A modified insulating paper and its preparation method

By forming a coating layer of aramid polymer solution on the surface of insulating paper and removing metal chlorides, the problems of high cost and poor interface performance of aramid fiber insulating paperboard are solved, and the heat resistance and electrical performance stability are improved, making it suitable for ultra-high voltage power transmission and large-capacity power transformers.

CN123109002APending Publication Date: 2026-11-17中国电气装备集团科学技术研究院有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611050908.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-15
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In the existing technology, aramid fiber insulating paperboard or aramid modified natural fiber insulating paperboard has problems such as high cost, poor interface performance, strong protic acid process corrosion of equipment, and residual acid deterioration of insulation performance, making it difficult to meet the high-temperature use requirements of ultra-high voltage power transmission and large-capacity power transformers.

Method used

A composite solvent system consisting of amide polar solvents and metal chlorides is used to form a polymer solution of aramid on the surface of insulating paper. A coating layer is formed by drying, and the metal chlorides are removed by soaking or rinsing, thus achieving interfacial bonding between aramid and cellulose fibers and avoiding the use of strong protic acids.

Benefits of technology

It achieves low-cost improvement in heat resistance, ensures a strong interfacial bond between aramid and cellulose fibers, maintains the electrical properties and pore structure of the insulating paper, and meets the requirements of power equipment at higher temperature levels.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123109002A_ABST
    Figure CN123109002A_ABST
Patent Text Reader

Abstract

This specification provides a modified insulating paper and its preparation method. The method includes: performing a polycondensation reaction of an aromatic diamine monomer and an aromatic diacyl chloride monomer in a composite solvent comprising an amide polar solvent and a co-solvent to obtain an aramid polymerization solution; the co-solvent comprising a metal chloride; coating the aramid polymerization solution onto the surface of the insulating paper, such that the dry basis loading of the aramid is 2-10 wt%; subjecting the coated insulating paper to a first drying treatment to form a coating layer of aramid on the cellulose fiber surface of the insulating paper; soaking or rinsing the insulating paper after the first drying treatment to remove the metal chloride; and subjecting the insulating paper after removing the metal chloride to a second drying treatment to obtain the modified insulating paper.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the interdisciplinary field of papermaking technology and materials industry, and in particular to a modified insulating paper and its preparation method. Background Technology

[0002] With the rapid development of ultra-high voltage power transmission, large-capacity power transformers, and the new energy industry, natural fiber insulating paperboard, as a core material for turn insulation, interlayer insulation, and partition insulation, faces increasingly stringent requirements for performance indicators such as long-term heat resistance, thermal aging stability, and electrical breakdown strength. Conventional coniferous sulfate natural fiber insulating paperboard has a heat resistance rating of only Class A (105℃). Under long-term high-temperature conditions, it is prone to cellulose hydrolysis and thermal oxidative degradation, leading to a rapid decline in mechanical strength and insulation performance. This makes it unsuitable for use in high-temperature power equipment requiring Class F (155℃) or even Class H (180℃).

[0003] Currently, to improve the heat resistance of insulating paper, aramid fibers are typically produced using a wet papermaking process alone or mixed with natural fibers. However, this approach has significant drawbacks: aramid fibers themselves are expensive, and a large amount is required to achieve a significant modification effect; furthermore, the dissociation process of aramid fibers involves the use of strong protic acids, which are highly corrosive, placing stringent requirements on production equipment, and the residual acid radicals can also degrade the electrical properties of the insulating paper. Additionally, the strong chemical inertness and small specific surface area of ​​aramid fibers make interfacial bonding with cellulose fibers difficult, compromising the paper's performance.

[0004] There are currently no effective solutions to the problems of high cost and poor interface performance of aramid fiber insulating paperboard or aramid modified natural fiber insulating paperboard technology, as well as the defects of strong protic acid process corrosion of equipment and residual acid deterioration of insulation performance. Summary of the Invention

[0005] This specification provides a modified insulating paper and its preparation method to solve the problems of high cost, poor interface performance, strong protic acid process corrosion of equipment, and residual acid degradation of insulation performance in the existing aramid fiber insulating paperboard or aramid modified natural fiber insulating paperboard technologies.

[0006] To solve the above-mentioned technical problems, the first aspect of this specification provides a method for preparing modified insulating paper, comprising: In a composite solvent comprising an amide-based polar solvent and a co-solvent, an aromatic diamine monomer and an aromatic diacyl chloride monomer are subjected to a polycondensation reaction to obtain a polymerization solution for aramid fibers; the co-solvent comprises a metal chloride. The polymer solution of aramid is coated onto the surface of insulating paper, so that the dry basis loading of aramid is 2~10wt%; The coated insulating paper undergoes a first drying process to form a coating layer of aramid on the surface of the cellulose fibers of the insulating paper. The insulating paper after the first drying treatment is soaked or rinsed to remove metal chlorides; The insulating paper after removing metal chlorides is subjected to a second drying treatment to obtain modified insulating paper.

[0007] Furthermore, the amide polar solvent includes one or more of N,N-dimethylacetamide, N-methylpyrrolidone, and dimethylformamide; the metal chloride includes one or more of lithium chloride, calcium chloride, and zinc chloride.

[0008] Furthermore, the aromatic diamine monomer includes p-phenylenediamine, and the aromatic diacyl chloride monomer includes terephthaloyl chloride.

[0009] Furthermore, the molar ratio of the aromatic diamine monomer to the aromatic diacyl chloride monomer is 0.98:1 to 1.02:1.

[0010] Furthermore, the temperature of the polycondensation reaction is -5 to 5°C, and the reaction time is 0.5 to 3 hours; the solid content of the polymerization solution of the aramid is 2 to 20 wt%.

[0011] Furthermore, the coating includes single-sided coating and double-sided coating; in the double-sided coating, the dry basis loading of aramid on each side is 2~10wt%.

[0012] Furthermore, the temperature of the first drying treatment is 80~110℃, and the time is 10~25min; The first drying treatment of the coated insulating paper, which forms a coating layer of aramid on the surface of the cellulose fibers of the insulating paper, includes: The coated insulating paper is placed in a hot air oven for a first drying treatment, which causes the solvent in the aramid polymerization solution to evaporate. The solvent evaporation causes phase separation of the aramid on the surface of the cellulose fiber, forming a continuous coating layer. The molecular chain of the aramid includes amide groups, and the surface of the cellulose fiber includes hydroxyl groups. The coating layer is attached to the surface of the cellulose fiber through hydrogen bonds between the amide groups and the hydroxyl groups.

[0013] Further, the soaking or rinsing of the insulating paper after the first drying treatment to remove metal chlorides includes: The insulating paper after the first drying treatment was repeatedly soaked or rinsed with a displacement solvent to remove impurities from the aramid polymerization solution. The replacement solvent is water, ethanol, or a mixture of water and ethanol.

[0014] Furthermore, the temperature of the second drying treatment is 100~130℃, and the time is 10~60min; The second drying treatment of the insulating paper after removing metal chlorides yields modified insulating paper, comprising: The insulating paper after removing metal chlorides is dried by hot air or vacuum to remove the solvents introduced by soaking or rinsing.

[0015] Secondly, the embodiments of this specification also provide a modified insulating paper, which is prepared by the above-described method for preparing modified insulating paper.

[0016] As can be seen from the technical solutions provided in the embodiments of this specification above, the embodiments of this specification can prepare the polymerization solution of aramid by using a composite solvent system composed of amide polar solvents and metal chlorides, thus avoiding the defects of traditional strong protic acids in corroding equipment and acid residues degrading insulation performance. Furthermore, the polymerization solution is directly coated onto the surface of insulating paper and dried to form a coating layer, creating an interfacial bond between aramid and cellulose fibers. Modification can be achieved with a low loading of only 2-10 wt%, effectively controlling production costs. Impurities are removed by soaking or rinsing, ensuring the electrical purity of the product. In addition, the aramid coating layer gives the cellulose insulating paper higher heat resistance and thermal aging stability, enabling it to meet the requirements of higher temperature-rated power equipment, while the process is simplified and suitable for continuous production. Attached Figure Description

[0017] To more clearly illustrate the technical solutions in the embodiments or prior art of this specification, the drawings used in the description of the embodiments or prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in this specification. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0018] Figure 1 A schematic flowchart illustrating a method for preparing modified insulating paper provided in the embodiments of this specification; Figure 2 This is a schematic diagram of the overall process for preparing a modified insulating paper, as provided in the embodiments of this specification. Detailed Implementation

[0019] The technical solutions in the embodiments of this specification will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this specification, and not all embodiments. Based on the embodiments in this specification, all other embodiments obtained by those skilled in the art without creative effort should fall within the scope of protection of this specification.

[0020] It should be noted that the terms "first," "second," etc., used in this specification, claims, and the foregoing drawings are used to distinguish similar objects and are not necessarily used to describe a specific order or sequence. It should be understood that such data can be interchanged where appropriate so that the embodiments described herein can be implemented in orders other than those illustrated or described herein. Furthermore, the terms "comprising" and "having," and any variations thereof, are intended to cover a non-exclusive inclusion; for example, a process, method, apparatus, product, or device that comprises a series of steps or units is not necessarily limited to those steps or units explicitly listed, but may include other steps or units not explicitly listed or inherent to such processes, methods, products, or devices.

