely eliminating the thermal stress generated by single high-temperature curing. It avoids the micropores and thermal stress concentration problems caused by the rapid evaporation of solvents in traditional single-temperature curing, greatly improving the density of the coating and the stability of the interface bonding. The product's dimensional thermal deformation rate is ≤0.08%, and the structural stability and resistance to damp heat are greatly improved.

[0092] Precision coating and dust-free production ensure high batch performance consistency: Micro-gravure precision coating enables micron-level precise film control, with coating thickness uniformity deviation ≤ ±0.5×10⁻⁶. -6 m, combined with a Class 10,000 cleanroom with constant temperature and humidity, eliminates performance deviations caused by environmental impurities and temperature and humidity fluctuations, solves the defects of large product dispersion and significant performance fluctuations in traditional processes, and meets the consistency requirements of high-end electronic substrates.

[0093] Interface crosslinking modification enhances hydrophobic properties and extends product service life: A stable Si-O-Si covalent bond structure is formed through silane interface crosslinking reaction, which completely covers the hydrophilic sites of the substrate and constructs a dense hydrophobic protective interface. This significantly improves the performance stability of the product under high and low temperature alternation and long-term humid and hot aging conditions, making it suitable for harsh industrial application scenarios.

[0094] A comprehensive quality control system enables stable industrial mass production: A three-level closed-loop quality control mechanism of IQC / IPQC / FQC is constructed to achieve full parameter controllability, traceability, and real-time correction of raw material entry, production process, and finished product exit. This effectively solves the mass production problems of large batch dispersion and unstable performance of traditional modified products, and realizes the standardized and stable mass production of high-end modified fiberglass electronic cloth.

[0095] Green and compliant production, adapted to the development requirements of high-end industries: This application has a complete set of waste gas, wastewater and solid waste classification and treatment processes, which realizes green and pollution-free production process and pollutant discharge in compliance with standards. It solves the shortcomings of traditional fine modification processes, such as poor environmental performance and difficulty in large-scale production, and forms a complete set of independent technology system that can be directly promoted for industrialization and has complete compliance.

[0096] This application also provides a series of embodiments to further verify the implementation effect of the glass fiber electronic cloth and its preparation method in this application. The implementation effect of the technical solution of this application will be described in detail below with reference to specific embodiments.

[0097] Example 1: The production environment is a Class 10,000 cleanroom with a constant temperature of 297.15K and a relative humidity of 50%. Qualified E6 alkali-free fiberglass base fabric is selected and pretreated with high-temperature desizing to remove surface residue and oil.

[0098] The proportions of each raw material are as follows: 2.2 wt% modified CNF nanofibers, 1.1 wt% silane coupling agent, 0.45 wt% crosslinking aid, and 96.25 wt% electronic grade anhydrous ethanol.

[0099] A gradient stepwise feeding process was adopted, in which organic solvent, hydrophobically modified CNF nanofibers, silane coupling agent, and crosslinking aid were dispersed and vacuum degassed sequentially according to the mass ratio. High-speed dispersion was performed for 1800 s, and the vacuum degassing negative pressure was -8.5 × 10⁻⁶. 4 Pa, vacuum degassing for 1080s, to prepare a uniform and defect-free functional slurry.

[0100] Using a 0.8m microgravure coating machine, the nanofiber low-dielectric functional coating was uniformly coated on one side of the glass fiber substrate at a feeding speed of 6m / min and a constant tension of 22N, controlling the dry film thickness to 5×10. -6 m.

[0101] The coated fiberglass cloth was sent into a three-stage gradient explosion-proof oven and pre-baked at 358.15K for 50 seconds, cured at 398.15K for 90 seconds, and aged at 428.15K for 110 seconds in sequence. The temperature difference between each zone was controlled within ±2K.

[0102] The explosion-proof cured glass fiber cloth was subjected to silane interface hydrophobic crosslinking modification treatment using a 3.0% (w / w) fluorinated silane modification solution. The impregnation temperature was 323.15K, the constant temperature impregnation time was 40s, and the interface modification was completed by hot air setting at 373.15K for 20s.

