A method for preparing high-performance household paper from bamboo pulp and the product thereof
By using enzyme pretreatment and orderly addition of additives, the problems of thick and rigid bamboo pulp fiber walls and weak interfiber bonding were solved, achieving a synergistic improvement in the wet strength and softness of bamboo pulp tissue paper, thus meeting the performance requirements of high-end tissue paper.
Patent Information
- Application Number
- CN202611569409.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-12
- Publication Date
- 2026-11-17
AI Technical Summary
Bamboo pulp fiber has thick cell walls and high rigidity, and the natural bonding between fibers is weak, resulting in insufficient wet strength and poor softness of the paper, making it difficult to meet the requirements of wet strength, soft hand feel and liquid absorption performance for high-end household paper. At the same time, wet strength agents and softeners compete for adsorption sites on the fiber surface, resulting in low utilization and mutual cancellation of effects, making it difficult to achieve synergistic optimization of strength and softness.
Enzyme-assisted pulping is used to treat bamboo chemical pulp, increasing the fiber specific surface area and hydroxyl exposure. By adding PAE wet strength agent first and then polyoxyethylene ether/polydimethylsiloxane softener, a stable wet strength crosslinking network and lubricating layer are constructed, thereby achieving fiber morphology regulation and surface softening.
While maintaining the strength of the fiber itself, it improves the wet strength and softness of the paper, achieving a synergistic improvement in strength and softness, and providing an industrial paradigm for the high-value utilization of bamboo pulp resources.
Smart Images

Figure CN123108997A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of papermaking technology, specifically relating to a method for preparing high-performance household paper using bamboo chemical pulp as raw material, through enzyme-assisted pulping and the orderly addition and synergistic regulation of wet strength agents and softeners, as well as the product prepared by this method. Background Technology
[0002] The upgrading of consumer demand for household paper has placed higher demands on the wet strength, softness, and absorbency of paper. Bamboo pulp fiber, due to its renewable raw materials, short growth cycle, and good fiber stiffness, has become an important supplement to wood pulp; however, bamboo fiber has thick cell walls, high rigidity, and weak natural bonding between fibers, resulting in paper with generally insufficient wet strength and poor softness, which limits its application in the high-end household paper sector.
[0003] In papermaking wet-end chemistry, polyamide-epoxychloropropane resin (PAE) is the most widely used wet strength agent. Its molecules contain amide groups, epoxy groups, and positively charged nitrogen-containing heterocyclic butyronitrile groups. These can electrostatically adsorb and covalently crosslink with hydroxyl groups on the fiber surface through cationic groups, and self-crosslink during paper drying and curing to form a three-dimensional network, thus imparting wet structural stability to the paper. Polyoxyethylene ether / polydimethylsiloxane blended softeners, on the other hand, form hydrogen bonds between the ether bonds in the polyoxyethylene ether component and the hydroxyl groups on the fiber surface. Simultaneously, the hydrophobic long chains in the polydimethylsiloxane structure form a lubricating and isolating layer on the fiber surface, reducing the coefficient of friction between fibers and the density of hydrogen bonds, thereby improving the softness and feel of the paper. However, there is an inherent contradiction between the mechanisms by which wet strength agents enhance inter-fiber bonding and softeners weaken it. Simply adding them simultaneously often leads to competition for adsorption sites on the fiber surface, resulting in low utilization and mutually canceling effects, making it difficult to achieve synergistic optimization of strength and softness.
[0004] Regarding the order of additive addition, Chinese patent CN103243609A discloses a manufacturing method for household paper. The technical solution involves adding a softener first, followed by a wet strength agent. By adding the softener first, it allows the softener to preferentially occupy the fiber surface, and then adding the wet strength agent allows for more efficient adhesion and cross-linking on the already softened surface, thereby improving the utilization rate of the additives. However, this solution focuses on applications prioritizing softness. For household paper products that require priority in ensuring wet strength (such as kitchen paper towels and hand towels), adding the softener first will form a pre-coating layer on the fiber surface, hindering the effective contact and chemical cross-linking between PAE and the fiber hydroxyl groups, resulting in a significant reduction in wet strength enhancement efficiency. Furthermore, this patent does not limit the type of fiber raw material, does not specifically design for the high surface charge density and rigidity of bamboo pulp fibers, and does not involve enzyme-assisted pulping pretreatment.