[0021] In existing technologies, to improve the heat resistance of natural fiber insulating paper, a method of mixing aramid fibers with natural fibers for papermaking is commonly used. This process involves dispersing chopped aramid fibers in an aqueous system, mixing them with softwood pulp fibers, and then wet-forming, pressing, and drying to produce composite insulating paper. The aramid fibers need to be pre-treated with strong protic acids (such as concentrated sulfuric acid or methanesulfonic acid) for dissolution or surface etching to improve their dispersibility in the aqueous phase and their interfacial bonding with cellulose fibers. However, this technical approach has many shortcomings: strong protic acids are highly corrosive, requiring extremely high-quality materials for production equipment, and the acid radicals are difficult to completely remove, leaving residues in the paper that significantly reduce the volume resistivity of the insulating paper and increase dielectric loss; aramid fibers are expensive, and to achieve a significant improvement in heat resistance, they typically need to be added at a rate of 10 wt%, making them uneconomical; more importantly, para-aramid fibers have a chemically inert surface and lack polar groups, resulting in a lack of strong chemical bonds between them and hydrophilic cellulose fibers rich in hydroxyl groups. The interface between the two relies solely on physical entanglement and limited van der Waals forces, making it prone to interfacial debonding under long-term thermal-mechanical combined action, leading to accelerated degradation of the mechanical strength and electrical properties of the insulating paper.

[0022] Meanwhile, aramid fibers have a small specific surface area, making it difficult to distribute evenly within the cellulose fiber network during papermaking, resulting in poor paper uniformity. Furthermore, after blending, aramid fibers easily clog the inherent micron-sized pore structure of natural cellulose paper, leading to a decrease in the porosity of the insulating paper and a significant reduction in oil absorption, affecting the impregnation and heat dissipation of insulating oil in oil-immersed transformers. In addition, in traditional wet papermaking processes, the large difference in sedimentation rates between aramid and cellulose fibers easily causes uneven component distribution in the Z-direction of the paper, further deteriorating the dielectric strength of the insulating paper. Therefore, existing hybrid papermaking technologies struggle to simultaneously achieve high heat resistance, excellent interfacial bonding strength, good electrical insulation properties, and a complete pore structure.

[0023] In addition, there have been attempts at post-treatment modification technology that uses aramid nanofiber suspension sprayed onto the surface of plant fiber paper. However, in this scheme, the aramid nanofibers are pre-made solid particles that can only be physically stacked on the fiber surface and cannot form a continuous molecular-level coating layer. The interface bonding is still mainly physical adhesion, and the coating is easy to peel off during long-term thermal aging, making it difficult to achieve a substantial leap in heat resistance level.

[0024] Therefore, there is an urgent need for a modification method that can achieve heat resistance modification of natural fiber insulating paper with low aramid addition without the use of strong protic acids, while ensuring that a strong interfacial bond is formed between the aramid component and the cellulose fiber, without damaging the original pore structure of the paper and maintaining excellent electrical insulation performance, so as to meet the increasingly demanding performance requirements of insulation materials for ultra-high voltage power transmission and large-capacity power transformers.

[0025] The modified insulating paper and its preparation method are described below with reference to the accompanying drawings.

[0026] See Figure 1 and Figure 2 As shown in the embodiments of this specification, a method for preparing modified insulating paper is provided. In specific implementation, this method may include the following: S101: In a composite solvent including an amide polar solvent and a co-solvent, an aromatic diamine monomer and an aromatic diacyl chloride monomer are subjected to a condensation reaction to obtain a polymerization solution for aramid; the co-solvent includes a metal chloride.

[0027] An amide-based polar solvent and a co-solvent constitute a composite solvent system. This system dissolves aromatic diamine monomers and aromatic diacyl chloride monomers and serves as a medium for the polycondensation reaction. The co-solvent contains a metal chloride, which disrupts the hydrogen bonds between aramid molecular chains in the composite solvent system, thereby improving the solubility of aramid in the composite solvent and the stability of the polymerization reaction. The aromatic diamine monomers and aromatic diacyl chloride monomers undergo a polycondensation reaction in the composite solvent system. This polycondensation reaction enables the monomers to form aramid molecular chains through an amidation reaction, yielding the aramid polymerization solution. Using this non-strong protic acid composite solvent system to prepare the aramid polymerization solution avoids the corrosion of production equipment by strong protic acids and the degradation of the electrical properties of insulating paper by residual acid radicals.

[0028] In some embodiments, the amide polar solvent includes one or more of N,N-dimethylacetamide, N-methylpyrrolidone, and dimethylformamide.

[0029] Amide polar solvents are used to dissolve aromatic diamine monomers, aromatic diacyl chloride monomers, and the resulting aramid polymers, serving as a homogeneous reaction medium for polycondensation reactions. These amide polar solvents are selected from one or more of N,N-dimethylacetamide, N-methylpyrrolidone, and dimethylformamide. Amide polar solvents possess high dipole moments and dielectric constants, effectively dissociating metal chlorides and promoting the dissolution of aromatic diamine monomers and aromatic diacyl chloride monomers, thus providing a homogeneous environment for the polycondensation reaction.

[0030] In some embodiments, the metal chloride includes one or more of lithium chloride, calcium chloride, and zinc chloride.

[0031] Metal chlorides are used to disrupt the hydrogen bonding interactions between aramid molecular chains, inhibiting premature precipitation and gelation of the polymer during the polycondensation reaction. The metal chlorides are selected from one or more of lithium chloride, calcium chloride, and zinc chloride. The metal cations in the metal chlorides can form coordinate bonds with the carbonyl oxygen atoms and amide nitrogen atoms on the aramid molecular chains, thereby weakening the hydrogen bonding forces between adjacent molecular chains and allowing the polymerization reaction to continue in a homogeneous system until the target molecular weight is reached.

[0032] In some embodiments, the molar ratio of aromatic diamine monomer to aromatic diacyl chloride monomer is 0.98:1 to 1.02:1.

[0033] The molar ratio of aromatic diamine monomer to aromatic diacyl chloride monomer is controlled within the range of 0.98:1 to 1.02:1. This molar ratio is used to characterize the stoichiometry of the polycondensation reaction. Controlling this stoichiometry within this range ensures that the reactive groups of the two monomers are essentially equivalent in the polycondensation reaction, resulting in a uniform degree of polymerization distribution and preventing premature termination of chain growth due to chain end capping caused by excess of any one component.

[0034] In some embodiments, the polycondensation reaction is carried out at a temperature of -5 to 5°C for 0.5 to 3 hours.

[0035] The temperature of the polycondensation reaction is controlled within the range of -5℃ to 5℃, and the reaction time is 0.5 hours to 3 hours. This reaction temperature is the low-temperature condition for initiating the polycondensation reaction and is used to suppress the occurrence of side reactions during the polycondensation process. The polycondensation reaction between aromatic diacyl chloride monomers and aromatic diamine monomers is an exothermic reaction. The low temperature condition can reduce the reaction rate, so that the chain growth process proceeds smoothly and avoids local overheating that could lead to polymer degradation or cross-linking. This reaction time is the range within which the polycondensation reaction continues, and is used to ensure that the monomer conversion rate reaches the target value.

[0036] In some embodiments, the solid content of the aramid polymerization solution is 2 to 20 wt%.

[0037] This solids content is used to characterize the percentage of the mass of aramid polymer in the aramid polymerization solution relative to the total mass of the polymerization solution. The solids content is controlled within this range to ensure that the polymerization solution has a viscosity and leveling properties suitable for coating operations.

[0038] In some embodiments, a co-solvent is dissolved in an amide-based polar solvent to obtain a mixture.

[0039] The dissolution process allows the metal chloride to fully dissociate into metal cations and chloride ions in an amide-based polar solvent, forming a homogeneous composite solvent system.

[0040] In some embodiments, the mixture is dehydrated so that the water content of the resulting composite solvent is ≤100ppm.

[0041] Dehydration is used to remove adsorbed water from the mixture and control the water content of the composite solvent within this range to avoid water from undergoing hydrolysis side reactions with aromatic diacyl chloride monomers, consuming acyl chloride groups and generating hydrochloric acid, which would lead to monomer imbalance and a decrease in polymer molecular weight.

[0042] In some embodiments, the polycondensation reaction is carried out under the protection of an inert gas.

[0043] Inert gas protection is used to isolate oxygen and moisture, preventing the aromatic diacyl chloride monomer from being hydrolyzed and deactivated by moisture in the air, while also preventing oxygen from reacting with the aromatic diamine monomer and causing it to deteriorate.

[0044] In some embodiments, during the polycondensation reaction, the aromatic diamine monomer is dissolved in a composite solvent and then the aromatic diacyl chloride monomer is added in batches.

[0045] In the polycondensation reaction, the aromatic diamine monomer is first dissolved in a composite solvent, and then the aromatic diacyl chloride monomer is added in batches. This batch addition method is used to control the instantaneous concentration of the aromatic diacyl chloride monomer in the polycondensation reaction system, so as to adjust the polycondensation reaction rate and avoid excessively vigorous reaction and local overheating caused by the one-time addition of the acyl chloride monomer.

[0046] In some embodiments, the reaction temperature is controlled to be ≤40°C during the batch addition of aromatic diacyl chloride monomer.

[0047] The polycondensation reaction between aromatic diacyl chloride monomers and aromatic diamine monomers has a significant exothermic effect. Controlling the reaction temperature to ≤40℃ is necessary to remove the heat of reaction in a timely manner and avoid local temperatures exceeding this range, which could lead to thermal degradation or cross-linking side reactions of the polymer.

[0048] In some embodiments, after the polycondensation reaction is completed, the reaction product is allowed to stand to degas, thereby obtaining the polymerization solution of aramid.

[0049] This static degassing process is used to allow air bubbles that are carried in by stirring during the polycondensation reaction to naturally rise to the surface of the liquid under the action of gravity and escape, thereby eliminating air bubble defects inside the polymerization solution.

[0050] In some embodiments, the standing degassing period is 24-48 hours.