[0103] After being precisely slit and wound under constant tension, the finished product undergoes full performance testing.

[0104] Testing revealed that the finished fiberglass electronic cloth of this embodiment has a dielectric constant of 3.12, a dielectric loss of 0.0072, and an insulation resistance of 1.2 × 10¹. 4 Ω, dimensional thermal deformation rate of 0.07%, dielectric performance decay rate of ≤2.8% after 2000h of damp heat aging, flat and defect-free fabric surface, uniform and stable performance, fully meeting the usage requirements of the core substrate of 5G high-frequency copper clad laminate.

[0105] Example 2: Control the dry film thickness of the coating to 3×10 -6 m, the equipment's fabric feeding speed is 5m / min, and the coating tension is 20N.

[0106] The three-stage curing temperature is finely adjusted to 355.15K for pre-baking, 395.15K for curing, and 425.15K for maturation. The curing time is taken as the lower limit: 40s for pre-baking, 80s for curing, and 100s for maturation.

[0107] The modified solution concentration was 2.0%, and the solution was immersed at a constant temperature of 318.15K for 30 seconds.

[0108] The remaining process parameters are completely consistent with those in Example 1.

[0109] Testing revealed that the coating of the finished fiberglass electronic cloth in this embodiment is ultra-thin and uniform, free from pinholes, bubbles, and agglomeration defects. The dielectric constant is 3.05, the dielectric loss is 0.0068, and the insulation resistance is 1.2 × 10¹. 4 With an Ω-shaped thermal deformation rate of 0.065% and a decay rate of 2.6% after 2000 hours of damp heat aging, the product boasts extremely high dimensional accuracy, making it suitable for high-end precision electronic insulation device manufacturing scenarios.

[0110] Example 3: Control the dry film thickness of the coating to 8×10 -6 m, equipment fabric feeding speed 8m / min, coating tension 24N, The three-stage curing temperature is finely adjusted to 363.15K for pre-baking, 403.15K for curing, and 433.15K for maturation. The curing time is set to the upper limit: 60s for pre-baking, 100s for curing, and 120s for maturation.

[0111] The modified solution was 3.5% concentrated and immersed at a constant temperature of 328.15K for 50 seconds.

[0112] The remaining process parameters are completely consistent with those in Example 1.

[0113] Testing revealed that the coating structure of the finished fiberglass electronic cloth in this embodiment exhibits significantly improved density, with a moisture absorption rate ≤0.25% and an insulation resistance of 1.15×10¹. 4 Ω, dimensional thermal deformation rate of 0.075%, damp heat aging attenuation rate of 2. % after 2000h, excellent high and low temperature alternating resistance, suitable for harsh working conditions such as automotive high-frequency electronics and outdoor communication substrates.

[0114] Example 4: The raw material ratio is taken as the minimum value of the process range: 1.5 wt% modified CNF nanofibers, 0.8 wt% silane coupling agent, 0.3 wt% crosslinking aid, and 97.4 wt% electronic grade anhydrous ethanol.

[0115] Process parameters: Coating thickness 3×10 -6 m, fabric speed is 5m / min, coating tension is 20N.

[0116] Curing parameters: 353.15K pre-baking for 40s, 393.15K curing for 80s, 423.15K ripening for 100s.

[0117] Modification parameters: 2.0% concentration of modification solution, immersion at 318.15K for 30s.

[0118] The properties of the finished fiberglass electronic cloth in this embodiment, as tested, are: dielectric constant 3.02, dielectric loss 0.0065, and insulation resistance 1.1×10¹. 4 Ω, dimensional thermal deformation rate 0.06%, damp heat decay rate 2.5% after 2000h.

[0119] This embodiment represents the optimal lower limit process for low dielectric properties in this application.

[0120] Example 5: The raw material ratio is taken as the maximum value of the process range: 3.0 wt% modified CNF nanofibers, 1.5 wt% silane coupling agent, 0.6 wt% crosslinking aid, and 94.9 wt% electronic grade anhydrous ethanol.