[0005] In academic research, existing literature reports that adding wet strength agents before softeners to wood pulp systems improves both paper softness and wet strength. However, bamboo pulp fibers have thicker cell walls, higher rigidity, and significantly different surface charge densities compared to wood pulp. Therefore, the adsorption behavior of additives on the surface of bamboo pulp fibers and the optimal addition process cannot be simply deduced from wood pulp. Furthermore, the aforementioned literature does not address enzyme-assisted pulping steps, failing to solve the problem of thick, rigid bamboo pulp fibers and poor base paper softness. Additionally, Chinese patent CN118360812A discloses a method for preparing high-strength bamboo-based tissue paper, using 100% bamboo pulp and simultaneously adding wet strength agents and softeners, but does not specify the order of addition or incorporate enzyme pretreatment. Chinese patent CN104452429A discloses a flexible tissue paper and its production method, simultaneously adding multiple additives, but also does not address the control of the addition order.
[0006] It is evident that the existing technology has the following technical problems that need to be addressed: bamboo pulp fiber cell walls are relatively thick and rigid, resulting in weak natural bonding between fibers, insufficient wet strength and poor softness of the paper, making it difficult to meet the requirements of high-end household paper for wet strength, soft hand feel and liquid absorption performance; at the same time, there is an inherent contradiction between the mechanism by which wet strength agents enhance the bonding between fibers and softeners weaken the bonding between fibers. Simply adding them at the same time can easily lead to the two additives competing for adsorption sites on the fiber surface, resulting in low utilization and mutual cancellation of effects, making it difficult to achieve synergistic optimization of strength and softness. Summary of the Invention
[0007] The technical problem to be solved by this invention is to provide a method for preparing high-performance tissue paper from bamboo pulp and the product thereof. This method involves enzymatically beating bamboo chemical pulp to effectively improve fiber fibrillation and swelling, and increase the specific surface area and hydroxyl exposure of the fibers. Then, by adding PAE wet strength agent first and then adding polyoxyethylene ether / polydimethylsiloxane softener, PAE preferentially occupies key binding sites on the fiber surface and builds a stable wet strength crosslinking network. The softener is then distributed in non-critical areas to form a lubricating layer without excessively damaging the existing reinforcing structure. Through multi-level synergistic regulation of enzyme pretreatment and orderly addition of additives, the wet strength, dry strength and soft hand feel are simultaneously improved while maintaining the strength of the bamboo pulp fibers, providing an important guarantee for the high-value utilization of bamboo pulp resources.
[0008] This invention is implemented as follows: A method for preparing high-performance household paper from bamboo pulp includes the following steps: using bamboo chemical pulp as raw material, adding cellulase or hemicellulase to the pulp for enzyme pretreatment, with an enzyme dosage of 30-50 u / g (relative to oven-dry pulp mass); washing the pulp and beating it after enzyme pretreatment to obtain enzymatically catalyzed bamboo pulp; preparing the enzymatically catalyzed bamboo pulp into a fiber suspension with a mass concentration of 0.1%-0.5%, and dispersing it; under stirring conditions, first adding polyamide-epoxychloropropane resin (PAE) wet strength agent to the fiber suspension, stirring and mixing evenly, then adding polyoxyethylene ether / polydimethylsiloxane compound softener to the resulting mixed pulp, stirring and mixing evenly; subjecting the resulting pulp to papermaking, pressing, drying and aging to obtain bamboo pulp household paper.
[0009] Furthermore, when using cellulase pretreatment, the enzyme dosage is 40 u / g, the pH is 4.5~5.5, the temperature is 45~55℃, and the reaction time is 60~120 min; when using hemicellulase pretreatment, the enzyme dosage is 40 u / g, the pH is 4.5~5.5, the temperature is 45~55℃, and the reaction time is 120~180 min.
[0010] Furthermore, the pulping process results in a pulp beating degree of 30~35 °SR.
[0011] Furthermore, the amount of PAE wet strength agent added is 10~30 kg / t (relative to the oven-dry pulp mass).
[0012] Furthermore, the amount of PAE wet strength agent added is 15~25 kg / t.
[0013] Furthermore, the amount of the polyoxyethylene ether / polydimethylsiloxane compound softener added is 3~10 kg / t (relative to the oven-dry pulp mass).
[0014] Furthermore, the amount of the polyoxyethylene ether / polydimethylsiloxane compound softener added is 5~8 kg / t.
[0015] Furthermore, the stirring time after adding the PAE wet strength agent is 3~10 min, and the stirring speed is 300~350 r / min; the stirring time after adding the polyoxyethylene ether / polydimethylsiloxane compound softener is 3~10 min, and the stirring speed is 300~350 r / min.
[0016] Furthermore, a bamboo pulp tissue paper prepared according to the method for preparing high-performance tissue paper from bamboo pulp.