[0051] The settling and degassing time is the time range required for the bubbles entrained in the polymerization solution to escape fully. If the degassing time is less than 24 hours, the bubbles will not escape sufficiently, and the residual bubbles inside the polymerization solution will form pinhole defects during subsequent coating and drying processes. If the degassing time exceeds 48 hours, the solvent in the polymerization solution may evaporate, leading to an increase in solid content. At the same time, the polymer may undergo slow physical cross-linking or intensified molecular chain entanglement, affecting the consistency of the coating operation.

[0052] S102: Coat the surface of insulating paper with the polymer solution of aramid, so that the dry basis loading of aramid is 2~10wt%.

[0053] Insulating paper is a sheet-like porous substrate formed from natural cellulose fibers through pulping, papermaking, pressing, and drying processes. Its fiber surface exposes a large number of free hydroxyl groups, which provide a physical adhesion interface and hydrogen bonding sites for the aramid coating layer. The aramid polymerization solution is a homogeneous liquid mixture containing aramid polymer, amide-based polar solvent, and metal chloride. The aramid polymer is dissolved in the composite solvent system in the form of molecular chains. The coating process allows the aramid polymerization solution to be uniformly spread as a liquid film on the surface of the insulating paper and in the gaps between the surface fibers. The dry-basis loading of aramid is used to characterize the percentage of the oven-dry mass of the aramid polymer finally attached to the insulating paper after coating and drying, relative to the total mass of the modified insulating paper. This loading is controlled between 2 wt% and 10 wt% based on a dual consideration of modification effect and cost control: when the loading is below 2 wt%, the coverage and continuity of the aramid polymer on the cellulose fiber surface are insufficient, making it difficult to form a complete heat-resistant barrier layer, and the effect on improving the heat resistance grade of the insulating paper is not significant; when the loading is above 10 wt%, further increasing the amount of aramid significantly weakens the marginal improvement effect on heat resistance performance, and... Excessively thick coatings increase the difficulty of removing residual solvents and salts through solvent replacement, and may also clog the inherent micron-sized pore structure of the insulating paper, leading to a decrease in oil absorption and oil immersion permeability. By controlling the loading amount within the range of 2wt% to 10wt%, the aramid polymer forms a continuous and moderately thick coating layer on the surface of the cellulose fibers, achieving a leap in heat resistance from Class A to Class F or H. At the same time, the porous structure and oil immersion properties of the insulating paper are maintained. In addition, the low loading amount also reduces the amount of aramid polymerization solution used and the workload of subsequent solvent replacement, thereby reducing material costs and process energy consumption.

[0054] In some embodiments, the insulating paper is pre-dried before coating.

[0055] Insulating paper absorbs moisture from the environment during storage and transportation, and its moisture content is usually in an equilibrium state. This moisture content affects the wetting, spreading, and penetration behavior of the subsequent polymerization solution on the surface of the insulating paper. Furthermore, the presence of moisture may vaporize during the subsequent drying process, forming bubble defects that adversely affect the integrity of the coating and the interfacial bonding strength. By proactively reducing the moisture content of the insulating paper through pre-drying treatment, the insulating paper is placed in a predictably low moisture content state before coating, thereby eliminating process uncertainties and coating defect risks caused by fluctuations in the substrate moisture content.

[0056] In some embodiments, the temperature conditions for the pre-drying treatment are 80°C to 110°C, and the treatment duration is 0.5 hours to 2 hours.

[0057] This temperature range is designed to balance the dual requirements of drying efficiency and substrate protection: below 80°C, the rate of moisture removal from the insulating paper is too low, making it difficult to reduce the moisture content to the target level within a reasonable time; above 110°C, natural cellulose insulating paper may experience irreversible strength loss or decreased dimensional stability under prolonged high-temperature treatment. This time range ensures that the moisture inside the insulating paper is fully removed without damaging the fiber structure, allowing the insulating paper to reach a stable low moisture content state before coating.

[0058] In some embodiments, the insulating paper is natural cellulose insulating paper with a basis weight of 60 g / m³. 2 Up to 120g / m 2 The thickness specifications range from 0.1mm to 0.3mm.

[0059] This basis weight range covers the standard specification range for softwood sulfate insulating paper, with a basis weight below 60 g / m³. 2 The mechanical strength of the insulating paper is insufficient to withstand the tension of subsequent coating, drying, and winding processes; the basis weight is higher than 120 g / m². 2 Excessive thickness of the insulating paper hinders the penetration and uniform distribution of the coating solution into the paper layer. This thickness range represents a typical thickness interval matching this basis weight range. When the thickness is less than 0.1 mm, the paper structure is too loose, allowing the coating solution to easily penetrate and cause leakage; when the thickness is greater than 0.3 mm, the paper structure is too dense, making it difficult for the coating solution to effectively adhere and penetrate the paper surface. Natural cellulose insulating paper possesses good hydrophilicity and a porous structure, with its fiber surface rich in hydroxyl groups. This fiber structure provides a physical adhesion interface and hydrogen bonding sites for the aramid coating layer.

[0060] In some embodiments, the coating method is single-sided coating or double-sided coating, and in double-sided coating, the dry basis loading of aramid on each side is independently 2wt% to 10wt%.

[0061] Single-sided coating is used to form an aramid coating layer on only one surface of the insulating paper, suitable for applications requiring single-sided heat resistance or surface strength. Double-sided coating is used to form an aramid coating layer independently on each of the two surfaces of the insulating paper, suitable for applications requiring heat resistance on both sides. In double-sided coating, the dry basis load on each side is independently controlled within a certain range. The loads on both sides can be the same or different, and are adjusted independently according to the functional requirements of each side and the coating process conditions.

[0062] In some embodiments, the coating method is any one of roller coating, doctor blade coating, or impregnation.

[0063] Roll coating controls the amount of polymer solution transferred to the surface of the insulating paper by adjusting the speed and gap of the metering rollers, and is suitable for continuous roll-to-roll production. Doctor blade coating controls the thickness of the coating layer by controlling the gap between the doctor blade and the surface of the insulating paper, and is suitable for applications requiring high precision in coating amount. Impregnation completely immerses the insulating paper in the polymer solution, allowing the solution to fully penetrate the paper, and is suitable for applications requiring simultaneous coating on both sides and specific penetration depth. These three coating methods are suitable for different production scales and coating precision requirements, and can be selected according to the substrate specifications and mass production requirements of the insulating paper.

[0064] S103: Perform a first drying treatment on the coated insulating paper to form a coating layer of aramid on the surface of the cellulose fibers of the insulating paper.

[0065] The first drying process removes at least a portion of the amide-based polar solvent from the aramid polymer solution coated on the surface of the insulating paper, causing the concentration of the aramid polymer to continuously increase until it precipitates from the solution and is fixed on the surface of the cellulose fibers. The coating layer is a solid film formed by phase separation of the aramid polymer on the surface of the cellulose fibers. This coating layer imparts the heat resistance of the aramid to the fiber surface area of ​​the insulating paper, giving the insulating paper a heat resistance level higher than that of the cellulose substrate itself. Solvent removal drives the aramid to solidify in situ on the fiber surface, forming a molecularly uniform coating layer, avoiding the interfacial defects and poor adhesion problems that exist when coating pre-prepared solid aramid particles.

[0066] In some embodiments, the temperature conditions for the first drying process are 80°C to 110°C, and the duration is 10 minutes to 25 minutes.

[0067] This temperature range is designed to provide sufficient heat for evaporation while ensuring that the cellulose in the insulating paper substrate does not undergo thermal degradation or significant strength loss, allowing the amide-based polar solvent to evaporate from the coating layer within a reasonable process time. When the temperature is below 80°C, the solvent evaporation rate is too low, and the solvent residue is too high within a time range of 10 to 25 minutes. The phase separation of the aramid is insufficient, and the resulting coating layer still contains a large amount of residual solvent, which may continue to evaporate in subsequent processes, leading to the collapse of the coating layer structure or the formation of bubble defects. When the temperature is above 110°C, the cellulose fibers may undergo irreversible thermal oxidative degradation under prolonged high-temperature exposure, manifested as a decrease in the degree of polymerization, a reduction in mechanical strength, and a darkening of color. This time range is used in conjunction with temperature conditions to ensure that the solvent in the coating layer evaporates sufficiently within this time. If the time is less than 10 minutes, the solvent evaporation time is insufficient, resulting in excessive residual solvent inside the coating layer, incomplete separation of the aramid phase, and compromised continuity and density of the coating layer. If the time exceeds 25 minutes, the trace amounts of residual solvent in the formed coating layer have largely evaporated, and further extending the drying time contributes little to the structural perfection of the coating layer while increasing process energy consumption and production cycle. This combination of temperature and time conditions ensures that the evaporation rate of the amide-based polar solvent in the coating layer reaches the target level for sufficient aramid phase separation and the formation of a complete coating layer, while the degree of polymerization and mechanical properties of the cellulose fibers are essentially maintained under these treatment conditions.

[0068] In some embodiments, the coated insulating paper is placed in a hot air oven for a first drying treatment, which causes the solvent in the aramid polymerization solution to evaporate. The solvent evaporation causes phase separation of the aramid on the surface of the cellulose fibers, forming a continuous coating layer.

[0069] A hot air oven is used to transfer heat to the coated insulating paper using forced convection heating and to remove volatile solvent vapors. During this hot air drying process, the polar amide solvent in the coating layer evaporates upon heating, and its concentration continuously decreases. As the solvent concentration decreases, the solubility state of the aramid polymer in the composite solvent system gradually becomes unbalanced. The aramid molecular chains precipitate from the solution, aggregate, and entangle with each other. This process is a solvent evaporation-driven phase separation process. This phase separation process allows the aramid to form a continuous coating layer in situ on the surface of the cellulose fibers, rather than physically depositing on the fiber surface as pre-formed solid particles. The continuous coating layer formed by this phase separation has a larger actual contact area and a tighter interfacial adhesion with the cellulose fiber surface, creating structural conditions for subsequent interfacial bonding through intermolecular forces.