[0121] Process parameters: Coating thickness 8×10 -6 m, fabric speed 8m / min, coating tension 25N. Curing parameters: 363.15K pre-baking for 60s, 403.15K curing for 100s, 433.15K aging for 120s.

[0122] Modification parameters: 3.5% concentration of modification solution, immersion at 328.15K for 50 seconds.

[0123] The properties of the finished fiberglass electronic cloth in this embodiment, as tested, are as follows: dielectric constant 3.18, dielectric loss 0.0078, and insulation resistance 1.3 × 10¹. 4 With an Ω-coated surface area, a dimensional heat distortion rate of 0.08%, and a damp heat decay rate of 2.9% over 2000 hours, it possesses high density and high weather resistance, making it suitable for high-end industrial mass production needs.

[0124] Example 6: The equipment was set with a fabric feeding speed of 5m / min and a coating tension of 20N. The other raw material ratios, curing parameters, modification parameters, and production environment were completely consistent with those in Example 1.

[0125] The properties of the finished fiberglass electronic cloth in this embodiment, as tested, are as follows: dielectric constant 3.08, dielectric loss 0.0069, and insulation resistance 1.2 × 10¹. 4 Ω, dimensional thermal deformation rate of 0.065%, damp heat decay rate of 2.6% after 2000 hours, suitable for ultra-high precision small batch customized production.

[0126] Example 7: The equipment was set with a fabric feeding speed of 8m / min and a coating tension of 25N. The other raw material ratios, curing parameters, modification parameters, and production environment were completely consistent with those in Example 1.

[0127] The properties of the finished fiberglass electronic cloth in this embodiment, as tested, are as follows: dielectric constant 3.15, dielectric loss 0.0075, and insulation resistance 1.15 × 10¹. 4 The Ω-value has a dimensional thermal deformation rate of 0.075% and a damp heat attenuation rate of 2.8% after 2000 hours. It is suitable for large-scale high-speed mass production, and the product performance is stable with no significant fluctuations.

[0128] Comparative Example 1 (Traditional Modified Electronic Cloth) The same type of glass fiber electronic cloth was prepared by using a simple coating process with traditional inorganic fillers, without modified CNF nanofiber pore blocking, three-stage gradient curing, dust-free production and interface hydrophobic modification process.

[0129] Testing revealed that the finished fiberglass electronic cloth in this embodiment exhibited the following properties: dielectric constant of 3.65, dielectric loss of 0.015, and a performance degradation rate exceeding 12% after 500 hours of damp heat aging. The cloth surface was prone to defects such as particles, pinholes, and uneven thickness. The batch performance exhibited significant dispersion, and the electrical stability under high-frequency operating conditions was poor, failing to meet the standards for high-end high-frequency electronic substrates.

[0130] Comparative Example 2 (Ordinary hydrophilic CNF replacing modified hydrophobic CNF): Based on the standard process of Example 1, only the hydrophobically modified high-purity wood-based CNF nanofibers in this application are replaced with conventional unmodified hydrophilic cellulose nanofibers, while the other raw materials, processes, environment, and quality control systems are completely identical.

[0131] The performance of the finished fiberglass electronic cloth in this embodiment was tested and found to be as follows: dielectric constant of 3.48, dielectric loss of 0.0125, insulation resistance of 6.8×10¹³Ω, dimensional heat deformation rate of 0.13%, and damp heat attenuation rate of 8.6% after 2000 hours.

[0132] The results show that ordinary hydrophilic CNF contains a large number of hydrophilic groups, which cannot block the micropores of glass fiber and will aggravate water vapor adsorption, significantly increase high-frequency polarization loss, and greatly deteriorate insulation performance and dimensional stability, thus verifying the necessity of the core technology of hydrophobic modified CNF in this application.

[0133] Comparative Example 3 (the three-stage gradient curing was cancelled, and a single-temperature zone constant temperature curing was adopted). Based on the standard process of Example 1, the three-stage gradient temperature control curing mechanism was cancelled and replaced with 403.15K single-temperature zone constant temperature curing. The total curing time remained the same as in Example 1, and all other parameters remained completely unchanged.