[0017] The present invention has the following advantages: First, addressing the issues of thick walls, high rigidity, and weak interfiber bonding in bamboo pulp, this invention pre-treats bamboo chemical pulp before beating using cellulase or hemicellulase. The enzymes' mild and selective hydrolysis of polysaccharide components on the fiber surface promotes fiber fibrillation and cell wall swelling, increasing the fiber specific surface area and surface hydroxyl exposure. This provides more effective binding sites for the subsequent adsorption and cross-linking of PAE wet strength agents, while also helping to weaken fiber rigidity and laying the foundation for improving paper softness.
[0018] Secondly, addressing the issue of competitive adsorption and mutual cancellation of effects between wet strength agents and softeners, this invention employs an ordered addition process: first adding PAE wet strength agent, then adding polyoxyethylene ether / polydimethylsiloxane softener (the traditional approach in the prior art is "softener first, then wet strength agent"). When PAE is added preferentially, the cationic groups in its molecules interact with the negatively charged hydroxyl groups on the fiber surface through electrostatic adsorption, preferentially occupying key binding sites on the fiber surface and constructing a stable fiber-PAE heterocrosslinking network. During paper drying, PAE molecules further undergo self-crosslinking, forming a stable multi-interaction network between fibers. The subsequently added softener is mainly distributed in areas of the fiber surface not occupied by PAE and outside the fiber cross-linking areas. Through hydrogen bonding adsorption of polyoxyethylene ether segments and lubrication of hydrophobic polydimethylsiloxane segments, it improves the frictional properties of the fiber surface, with a lower degree of damage to the established PAE reinforcement network, thereby improving paper softness while maintaining wet strength.
[0019] In summary, this invention creatively combines enzyme-assisted pulping, PAE preferential crosslinking enhancement, and subsequent surface regulation by softeners to form a multi-factor synergistic regulation pathway that integrates fiber morphology control, paper bonding enhancement, and surface softening treatment of bamboo chemical pulp. This method, while preserving the fiber's intrinsic strength, achieves a synergistic improvement in both wet paper strength and softness through gentle pretreatment with bio-enzymes and control over the adsorption sites and distribution of different additives on the fiber surface. This provides a replicable and scalable industrial paradigm for the high-value application of bamboo chemical pulp in the field of high-quality tissue paper. Attached Figure Description
[0020] The present invention will be further described below with reference to the accompanying drawings and embodiments.
[0021] Figure 1 The images shown are scanning electron microscope (SEM) images of the original bamboo fiber and the bamboo fiber treated with cellulase / hemicellulase and pulping in the embodiments of the present invention. In the images, a represents the original bamboo fiber, b represents the bamboo fiber treated with cellulase and pulping, and c represents the bamboo fiber treated with hemicellulase and pulping. Detailed Implementation
[0022] In one embodiment of the present invention, a method for preparing high-performance household paper from bamboo pulp includes: using bamboo chemical pulp as raw material, adding cellulase or hemicellulase to the pulp for enzyme pretreatment, with an enzyme dosage of 30-50 u / g (relative to the oven-dry pulp mass); washing the pulp after enzyme pretreatment and beating it to obtain bamboo pulp with a freeness of 30-35 °SR; preparing the obtained pulp into a fiber suspension with a mass concentration of 0.1%-0.5% and dispersing it; adding PAE wet strength agent to the fiber suspension under stirring conditions, with an addition amount of 10-30 kg / t (relative to the oven-dry pulp mass), and stirring to mix evenly; then adding polyoxyethylene ether / polydimethylsiloxane compound softener to the obtained mixed pulp, with an addition amount of 3-10 kg / t (relative to the oven-dry pulp mass), and stirring to mix evenly; and then performing papermaking and pressing on the obtained pulp, and drying and maturing it at 90-110 °C to obtain bamboo pulp household paper.
[0023] In some embodiments of the present invention, the cellulase pretreatment conditions are: enzyme dosage 40 u / g, pH 4.5-5.5, temperature 45-55 °C, and reaction time 60-120 min. In other embodiments of the present invention, the hemicellulase pretreatment conditions are: enzyme dosage 40 u / g, and reaction time 120-180 min. In some embodiments of the present invention, the amount of PAE wet strength agent added is 15-25 kg / t, preferably 20 kg / t. In other embodiments of the present invention, the amount of polyoxyethylene ether / polydimethylsiloxane compound softener added is 3-8 kg / t, preferably 5 kg / t. In some embodiments of the present invention, the stirring time after adding PAE wet strength agent is 5 min, and the stirring speed is 300-350 r / min; the stirring time after adding softener is 5 min, and the stirring speed is 300-350 r / min. In other embodiments of the present invention, the drying and curing temperature is 105 °C.