[0070] In some embodiments, the molecular chain of aramid includes amide groups, the surface of the cellulose fiber includes hydroxyl groups, and the coating layer is attached to the surface of the cellulose fiber through hydrogen bonds between the amide groups and the hydroxyl groups.

[0071] The nitrogen and oxygen atoms in the amide group possess lone pairs of electrons, enabling them to form hydrogen bonds with hydrogen atoms in the hydroxyl groups on the cellulose fiber surface. These hydrogen bonds establish a molecular-level interfacial bond between the aramid coating and the cellulose fiber, allowing the coating to adhere to the cellulose fiber surface. This hydrogen bonding mechanism differs from physical adsorption or mechanical anchoring; its binding force originates from the directional interaction between polar groups, possessing definite interaction sites and directionality. This allows two polymers with different chemical compositions to establish a strong adhesion at the interface at the molecular scale. This hydrogen bonding also prevents the coating from peeling or detaching from the cellulose fiber surface during subsequent processing and use, under mechanical stress, thermal stress, and solvent wetting, ensuring the stability of the modified insulating paper's heat resistance during long-term use.

[0072] S104: Soak or rinse the insulating paper after the first drying treatment to remove metal chlorides.

[0073] In the insulating paper after the first drying treatment, metal chlorides from the aramid polymerization solution remain inside the aramid coating layer and in the pores of the insulating paper. These metal chlorides exist in the insulating paper in the form of chloride ions and metal cations, exhibiting ionic conductivity. Their residue significantly reduces the volume resistivity of the insulating paper and increases dielectric loss. Immersion or rinsing is used to dissolve and remove the metal chlorides from the insulating paper by liquid displacement of the dielectric. This removal treatment eliminates the degrading effect of metal chlorides on the dielectric properties of the insulating paper, ensuring that the electrical insulation performance of the modified insulating paper meets the requirements for high-voltage power equipment. By removing ionic impurities through immersion or rinsing, the breakdown strength of the modified insulating paper is improved compared to the unmodified insulating paper, while maintaining a low level of dielectric loss.

[0074] In some embodiments, the insulating paper after the first drying treatment is repeatedly soaked or rinsed with a displacement solvent to remove residual metal chlorides in the polymerization solution of aramid.

[0075] The displacement solvent is used to contact and dissolve residual metal chlorides in the insulating paper, carrying them away. Multiple soakings or rinsings reduce the concentration of metal chlorides in the liquid phase by repeatedly replacing the displacement solvent, maintaining a concentration gradient of metal chlorides between the solid phase (insulating paper) and the liquid phase (displacement solvent), allowing the removal process to continue until the residual amount is reduced to the target level. This multiple soaking or rinsing method improves the removal efficiency under single displacement solvent usage conditions, avoiding process stagnation due to rapid saturation of metal chloride concentration in the displacement solvent.

[0076] In some embodiments, the replacement solvent is water, ethanol, or a mixture of water and ethanol.

[0077] Water is used to dissolve metal chlorides, which are highly soluble in water. Their cations and chloride ions can fully dissociate and disperse in the aqueous phase under hydration. Ethanol is used to reduce the surface tension of the displacement solvent and improve its wettability to the pores of the insulating paper. Furthermore, ethanol and water are miscible in any proportion to form a homogeneous phase. This mixed solvent of water and ethanol combines the high solubility of water for metal chlorides with the low surface tension wetting properties of ethanol in the pores of the insulating paper. This allows the displacement solvent to efficiently dissolve metal chlorides while also penetrating deeply into the micron-sized pores of the insulating paper for thorough removal.

[0078] In some embodiments, the soaking or rinsing temperature is room temperature.

[0079] Room temperature refers to the ambient temperature without active heating or cooling, typically between 15°C and 35°C. Operating at room temperature avoids the additional energy consumption required for heating to replace the solvent, and also prevents stress damage at the interface between the insulating paper and the fibers due to thermal expansion or dimensional changes in the cellulose fibers under high-temperature conditions. At room temperature, metal chlorides still possess sufficient solubility and diffusion rate in water or a mixture of water and ethanol, allowing for removal within a reasonable operating time.

[0080] In some embodiments, the soaking or rinsing is performed 2 to 3 times, with each soaking or rinsing lasting 10 to 15 minutes.

[0081] This range of number of replacements ensures that after 2 to 3 replacements, the residual metal chloride content in the insulating paper decreases to a level that does not significantly affect the dielectric properties. With fewer than 2 replacements, the metal chloride concentration in the replacement solvent is close to saturation after a single replacement, and the residual amount remains high. With more than 3 replacements, subsequent replacement operations have limited effect on further reducing the residual amount; further increasing the number of replacements decreases the marginal contribution to the removal effect but significantly increases process time and the amount of replacement solvent used. This time range ensures that metal chlorides have sufficient time to diffuse and dissolve from the interior of the insulating paper into the replacement solvent during each soaking or rinsing process. With less than 10 minutes, diffusion is insufficient, and metal chlorides deep within the insulating paper fail to dissolve completely. With more than 15 minutes, the soluble metal chlorides inside the insulating paper have essentially reached the equilibrium concentration for that replacement; further extending the time of a single replacement has limited contribution to the total removal amount.

[0082] S105: The insulating paper after removing metal chlorides is subjected to a second drying treatment to obtain modified insulating paper.

[0083] After removing metal chlorides, a displacement solvent is introduced into the insulating paper through soaking or rinsing. This solvent fills the pores of the insulating paper and the micropores of the coating layer, resulting in a high moisture content. This high moisture content reduces the insulation paper's breakdown strength and volume resistivity, and is also detrimental to its storage and subsequent processing. A second drying treatment removes the displacement solvent, restoring the insulating paper to a low-moisture state. In this dry state, the hydrogen bonds between the aramid coating and cellulose fibers are stable, and the dielectric and mechanical properties of the modified insulating paper reach the target levels. By achieving the target moisture content, the electrical insulation performance of the insulating paper meets the requirements of high-voltage power equipment, while also achieving dimensional and storage stability.

[0084] In some embodiments, the temperature conditions for the second drying process are 100°C to 130°C, and the duration is 10 minutes to 60 minutes.

[0085] This temperature range provides heat above the boiling point of the replacement solvent, allowing it to vaporize and escape from the insulation paper within a reasonable time. Simultaneously, this temperature is below the temperature threshold for significant thermal degradation of the cellulose fibers. The second drying process is at a higher temperature than the first because the binding force between the water or ethanol to the cellulose fibers is stronger than that between the organic solvent removed in the first drying process and the cellulose fibers, requiring a higher heat input for complete removal. Below 100°C, the vaporization rate of the replacement solvent is too low to reduce the moisture content of the insulation paper to the target level within a reasonable time. Above 130°C, although the vaporization rate of the replacement solvent continues to increase, prolonged exposure to high temperatures may lead to a decrease in the degree of polymerization and a loss of mechanical strength in the cellulose fibers. This time range is used in conjunction with temperature conditions to ensure that the insulating paper reaches the target moisture content within this time. If the time is less than 10 minutes, the vaporization time of the replacement solvent is insufficient, and the content of the replacement solvent remaining inside the insulating paper is still high, so the moisture content cannot be reduced to the target level. If the time exceeds 60 minutes, continuing to extend the drying time has limited contribution to further reducing the moisture content, but instead increases energy consumption and production cycle.

[0086] In some embodiments, the insulating paper after metal chloride removal is subjected to hot air drying or vacuum drying to remove the displacement solvent introduced by soaking or rinsing.

[0087] Hot air drying is used to transfer heat to the insulating paper through forced convection heating and remove the vaporized displacement solvent vapors. It is suitable for continuous roll-to-roll production processes. Vacuum drying is used to lower the boiling point of the displacement solvent in an environment below atmospheric pressure, allowing the displacement solvent to vaporize and escape at a lower temperature. It is suitable for insulating paper substrates that are sensitive to temperature or prone to strength loss at high temperatures. Both drying methods can achieve complete removal of the displacement solvent, and the appropriate method can be selected based on the characteristics of the insulating paper substrate, production scale, and equipment configuration.

[0088] In some embodiments, the modified insulating paper is cooled, wound up, and cut after the second drying process.

[0089] The modified insulating paper after the second drying treatment is at a high temperature, and its dimensions are in a state of thermal expansion. At the same time, the aramid coating and cellulose fibers have a certain degree of flexibility at this temperature. Cooling is used to lower the temperature of the modified insulating paper to room temperature, stabilize its dimensions, and keep it flat during subsequent winding and cutting. Winding is used to continuously wind the sheet-like modified insulating paper into rolls for easy storage, transportation, and subsequent processing. Cutting is used to slit the wide modified insulating paper longitudinally into narrow rolls of the target width or transversely into sheets of the target length to adapt to the size requirements of different power equipment.