[0134] The performance of the finished fiberglass electronic cloth in this embodiment was tested and found to be as follows: dielectric constant of 3.35, dielectric loss of 0.0102, insulation resistance of 8.5×10¹³ Ω, dimensional heat deformation rate of 0.11%, and damp heat attenuation rate of 6.3% after 2000 hours.

[0135] The results show that single-temperature high-temperature curing easily causes rapid solvent evaporation, resulting in microscopic pinholes and gaps, insufficient cross-linking density of the coating, and thermal stress concentration, leading to drift in the dielectric properties of the product and a decrease in dimensional stability, thus verifying the technical superiority of the gradient curing process of this invention.

[0136] Comparative Example 4 (replacing microgravure coating with traditional dip coating process): Based on the standard process of Example 1, the precision micro-groove coating process is eliminated, and the traditional full-area immersion coating process is adopted. There is no precise closed-loop control of film thickness, but the other raw materials, curing, modification and quality control parameters are completely consistent.

[0137] The performance of the finished fiberglass electronic cloth in this embodiment was tested and found to be as follows: dielectric constant of 3.29, dielectric loss of 0.0095, insulation resistance of 9.2×10¹³Ω, dimensional heat deformation rate of 0.095%, and damp heat attenuation rate of 4.8% after 2000 hours.

[0138] The results show that traditional impregnation coating cannot achieve micron-level uniform film formation. The coating thickness is uneven, local accumulation is prominent, the film density has large dispersion, and the high-frequency electrical performance is unstable, which cannot meet the requirements of high-end precision production.

[0139] Comparative Example 5 (Cancellation of the three-level quality closed-loop control system): Based on the standard process of Example 1, the raw materials, equipment, process, and environmental parameters remain completely unchanged. The three-level quality closed-loop control and anomaly review mechanism of IQC / IPQC / FQC are cancelled, and only simple sampling inspection of finished products is retained.

[0140] Testing revealed the following performance fluctuation ranges for the finished product batches: dielectric constant 3.10–3.32, dielectric loss 0.0070–0.0092, and insulation resistance 7.5 × 10¹³ Ω–1.2 × 10¹³ Ω. 4 Ω, dimensional thermal deformation rate 0.07%~0.10%, damp heat decay rate 2.8%~5.2% after 2000h.

[0141] The results show that the lack of full-process control can easily lead to the inability to correct process parameter deviations in a timely manner, resulting in significant differences in product batch performance, poor mass production stability, and the inability to achieve standardized industrial production.

[0142] It should be noted that the order of the embodiments described above is merely for descriptive purposes and does not represent the superiority or inferiority of the embodiments. Furthermore, specific embodiments have been described above. Other embodiments are within the scope of the appended claims. In some cases, the actions or steps described in the claims can be performed in a different order than that shown in the embodiments and still achieve the desired result. Additionally, the processes depicted in the drawings do not necessarily require a specific or sequential order to achieve the desired result. In some embodiments, multitasking and parallel processing are also possible or may be advantageous.

[0143] The various embodiments in this specification are described in a progressive manner. The same or similar parts between the various embodiments can be referred to each other. Each embodiment focuses on describing the differences from other embodiments.

[0144] It should be noted that all features described in the embodiments of this application (including technical features described in different embodiments) can be combined arbitrarily under reasonable circumstances, and the new technical solutions formed by the combination are all within the protection scope of the embodiments of this application. The above description is only some embodiments of the embodiments of this application and is not intended to limit the embodiments of this application. Those skilled in the art should understand that there will be various changes and improvements to the embodiments of this application, and any modifications, equivalent substitutions and improvements made in accordance with the embodiments of this application fall within the protection scope claimed by the embodiments of this application.