[0024] The following will be combined with the appendix Figure 1 The technical solution of the present invention will be clearly and completely described in detail with specific embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments used, unless otherwise specified, are all commercially available conventional products. Example 1
[0025] A method for preparing high-performance household paper from bamboo pulp includes the following steps: 1. Take bamboo chemical pulp and add cellulase (Shanghai Yuanye Biotechnology Co., Ltd., S10041) for pretreatment. The enzyme dosage is 40 u / g, pH 4.8, temperature 50 ℃, and reaction time is 90 min. After enzyme pretreatment, wash the pulp thoroughly and beat it to 30 °SR using a PFI mill to obtain enzyme-catalyzed bamboo pulp. 2. Prepare an enzyme-catalyzed bamboo pulp into a fiber suspension with a mass concentration of 0.2%, and use a standard fiber disintegrator to disperse the fibers for 4 minutes to ensure uniform fiber dispersion. 3. Under mechanical stirring conditions of 300 r / min, first add PAE wet strength agent (polyamide-epoxychloropropane resin) to the fiber suspension at a rate of 20 kg / t (relative to the oven-dry pulp mass) and stir for 5 min; then add polyoxyethylene ether / polydimethylsiloxane softener to the mixed pulp at a rate of 5 kg / t and stir for 5 min. 4. The above pulp is processed into paper, pressed, and dried to obtain bamboo pulp household paper.
[0026] The paper was tested and found to have a dry tensile index of 23.67 N·m / g, a wet tensile index of 1.57 N·m / g, an interlayer bond strength of 221.8 J / m², and a softness value of 356 mN. Example 2
[0027] A method for preparing high-performance household paper from bamboo pulp is identical to Example 1, except for the following differences: Cellulase is replaced with hemicellulase (Shanghai Yuanye Biotechnology Co., Ltd., S10044) for pretreatment, with an enzyme dosage of 40 u / g, a reaction time of 150 min, and beating to 30 °SR; all other conditions remain unchanged. The resulting paper exhibits a dry tensile index of 28.00 N·m / g, a wet tensile index of 1.44 N·m / g, an interlaminar bond strength of 182.7 J / m², and a softness value of 466 mN.
[0028] The morphology of the original bamboo fibers and the bamboo fibers after cellulase / hemicellulase treatment with pulping in Examples 1 and 2 above is shown in Figure 1. The water retention values of the original bamboo pulp samples and the enzymatically catalyzed bamboo pulp after cellulase / hemicellulase treatment in Examples 1 and 2 above are shown in the table below: Table 1. Water retention value of bamboo pulp fiber
[0029] It can be seen that the present invention pretreats bamboo chemical pulp with cellulase or hemicellulase before pulping, and promotes fiber fibrillation and cell wall swelling by utilizing the mild and selective hydrolysis of polysaccharide components on the fiber surface by enzymes, thereby increasing the specific surface area of the fiber and the exposure of surface hydroxyl groups. Example 3
[0030] A method for preparing high-performance household paper from bamboo pulp is identical to Example 1, except for the following differences: the PAE addition amount is adjusted to 15 kg / t. The resulting paper has a dry tensile index of 21.82 N·m / g, a wet tensile index of 1.43 N·m / g, an interlayer bond strength of 195.1 J / m², and a softness value of 332 mN. Example 4
[0031] A method for preparing high-performance household paper from bamboo pulp is identical to Example 1, except for the following differences: the PAE addition amount is adjusted to 25 kg / t. The resulting paper has a dry tensile index of 24.95 N·m / g, a wet tensile index of 1.68 N·m / g, an interlayer bond strength of 230.4 J / m², and a softness value of 403 mN. Example 5
[0032] A method for preparing high-performance household paper from bamboo pulp is identical to Example 1, except for the following differences: the amount of softener added is adjusted to 8 kg / t. The resulting paper has a dry tensile index of 20.14 N·m / g, a wet tensile index of 1.24 N·m / g, an interlayer bond strength of 178.9 J / m², and a softness value of 287 mN.
[0033] Comparative Example 1 A method for preparing bamboo pulp household paper is the same as in Example 1, except for the following differences: the order of addition is adjusted to first add polyoxyethylene ether / polydimethylsiloxane softener (5 kg / t), stir for 5 min, then add PAE wet strength agent (20 kg / t), stir for 5 min, and the other conditions remain unchanged.