[0090] In some embodiments, the modified insulating paper prepared based on the above method has a heat resistance rating of F (155°C) or H (180°C). The heat resistance rating characterizes the highest operating temperature that the insulating paper can withstand under long-term use conditions. The rating is based on the fact that after thermal aging at the corresponding temperature for a specified time, the mechanical and electrical properties of the insulating paper remain within acceptable ranges. The unmodified natural cellulose insulating paper has a heat resistance rating of A (105°C) because the glycosidic bonds in the cellulose molecular chain undergo significant thermal decomposition at temperatures above 105°C, resulting in a rapid decrease in the degree of polymerization. The heat resistance rating of modified insulating paper has been upgraded to Class F (155℃) or Class H (180℃) because the aramid coating on the surface of the cellulose fibers provides physical isolation and thermal protection during high-temperature exposure. The coating has a higher thermal decomposition temperature than cellulose, exhibiting no significant structural changes or strength loss within the 155℃ to 180℃ range. Simultaneously, the continuous coverage of the coating effectively blocks direct contact between the cellulose fibers and oxygen and moisture in the surrounding environment, significantly reducing the rates of thermal oxidative and hydrolytic degradation of cellulose. This heat resistance rating expands the application range of natural cellulose insulating paper from Class A heat-resistant equipment to Class F and H heat-resistant equipment, meeting the long-term heat resistance requirements of insulating materials in ultra-high voltage power transmission, large-capacity power transformers, and new energy fields. Through the physical isolation and thermal protection provided by the aramid coating, cellulose insulating paper maintains stable structure and performance at operating temperatures between 150℃ and 180℃, significantly broadening the application temperature window of natural fiber insulating paper.

[0091] Based on the above embodiments, by directly coating the polymer solution of aramid onto the surface of insulating paper, and then subjecting it to a first drying treatment to allow solvent evaporation, the aramid undergoes in-situ phase separation on the cellulose fiber surface, forming a continuous coating layer. This in-situ film-forming method avoids the interface defects and poor adhesion problems that exist when coating pre-prepared solid aramid particles. Simultaneously, the coating layer is firmly attached to the fiber surface through hydrogen bonds between the amide groups on the aramid molecular chain and the hydroxyl groups on the cellulose fiber surface, forming a gradient-reinforced structure with a chemically bonded interface. Compared with the existing technology that uses strong protic acid to dissociate aramid fibers and then mixes them with natural fibers for papermaking, this method eliminates the need for strong protic acid throughout the process, avoiding the risks of equipment corrosion and acid residue deteriorating insulation performance from the source. Furthermore, compared with the post-treatment method of spraying pre-prepared aramid nanofiber suspension onto the paper surface, the coating layer formed by molecular-level solution coating has substantial differences in continuity and interfacial bonding strength, enabling a leap in heat resistance from Class A to Class F and even Class H with only 2-10 wt% aramid loading. Through the synergistic effect of multiple steps including a first drying treatment, solvent immersion or rinsing to remove metal chlorides, and a second drying treatment, residual ionicly conductive metal chlorides can be effectively removed without damaging the integrity of the aramid coating layer. This results in a 15%–30% increase in the breakdown strength of the modified insulating paper compared to the unmodified paper, while preserving the inherent micron-sized pore structure of the insulating paper and maintaining an oil absorption retention rate of ≥90%. It also achieves a balance of high heat resistance, excellent electrical insulation performance, and good oil immersion compatibility. This modification method eliminates the need for complex strong acid treatment equipment and high-voltage homogenization equipment, simplifies the process, allows for solvent recovery, is suitable for continuous roll-to-roll production, and is applicable to various specifications of natural cellulose insulating paper substrates, demonstrating good industrial versatility and economic efficiency.

[0092] In some embodiments, the difference between the second drying treatment and the first drying treatment is that the first drying treatment is used to remove the organic solvent in the polymerization solution of aramid and induce the aramid phase to separate into a film, while the second drying treatment is used to remove the displacement solvent and moisture introduced in the soaking or rinsing step.

[0093] The first drying process is used to remove organic solvents from the aramid polymerization solution coated on the surface of the insulating paper. The removal of organic solvents drives the aramid to undergo phase separation on the surface of the cellulose fibers and form a coating layer. That is, the first drying process has the dual functions of "solvent removal" and "phase separation and film formation". The processing temperature and processing time are controlled to ensure the full evaporation of organic solvents and the complete formation of the coating layer. The second drying process is used to remove the introduced displacement solvents and residual moisture from the insulating paper after soaking or rinsing. The function of the second drying process is limited to "displacement solvent and moisture removal" and does not involve the structural formation of the coating layer. The processing temperature and processing time are controlled to reduce the moisture content of the insulating paper to a target level. The differences between the first and second drying processes in terms of temperature range, duration, and functional purpose are as follows: the temperature conditions (80~110℃) and time conditions (10~25min) of the first drying process are based on the evaporation rate of the organic solvent and the sufficient occurrence of phase separation, while the temperature conditions (100~130℃) and time conditions (10~60min) of the second drying process are based on the sufficient removal of the replacement solvent and moisture. After the first drying process, the coating layer is basically formed, and the second drying process is based on this, performing structural reconstruction that does not involve the coating layer. This functional distinction is used to clarify the operational purpose and control objectives of each drying process in the process flow, avoiding treating the two drying processes as a repetition of the same operation, and making the functions of each step complementary rather than redundant.

[0094] In some embodiments, prior to coating, the process further includes fumigating the surface of the insulating paper with organic solvent vapor containing metal chlorides to cause the cellulose on the surface of the insulating paper to swell.

[0095] Insulating paper is a sheet-like substrate formed from cellulose fibers through a papermaking process. Its surface layer, the area near the outer surface along the thickness direction of the insulating paper, undergoes irreversible keratinization during pulping and drying. The previously accessible hydroxyl groups on the fiber surface are blocked by hydrogen bonds between adjacent molecular chains, reducing the chemical affinity with the subsequent coating aramid polymer solution. Fumigation treatment uses vaporized solvents and metal chlorides to penetrate into the surface fibers of the insulating paper. The swelling effect of the solvent on the cellulose and the disrupting effect of the metal chlorides on the hydrogen bonds cause the keratinized fiber surface to re-expand, providing a more chemically active fiber surface for subsequent coating. This vapor pretreatment activates the fiber surface, enabling the subsequent coating aramid polymer solution to establish more hydrogen bonds with the cellulose fibers, improving the bonding strength between the coating layer and the insulating paper.

[0096] In some embodiments, the organic solvent is an amide-based polar solvent, and the metal chloride is lithium chloride; the lithium chloride content in the vapor is 0.5~2 wt%.

[0097] Amide-based polar solvents are used as carriers for lithium chloride and swelling agents for cellulose. The carbonyl groups in their molecular structure can form hydrogen bonds with the hydroxyl groups of cellulose, thereby weakening the original hydrogen bond network between cellulose molecular chains. Lithium chloride is used to synergistically enhance the swelling capacity of cellulose by the amide-based polar solvents. Lithium ions can coordinate with the hydroxyl groups of cellulose, further disrupting the hydrogen bonds between molecular chains. Within this range, the synergistic swelling effect of lithium ions is insufficient when the content is below 0.5 wt%, resulting in limited activation. When the content is above 2 wt%, the lithium chloride concentration in the vapor is too high, which may cause crystallization on the surface of the insulating paper, introducing additional metal chloride residues and increasing the load on subsequent removal processes.

[0098] In some embodiments, the penetration depth of the fumigation treatment is 5% to 15% of the thickness of the insulating paper.

[0099] Penetration depth characterizes the extent to which steam treatment affects the thickness of the insulating paper. This penetration depth is determined by the fumigation time, temperature, and steam concentration. Controlling the penetration depth within this range confines the activation effect to the surface region of the insulating paper, ensuring sufficient exposure of the hydroxyl active sites on the surface fibers while maintaining the original dense structure and mechanical properties of the inner core layer. When the penetration depth is below 5%, the activation effect is limited to the outermost layer of the fiber surface, resulting in a limited number of exposed hydroxyl groups and insufficient contribution to improving the bonding strength of subsequent coatings. When the penetration depth is above 15%, the activation effect extends to the inner core layer of the insulating paper, potentially disrupting the original hydrogen bond network of the core fibers and leading to a decrease in the overall mechanical strength of the insulating paper.

[0100] In some embodiments, the fumigation treatment temperature is 60~90℃ and the time is 30~120s.

[0101] This temperature range is used to maintain the organic solvent vapor in a gaseous state and ensure sufficient molecular kinetic energy for penetration into the surface fibers of the insulating paper. Below 60°C, the vapor molecules lack sufficient kinetic energy, resulting in a low penetration rate and difficulty reaching the target penetration depth within a reasonable time. Above 90°C, the steam treatment intensity is too high, potentially causing excessive swelling or even localized dissolution of the cellulose fibers under humid conditions, thus compromising the dimensional stability of the insulating paper. This time range is used in conjunction with temperature conditions to control the penetration depth. A time shorter than 30 seconds results in insufficient vapor penetration and inadequate activation. Extending the treatment time beyond 120 seconds may cause the penetration depth to exceed the target range and increase energy consumption.

[0102] In some embodiments, fumigation treatment exposes the hydroxyl active sites of the cellulose on the surface of the insulating paper and opens the microporous channels of the fiber cell walls.

[0103] Cellulose fibers consist of a multi-layered structure including primary and secondary walls. Micropores, nanoscale voids within the fiber cell walls, tend to close during wet papermaking and drying due to fiber shrinkage. The swelling effect of steam on cellulose during fumigation reopens these closed micropores and exposes hydroxyl groups previously masked by inter-chain hydrogen bonds to the fiber surface. These changes provide physical penetration channels and chemical bonding sites for the subsequent coating of aramid molecules, expanding interfacial bonding from two-dimensional surface contact to a three-dimensional interpenetrating network.

[0104] In some embodiments, during the fumigation treatment, the steam acts only on the surface layer of the insulating paper, causing the cellulose in the surface layer to swell asymmetrically, while the internal core layer of the insulating paper retains its original dense structure.