Claims

1. A type of fiberglass electronic cloth, characterized in that, The fiberglass electronic cloth comprises a fiberglass base cloth and a nanofiber low-dielectric functional coating, wherein the nanofiber low-dielectric functional coating is composited on one or both sides of the surface of the fiberglass base cloth. The nanofiber low-dielectric functional coating comprises the following raw materials by mass percentage: Hydrophobically modified CNF nanofibers: 1.5wt%~3.0wt%; Silane coupling agent: 0.8wt%~1.5wt%; Crosslinking aid: 0.3wt%~0.6wt% Organic solvents: 94.9 wt% to 97 wt%; The hydrophobically modified CNF nanofibers are obtained by using lignin-based CNF nanofibers as raw materials and then performing hydrophobic modification treatment.

2. The fiberglass electronic cloth according to claim 1, characterized in that, The fiberglass base fabric is alkali-free fiberglass cloth, the thickness of the fiberglass base fabric ranges from 0.08 mm to 0.20 mm, and the organic solvent is electronic grade anhydrous ethanol.

3. The fiberglass electronic cloth according to claim 1, characterized in that, The thickness of the nanofiber low-dielectric functional coating is 3×10⁻⁶. -6 m~8×10 -6 m.

4. A method for preparing a glass fiber electronic cloth as described in any one of claims 1 to 3, characterized in that, The preparation method includes: S1. Provide fiberglass base fabric; S2. The hydrophobically modified CNF nanofibers, silane coupling agent, crosslinking aid, and organic solvent are dispersed and vacuum degassed according to the mass ratio to obtain a low dielectric functional coating of nanofibers. S3. The nanofiber low dielectric functional coating is uniformly coated on one or both sides of the glass fiber base cloth to obtain the coated glass fiber cloth. S4. The coated glass fiber cloth is subjected to explosion-proof curing treatment to obtain explosion-proof cured glass fiber cloth; S5. In the modified liquid, the glass fiber cloth after the explosion-proof curing treatment is subjected to silane interface hydrophobic crosslinking modification treatment to obtain glass fiber electronic cloth.

5. The preparation method according to claim 4, characterized in that, In step S2, an organic solvent, hydrophobically modified CNF nanofibers, silane coupling agent, and crosslinking aid are sequentially added using a gradient step feeding process. The dispersion speed of the slurry in the dispersion treatment is 800 r / min to 1200 r / min, and the dispersion time is 1500 s to 2100 s; The vacuum degassing negative pressure during the vacuum degassing process is -8×10⁻⁸. 4 Pa ~ -9×10 4 Pa, degassing time is 900s to 1200s.

6. The preparation method according to claim 4, characterized in that, In step S3, the coating speed is 5 m / min to 8 m / min, the coating tension is 20 N to 25 N, and the coating thickness deviation is ≤ ±0.5 × 10⁻⁶. -6 m.

7. The preparation method according to claim 4, characterized in that, The explosion-proof curing treatment in step S4 is a three-stage gradient explosion-proof curing treatment, which includes a pre-baking stage, a curing stage, and a ripening stage. The temperature of the pre-baking stage is 353.15K to 363.15K, and the pre-baking time is 40s to 60s; The curing stage has a temperature of 393.15K to 403.15K and a curing time of 80s to 100s. The temperature during the curing stage is 423.15K to 433.15K, and the curing time is 100s to 120s.

8. The preparation method according to claim 4, characterized in that, In step S5, the modified liquid is a fluorinated silane anhydrous ethanol solution, the mass concentration of the modified liquid is 2.0% to 3.5%, the immersion temperature is 318.15K to 328.15K, and the immersion time is 30s to 50s.

9. The preparation method according to claim 4, characterized in that, After subjecting the explosion-proof cured glass fiber cloth to silane interfacial hydrophobic crosslinking modification treatment, the method further includes: A constant tension slitting and winding machine was used to slit and rewind the cross-linked modified glass fiber cloth under constant tension. The constant tension slitting and winding machine has a fabric feeding speed of 6m / min to 10m / min, a slitting tension of 18N to 20N for thin coatings, a slitting tension of 22N to 24N for thick coatings, and a slitting accuracy of ±0.1×10⁻⁶. - ³m, with a winding pressure of 0.3MPa~0.5MPa.

10. The preparation method according to claim 4, characterized in that, The preparation method is carried out in a dust-free environment with an ambient temperature of 295.15K to 299.15K and a relative humidity of 45% to 60%.