[0034] The paper was tested and found to have a dry tensile index of 19.23 N·m / g, a wet tensile index of 1.29 N·m / g, an interlayer bond strength of 170.9 J / m², and a softness value of 322 mN.
[0035] Comparative Example 2 A method for preparing bamboo pulp household paper is identical to Example 1, except for the following differences: the addition of PAE wet strength agent is omitted, and only polyoxyethylene ether / polydimethylsiloxane softener (5 kg / t) is added, while other conditions remain unchanged. The resulting paper has a dry tensile index of 12.67 N·m / g, a wet tensile index of 0.22 N·m / g, an interlaminar bond strength of 160.7 J / m², and a softness value of 281 mN.
[0036] Comparative Example 3 A method for preparing bamboo pulp household paper is identical to Example 1, except for the following differences: the addition of softener is omitted, and only PAE wet strength agent (20 kg / t) is added, while other conditions remain unchanged. The resulting paper has a dry tensile index of 24.44 N·m / g, a wet tensile index of 1.64 N·m / g, an interlaminar bond strength of 253.6 J / m², and a softness value of 461 mN.
[0037] The above results indicate that the synergistic effect of enzyme pretreatment, PAE wet strength agent, softener, and the order of adding PAE followed by softener can improve paper softness while maintaining high dry and wet tensile strength, achieving a synergistic improvement in wet strength and soft hand feel.
[0038] While specific embodiments of the present invention have been described above, those skilled in the art should understand that the specific embodiments described are merely illustrative and not intended to limit the scope of the present invention. Equivalent modifications and variations made by those skilled in the art in accordance with the spirit of the present invention should be covered within the scope of protection of the claims of the present invention.
Claims
1. A method for preparing high-performance household paper from bamboo pulp, characterized in that: Includes the following steps: Using bamboo chemical pulp as raw material, cellulase or hemicellulase is added to the pulp for enzyme pretreatment. The enzyme dosage is 30~50 u / g relative to the oven-dry pulp mass. After enzyme pretreatment, the pulp is washed and beaten to obtain enzyme-catalyzed bamboo pulp. The enzyme-catalyzed bamboo pulp is prepared into a fiber suspension with a mass concentration of 0.1%~0.5% and then dispersed. Under stirring conditions, polyamide-epoxychloropropane resin (PAE) wet strength agent is first added to the fiber suspension and stirred until uniform. Then, polyoxyethylene ether / polydimethylsiloxane compound softener is added to the resulting mixed pulp and stirred until uniform. The resulting pulp is then subjected to papermaking, pressing, and drying to obtain bamboo pulp tissue paper.
2. The method for preparing high-performance household paper from bamboo pulp according to claim 1, characterized in that: When using cellulase pretreatment, the enzyme dosage is 40 u / g, the pH is 4.5~5.5, the temperature is 45~55 ℃, and the reaction time is 60~120 min; when using hemicellulase pretreatment, the enzyme dosage is 40 u / g, the pH is 4.5~5.5, the temperature is 45~55 ℃, and the reaction time is 120~180 min.
3. The method for preparing high-performance household paper from bamboo pulp according to claim 1, characterized in that: The pulping process achieves a pulping degree of 30~35 °SR.
4. The method for preparing high-performance household paper from bamboo pulp according to claim 1, characterized in that: The amount of PAE wet strength agent added is 10~30 kg / t relative to the oven-dry pulp quality.
5. The method for preparing high-performance household paper from bamboo pulp according to claim 4, characterized in that: The amount of PAE wet strength agent added is 15~25 kg / t.
6. The method for preparing high-performance household paper from bamboo pulp according to claim 1, characterized in that: The amount of the polyoxyethylene ether / polydimethylsiloxane compound softener added is 3~10 kg / t relative to the oven-dry pulp quality.
7. The method for preparing high-performance household paper from bamboo pulp according to claim 6, characterized in that: The amount of the polyoxyethylene ether / polydimethylsiloxane compound softener added is 5~8 kg / t.
8. The method for preparing high-performance household paper from bamboo pulp according to claim 1, characterized in that: The stirring time after adding the PAE wet strength agent is 3~10 min, and the stirring speed is 300~350 r / min; the stirring time after adding the polyoxyethylene ether / polydimethylsiloxane compound softener is 3~10 min, and the stirring speed is 300~350 r / min.
9. A bamboo pulp tissue paper prepared by a method for preparing high-performance tissue paper from bamboo pulp according to any one of claims 1 to 8.
Citation Information
Patent Citations
Manufacturing method of paper for daily use
CN103243609A
Super-soft super-tough household paper and production method thereof
CN104452429A
Manufacturing method of flame-retardant quartz fiber sealing rope