[0105] During fumigation, the steam acts only on the surface layer of the insulating paper, causing asymmetric swelling of the cellulose fibers. The core layer of the insulating paper retains its original dense structure during fumigation. Asymmetric swelling refers to the greater swelling of cellulose fibers near the surface of the insulating paper compared to the core layer in the thickness direction. This asymmetry arises because steam diffuses only from the surface inwards, with the concentration and penetration decreasing with depth along the diffusion path. This asymmetric swelling creates an activated region with a gradient structure on the surface of the insulating paper. The surface of this gradient activated region has high chemical activity and micropore openness, suitable for the penetration and anchoring of aramid molecular chains, while the core layer maintains its original fiber network structure and mechanical properties, ensuring the overall strength of the insulating paper remains unaffected.

[0106] In some embodiments, when the polymer solution of aramid is coated onto the surface of insulating paper after fumigation treatment, the molecular chains of aramid penetrate into the interior of the surface layer of the insulating paper along the microporous channels.

[0107] After fumigation, the aramid polymer solution is coated onto the surface of insulating paper. The aramid molecular chains penetrate into the interior of the insulating paper's surface layer along microporous channels. The microporous channels opened by the fumigation treatment exhibit capillary forces, driving the aramid polymer solution coated on the insulating paper surface to penetrate into the micropores. Simultaneously, the affinity between the amide-based polar solvent in the aramid polymer solution and cellulose further promotes this penetration process. This penetration behavior allows the aramid molecular chains to enter the micropores of the cellulose fiber cell walls, rather than being limited to the outer surface of the cellulose fibers. This results in a spatially interwoven distribution of the aramid solid phase formed during subsequent phase separation and the cellulose fibers.

[0108] In some embodiments, after the first drying treatment, the molecular chains of aramid form mechanically interlocked anchor points inside the surface layer of the insulating paper, forming an integrated reinforcing structure with the outer coating layer.

[0109] After the first drying process, the aramid molecular chains form mechanically interlocked anchor points within the surface layer of the insulating paper. These mechanically interlocked anchor points, together with the outer coating layer, constitute an integrated reinforcing structure. During the first drying process, the aramid polymer solution that has penetrated into the micropores of the surface layer undergoes phase separation as the solvent evaporates. The solidified aramid phase fills the micropores, forming anchor points embedded in the cell walls of cellulose fibers. These anchor points are physically connected to the continuous coating layer covering the outer surface of the cellulose fibers through the continuity of the aramid molecular chains, preventing the coating layer from sliding or peeling off along the fiber surface. This integrated reinforcing structure provides an additional mechanically interlocked anchoring force between the aramid coating layer and the cellulose fibers, in addition to hydrogen bonding. The synergistic effect of these two bonding mechanisms results in a significantly higher interfacial bonding strength than single hydrogen bonding or physical adhesion, thereby maintaining interfacial integrity under long-term thermal aging and mechanical stress.

[0110] In some embodiments, the insulating paper after the first drying treatment is repeatedly soaked or rinsed with a displacement solvent, including: in a first stage, soaking the insulating paper after the first drying treatment with a mixture of an amide polar solvent and water; in a second stage, soaking or rinsing the insulating paper after the first stage treatment with water; and in a third stage, soaking or rinsing the insulating paper after the second stage treatment with a mixture of an alcohol solvent and water.

[0111] The first stage involves soaking the first-drying-treated insulating paper in a mixture of an amide-based polar solvent and water. The second stage involves soaking or rinsing the first-stage treated insulating paper with water. The third stage involves soaking or rinsing the second-stage treated insulating paper in a mixture of an alcohol-based solvent and water. This three-stage gradient replacement method gradually reduces the concentration of the amide-based polar solvent in the replacement solvent, allowing for the step-by-step removal of residual metal chlorides and organic solvents from the insulating paper. This avoids structural damage to the aramid coating layer caused by sudden changes in the composition of the replacement solvent. Gradient replacement achieves gentle removal of impurities, enabling the modified insulating paper to achieve high electrical purity while maintaining the structural integrity of the coating layer, increasing breakdown strength by 15% to 30%, and keeping dielectric loss at a low level.

[0112] In some embodiments, in the first stage, the volume ratio of the amide polar solvent to water is 7:3 to 5:5.

[0113] This volume ratio range is used to control the concentration of amide-based polar solvents in the first-stage replacement solution, ensuring that the concentration difference between the replacement solution and the residual amide-based polar solvents inside the coating layer is within a controllable range. When the volume ratio is higher than 7:3, the concentration of amide-based polar solvents in the replacement solution is too high, resulting in insufficient dissolution capacity for metal chlorides and low removal efficiency in the first stage. When the volume ratio is lower than 5:5, the concentration of amide-based polar solvents in the replacement solution is too low, leading to an excessively large concentration difference between the replacement solution and the residual solvents inside the coating layer. This causes the solvent to migrate out of the coating layer too quickly, potentially resulting in microcracks in the coating layer due to uneven volume shrinkage.

[0114] In some embodiments, during the first stage, the volume ratio of the amide-based polar solvent to water is 7:3 to suppress the formation of microcracks in the coating layer while removing impurities.

[0115] This volume ratio is used to suppress microcrack formation in the coating layer while removing impurities. The 7:3 volume ratio ensures that the concentration of amide polar solvents in the replacement solution is close to the concentration of amide polar solvents remaining in the coating layer after the first drying treatment. This results in a gradual migration rate of solvent molecules from inside the coating layer into the replacement solution driven by the concentration gradient, leading to uniform volume shrinkage of the coating layer and preventing microcrack initiation due to stress concentration caused by localized shrinkage. The 7:3 volume ratio first-stage replacement solution has sufficient metal chloride dissolving capacity to initially remove some soluble metal chlorides from the surface of the coating layer and the pores of the insulating paper, providing a lower impurity concentration as initial conditions for the subsequent second-stage aqueous phase replacement.

[0116] In some embodiments, in the third stage, the volume ratio of alcohol solvent to water is 5:5 to 7:3.

[0117] This volume ratio range is used to ensure that the third-stage replacement solution possesses both the low surface tension characteristics of alcohol solvents and maintains a certain solubility for residual water-soluble impurities. When the volume ratio of alcohol solvent is below 5:5, the surface tension of the replacement solution remains close to that of pure water, which is insufficient to suppress capillary collapse. When the volume ratio of alcohol solvent is above 7:3, the alcohol solvent content in the replacement solution is too high, reducing its ability to dissolve and carry away trace amounts of metal chloride residues that may precipitate. At the same time, high concentrations of alcohol solvent may cause excessive swelling of the aramid fibers in the coating layer.

[0118] In some embodiments, the alcohol solvent in the third stage is ethanol.

[0119] Ethanol is used as a low surface tension organic solvent to form a mixed displacement solution with water. The surface tension of ethanol (about 22 mN / m) is significantly lower than that of water (about 72 mN / m), which can effectively reduce the overall surface tension of the displacement solution. At the same time, ethanol and water can be miscible in any proportion to form a uniform displacement solution phase.

[0120] In some embodiments, after the third stage is completed, the insulating paper is dried.

[0121] Air drying is used to allow most of the displacement solvent in the insulating paper to initially evaporate under natural ventilation before the second drying process. This air drying operation removes a large amount of displacement solvent from the insulating paper before entering the second drying process, reducing the load on the second drying process. During the air drying process, the small amount of ethanol / water mixture remaining in the insulating paper evaporates preferentially due to the higher volatility of ethanol compared to water. This causes the composition of the residual liquid in the insulating paper to gradually change towards a water-rich direction. During this compositional change, the coating layer slowly shrinks due to the decrease in ethanol concentration. This slow shrinkage helps to release the residual stress accumulated inside the coating layer during the first drying and displacement processes.

[0122] In some embodiments, the first stage is used to gradually reduce the concentration of amide-based polar solvents inside the coating layer to avoid microcracks in the coating layer due to sudden concentration changes.

[0123] After phase separation to form the coating layer, some of the amide-based polar solvent inside the coating layer remains in the amorphous region of the coating layer. This solvent portion has intermolecular interactions with the aramid molecular chains, constituting the plasticizing phase of the coating layer. The high concentration of amide-based polar solvent in the first-stage displacement solution results in a smaller chemical potential difference between the coating layer and the displacement solution phase. The diffusion rate of solvent molecules from the coating layer to the displacement solution is low, and the volume shrinkage of the coating layer proceeds at a slower rate. The shrinkage stress is gradually released in the viscoelastic response of the coating layer, effectively suppressing the risk of microcracks initiating due to shrinkage stress exceeding the strength of the coating layer material.

[0124] In some embodiments, the second stage is used to remove residual amide-based polar solvents and metal chlorides.

[0125] The second stage uses pure water as the replacement medium, as water has excellent solubility for both amide polar solvents and metal chlorides. After the first stage treatment, the concentration of amide polar solvents inside the coating layer has been initially reduced. In the second stage, there is a large concentration difference between pure water and the coating layer, which allows the residual amide polar solvents and metal chlorides to quickly migrate into the aqueous phase and dissolve. This stage completes the removal of most impurities.

[0126] In some embodiments, the third stage is used to replace the moisture inside the pores of the insulating paper with a low surface tension replacement liquid, thereby suppressing the collapse and damage to the pore structure of the coating layer and the insulating paper caused by capillary forces during the drying process.

[0127] After the second stage of treatment, the pores of the insulating paper and the micropores of the coating layer are filled with a large amount of water. During the subsequent drying process, when the water evaporates from the pores, the capillary force formed at the gas-liquid interface on the pore walls exerts an inward pulling force on the pore walls. This capillary force may cause micropore collapse and cracking of the coating layer. In the third stage, the mixture of alcohol solvent and water has a lower surface tension than pure water due to the low surface tension of the alcohol solvent. After replacing the pure water in the pores with this low surface tension replacement liquid, the capillary force formed at the gas-liquid interface during the subsequent drying process is significantly reduced, allowing the micron-sized pores of the insulating paper and the nano-sized micropores of the coating layer to remain open during the drying process.

[0128] In some embodiments, the third stage is also used to induce stress release and ordered rearrangement of the aramid molecular chains within the coating layer.

[0129] Alcohol solvents, acting as swelling agents for aramid fibers, can penetrate to some extent into the amorphous regions of aramid and weaken the intermolecular forces. In this swollen state, the aramid molecular chains exhibit high mobility. In the third stage, the concentration of the alcohol solvent gradually decreases (with replacement and subsequent drying processes), and the intermolecular forces gradually recover. During this recovery process, the molecular chains can rearrange at lower energy levels, releasing the frozen internal stress formed during phase separation and the initial drying process. Simultaneously, the orderliness of the molecular chains in the amorphous regions is improved, leading to an increase in the crystallinity of the coating layer. This stress release and ordered rearrangement synergistically optimize the microstructure of the coating layer, further enhancing its density and mechanical properties.

[0130] In some embodiments, the first drying process includes: hot air drying the coated insulating paper to a semi-dry state, so that the coating layer is in a gel state; applying pressure to the coating layer in the gel state, so that the residual solvent in the aramid polymerization solution carries the aramid to the depressions and intersections on the surface of the cellulose fibers; and continuing to dry until the coating layer is completely cured to form a continuous coating layer.

[0131] The first drying process employs a segmented drying method, including a pre-drying stage, a pressure-assisted stage, and a final drying stage. In the pre-drying stage, the coated insulating paper is dried with hot air to a semi-dry state. This semi-dry state is characterized by a reduction in the residual solvent content of the coating layer to 30% to 40% of the initial total solvent. At this point, most of the solvent in the coating layer has evaporated, but some remains inside, placing the coating layer in a gel state. This gel state represents an intermediate state where the aramid polymer molecular chains have formed a preliminary physical cross-linked network, but the network still contains sufficient solvent as a plasticizer. Under external force, the gel-state coating layer can undergo viscous flow and deformation without cracking. When pressure is applied in the semi-dry state, the residual solvent acts as a plasticizer and lubricant, allowing the aramid molecular chains to relatively slide and redistribute under pressure, preventing cracking or delamination due to the coating layer being completely cured.

[0132] Applying pressure to the gel-state coating layer causes residual solvent in the aramid polymerization solution to carry the aramid fibers to the depressions and intersections on the cellulose fiber surface. The residual solvent in the gel-state coating layer still possesses a certain dissolving and carrying capacity. The applied pressure creates a pressure gradient within the coating layer, driving the residual solvent to flow from pressurized areas to unpressurized or low-pressure areas. This flowing solvent carries along the incompletely cured aramid molecular chains. The cellulose fiber surface contains depressions and intersections formed by fiber interweaving. During conventional coating and drying processes, these areas often become the thinnest or even uncovered areas of the coating layer due to liquid film surface tension. The pressure-driven migration of aramid molecular chains and residual solvent fills these depressions and intersections, increasing the coating layer's coverage on the fiber surface. By driving the solvent and aramid molecular chains to migrate to the depressions with pressure, a complete covering network is formed on the fiber surface, preventing the formation of island-like discontinuous distributions due to coating shrinkage under low loads, which would weaken the overall heat resistance.

[0133] Continue drying until the coating is completely cured, forming a continuous coating layer. Complete curing means that the residual solvent content in the coating layer has decreased to a level that no longer significantly affects the glass transition temperature and mechanical properties of the aramid polymer. At this point, the physical cross-linking network between the aramid molecular chains has been fully established, and the coating layer transitions from a gel state to a solid state, forming a structurally complete and mechanically stable continuous coating layer. This continued drying stage is used to fix the structure of the coating layer after pressure-assisted leveling, ensuring that the pressure-driven continuous coating form is maintained during subsequent processing and use.

[0134] In some embodiments, the semi-dry state refers to the coating layer containing 30% to 40% of the total initial solvent content.

[0135] The residual solvent content, as a percentage of the initial total solvent, is used to quantitatively determine whether the coating has reached a suitable gel state for pressure application: When the residual solvent content is higher than 40%, the liquid phase ratio in the coating is too high, the gel network is not fully established, and the coating is prone to excessive flow and dilution under pressure, leading to excessive migration of aramid molecular chains under pressure, uneven overall coating thickness distribution, and some areas failing to form effective coating due to excessive aramid loss; when the residual solvent content is lower than 30%, there is insufficient plasticizer in the coating, the gel network is too dense, and the viscous flow capacity of the coating is insufficient under pressure, with pressure mainly absorbed by the elastic deformation of the gel network and unable to effectively drive the solvent and aramid molecular chains to migrate to the recessed areas. Controlling the residual solvent content within this range ensures that the coating has both sufficient viscous flow capacity to respond to pressure and sufficient structural integrity to maintain the continuous morphology of the coating.

[0136] In some embodiments, pressure is applied by roller pressing.

[0137] Roll forming uses a pair of rotating rollers to apply linear pressure to the insulating paper and its surface coating. As the insulating paper passes between the rollers, the coating experiences uniform vertical pressure at the roller gap, which is evenly distributed along the width of the insulating paper. Roll forming is used to apply pressure to a large area of ​​coating with uniform pressure distribution on a continuous production line. Its uniformity and controllability of linear pressure are superior to other pressing methods, and its continuous operation characteristics are well-suited to roll-to-roll production processes.

[0138] In some embodiments, the roller temperature used for rolling is 100~120℃, and the linear pressure is 2~5kg / cm.

[0139] Roller temperature is used to transfer heat to the coating layer, maintaining its temperature within a range conducive to viscous flow. If the roller temperature is below 100°C, the coating layer temperature is too low, resulting in insufficient flowability of residual solvent, limited mobility of aramid molecular chains, and low pressure-driven migration efficiency. If the roller temperature is above 120°C, the coating layer temperature is too high, significantly accelerating the evaporation rate of residual solvent. Excessive solvent evaporation during rolling may cause the coating layer to solidify before the pressure application is complete. Simultaneously, high temperatures may cause thermal damage to the cellulose fibers. Linear pressure characterizes the pressure applied by the roller to the insulation paper per unit width. If the linear pressure is below 2 kg / cm, the driving force is insufficient, making it difficult to effectively drive the solvent and aramid molecular chains to migrate towards the recesses. If the linear pressure is above 5 kg / cm, the pressure is too high, potentially causing irreversible compression deformation of the insulation paper at the roll gap, leading to reduced insulation paper thickness and decreased porosity. Excessive pressure may also excessively compress residual solvent and aramid molecular chains in the coating layer into the insulation paper, resulting in insufficient surface coating thickness.

[0140] In some embodiments, pressure is applied to cause the coating to level and bridge under pressure assistance in order to form a continuous cover layer on the surface of the cellulose fibers.

[0141] Leveling is the process by which the coating layer becomes more uniform in thickness under pressure. The coating layer, which was originally thicker at fiber protrusions and thinner or missing at depressions due to surface tension contraction, is redistributed under pressure, resulting in a more consistent coating thickness on the fiber surface. Bridging is the process by which previously isolated aramid aggregates in the coating layer connect with each other under pressure through flowing aramid molecular chains and residual solvent. This bridging connects the isolated aggregates into a continuous network structure. The synergistic effect of leveling and bridging allows the coating layer to form a complete cover layer on the cellulose fiber surface. This continuous cover layer provides a uniform heat-resistant barrier for the insulating paper.

[0142] In some embodiments, after the coating has been dried to complete curing, it is soaked or rinsed.

[0143] Once fully cured, the coating has transitioned from a gel state to a solid state, and its structure is essentially finalized, enabling it to withstand liquid immersion or rinsing. This timing sequence ensures that the displacement solvent used in immersion or rinsing operations will not redissolve or wash away the uncured aramid molecular chains from the coating. Simultaneously, the cured coating maintains its structural integrity and surface density, preserving its continuity and bonding strength with the cellulose fibers during the displacement and removal of impurities.

[0144] The following is a specific scenario example provided in this specification: I. Technical formula (parts by weight).

[0145] 1. Formulation of para-aramid polymerization solution.

[0146] N,N-Dimethylacetamide (DMAC): 100 parts; Anhydrous lithium chloride (LiCl): 3-7 parts, as a co-solvent to improve the solubility and solution stability of PPTA; p-Phenylenediamine (PPD): 2.5–5.5 parts; Terephthaloyl chloride (TPC): 4.7–10.4 parts, with the molar ratio of p-phenylenediamine to terephthaloyl controlled at 0.98–1.02:1 to ensure uniform degree of polymerization.

[0147] 2. Substrate: Natural cellulose insulating paper, using conventional softwood sulfate insulating paper, basis weight 60–120 g / m² 2 Thickness 0.1~0.3mm, conforming to GB / T 1913.1 standard.

[0148] II. Preparation process flow.

[0149] 1. Solvent pretreatment: Anhydrous lithium chloride is added to DMAC and stirred at room temperature until completely dissolved. Dehydration is performed using molecular sieves to control the water content of the system to ≤100 ppm. High-purity nitrogen is introduced throughout the process to isolate air and water vapor and prevent oxidation of the raw materials.

[0150] 2. Synthesis of para-aramid dopant: Under nitrogen protection and at a low temperature of -5 to 5°C, p-phenylenediamine was completely dissolved in the pretreated mixed solvent; terephthaloyl chloride was added slowly in batches, with the temperature controlled at ≤40°C throughout the process, and the reaction was stirred for 0.5 to 3 h; after the reaction was completed, the mixture was allowed to stand for degassing for 24 to 48 h to obtain a homogeneous and stable PPTA polymerization dopant, with the solid content of the dopant controlled at 2 to 20 wt%.

[0151] 3. Direct coating: Use a single-sided or double-sided single-pass direct coating process, using either doctor blade coating or roller coating, to uniformly coat the PPTA stock solution onto the surface of the natural cellulose insulating paper, controlling the aramid dry basis loading to be 2-10 wt% after single-sided coating.

[0152] 4. First drying: The coated insulating paper is placed in a hot air oven and dried at 80-110℃ for 10-25 minutes to allow most of the DMAC solvent to evaporate, and the para-aramid to penetrate into the insulating paper and form a continuous coating layer on the surface.

[0153] 5. Solvent replacement rinsing and desalination: The insulation is repeatedly soaked and rinsed with replacement solvents such as water and ethanol to replace residual DMAC solvent and soluble lithium.

[0154] 6. Secondary drying and shaping: The desalted / desolventized insulating paper is dried at 100-130℃ for 10-60 minutes to completely remove moisture. After cooling, it is rolled up and cut to obtain the finished modified heat-resistant insulating paper.

[0155] The following provides two specific embodiments and a comparative example of this specification, as shown in Table 1: Example 1: 1. Preparation of stock solution: Take 100 parts of DMAC, add 5 parts of anhydrous lithium chloride, stir to dissolve, and then dehydrate with molecular sieve to a water content of 100 ppm. Under nitrogen protection, add 3.6 parts of p-phenylenediamine at 0℃, and add 7.0 parts of terephthaloyl chloride in 3 portions. The reaction is carried out at ≤35℃ for 2 h, and then allowed to stand for degassing for 36 h to obtain a PPTA stabilized stock solution with a solid content of 5.5 wt%.

[0156] 2. Insulating paper pretreatment: Select paper with a basis weight of 80 g / m². 2 0.18 mm thick coniferous cellulose insulating paper, dried at 100℃ for 1 h.

[0157] 3. Direct coating: A single-sided roller coating process is used, and the dry aramid loading is controlled at 6 wt%.

[0158] 4. First drying: Dry with hot air at 90℃ for 15 minutes.

[0159] 5. Washing and desalination: Soak and rinse twice with room temperature deionized water.

[0160] 6. Secondary drying: Vacuum drying at 110℃ for 1 h to obtain the finished modified insulating paper.

[0161] Performance testing: Heat resistance rating 155℃; breakdown strength 27.4 kV / mm; 88% retention of heat aging strength at 180℃ / 1000 h; 91% retention of oil absorption rate.

[0162] Example 2: 1. Preparation of stock solution: Take 100 parts of DMAC, add 6 parts of anhydrous lithium chloride, and dehydrate to a water content of 95 ppm; dissolve 4.59 parts of p-phenylenediamine at -2℃, add 8.5 parts of terephthaloyl chloride in 4 portions, control the temperature ≤30 h, react for 2.5 h, degas for 48 h, and the solid content is 6.8 wt%.

[0163] 2. Insulating paper pretreatment: Select insulating paper with a basis weight of 100 g / m² and a thickness of 0.22 mm, and dry it at 100℃ for 1 h.

[0164] 3. Direct coating: Double-sided roller coating, aramid dry basis total loading 10 wt%.

[0165] 4. First drying: Dry with hot air at 100℃ for 12 minutes.

[0166] 5. Water washing to remove salt: Soak in room temperature deionized water for 12 minutes, then rinse with spray 3 times.

[0167] 6. Secondary drying: Dry with hot air at 125℃ for 20 min to obtain the finished modified insulating paper.

[0168] Performance testing: Heat resistance rating 180℃; breakdown strength 29.1 kV / mm; 90% retention rate of heat aging strength at 180℃ / 1000 h; 90% retention rate of oil absorption.

[0169] Comparative example (traditional aramid fiber blend): 10 wt% of micron-sized para-aramid fibers were mixed with cellulose pulp to produce insulating paper of the same specifications.

[0170] Test results: Heat resistance rating 155℃, breakdown strength 24.0 kV / mm, oil absorption rate decreased to 81%.

[0171] Table 1

[0172] Corresponding to the above-described method for preparing modified insulating paper, this specification also provides a modified insulating paper, which is prepared according to the above-described method for preparing modified insulating paper.

[0173] In some embodiments, the modified insulating paper prepared based on the above method retains at least 85% of its tensile strength after 1000 hours of thermal aging at 180°C. The tensile strength retention rate characterizes the ability of the insulating paper to maintain its mechanical load-bearing capacity under high-temperature aging conditions. This retention rate is the ratio of the tensile strength after aging to the tensile strength before aging, expressed as a percentage. 1000 hours of thermal aging at 180°C is a typical thermal aging evaluation condition for H-grade heat-resistant insulating paper. This temperature and time combination is used to assess the performance stability of the insulating paper under long-term high-temperature service conditions. Under these aging conditions, the cellulose molecular chains of natural cellulose insulating paper undergo large-scale breakage due to the synergistic effect of thermal oxidation and hydrolysis reactions. The degree of polymerization decreases from an initial value of approximately 1000-1300 to below 250, and the tensile strength retention rate is typically no higher than 50%, indicating that its molecular chains have undergone severe degradation, and the insulating paper has entered the late stage of its lifespan. The modified insulating paper retains at least 85% of its tensile strength under these aging conditions. This is because the continuous coverage of the aramid coating significantly reduces the direct contact area between the cellulose fibers and oxygen in the high-temperature environment, thus inhibiting the rate of thermal oxidation. Simultaneously, the interfacial bonding structure formed by hydrogen bonding and mechanical interlocking between the aramid coating and the cellulose fiber surface remains stable at high temperatures, maintaining the thermal protection function of the coating during long-term aging. The rate of decrease in the degree of polymerization of the cellulose fibers is significantly slower than in unmodified insulating paper. This tensile strength retention characteristic ensures that the insulating paper maintains sufficient mechanical strength and structural integrity after long-term service at high temperatures. Through the thermal-oxygen isolation of the coating and the long-term stability of the interfacial bonding, the insulating paper maintains excellent mechanical properties after 1000 hours of aging under H-grade temperature conditions. Its strength retention level meets the long-term reliable operation requirements of power equipment under H-grade heat resistance, significantly extending the service life of the insulating paper under high-temperature conditions.

[0174] In some embodiments, the modified insulating paper prepared by the above method exhibits a breakdown strength that is 15% to 30% higher than that of the unmodified insulating paper, and an oil absorption retention rate greater than or equal to 90%. Breakdown strength characterizes the ability of insulating paper to resist electrical breakdown under an electric field; its value depends on the dielectric properties and internal defect density of the insulating paper. The breakdown strength of the unmodified insulating paper is limited by interfacial defects between cellulose fibers and local electric field distortion in the microporous structure within the paper sheet. The 15% to 30% increase in breakdown strength of the modified insulating paper compared to the unmodified insulating paper is due to the following reasons: the aramid coating fills the defect areas on the surface of the cellulose fibers, reducing the concentration points of the electric field on the fiber surface; simultaneously, aramid itself has a higher dielectric strength than cellulose, and the coating forms a continuous barrier layer with higher electrical resistance in the thickness direction of the insulating paper; after soaking or rinsing with a displacement solvent to remove metal chlorides, the content of ionicly conductive residual impurities in the insulating paper is reduced to an extremely low level, eliminating the risk of localized breakdown due to ion migration. Oil absorption retention rate characterizes the ability of modified insulating paper to retain its oil-impregnation properties after coating modification. The oil absorption rate is the percentage of the mass of oil absorbed by the insulating paper after impregnation with insulating oil, relative to the oven-dry mass of the insulating paper. The oil absorption rate of unmodified insulating paper is set as a baseline of 100%, derived from the oil storage space provided by the abundant micron-sized pores between cellulose fibers. The oil absorption retention rate of modified insulating paper is not less than 90%, because: the dry basis loading of aramid is controlled within a low range of 2wt% to 10wt%, the coating layer is mainly formed on the surface of cellulose fibers without extensively filling the micron-sized pores between fibers; simultaneously, the use of a low surface tension replacement liquid during the multi-stage gradient replacement process inhibits the collapse and destruction of the pore structure, and the internal pore morphology and connectivity of the insulating paper are protected during coating and replacement. This combination of improved breakdown strength and oil absorption retention characteristics enables the modified insulating paper to possess both high electrical insulation performance and good oil-impregnation compatibility. The improved breakdown strength enables the modified insulating paper to withstand higher operating voltages and more severe overvoltage impacts. The high oil absorption rate ensures that the insulating paper can fully absorb insulating oil in oil-immersed power equipment, maintaining the heat dissipation efficiency and dielectric strength of the oil-paper composite insulation system of the equipment. The synergy of both makes the modified insulating paper fully adaptable to the multi-dimensional performance requirements of high-voltage oil-immersed power equipment for insulating materials.

[0175] Although the process described above includes multiple operations that occur in a specific order, it should be clearly understood that these processes may include more or fewer operations that can be executed sequentially or in parallel (e.g., using parallel processors or a multithreaded environment).

[0176] This application is described with reference to flowchart illustrations and / or block diagrams of methods, apparatus (systems), and computer program products according to embodiments of this specification. It will be understood that each block of the flowchart illustrations and / or block diagrams, and combinations of blocks in the flowchart illustrations and / or block diagrams, can be implemented by computer program instructions. These computer program instructions can be provided to a processor of a general-purpose computer, special-purpose computer, embedded processor, or other programmable data processing apparatus to produce a machine, such that the instructions, which execute via the processor of the computer or other programmable data processing apparatus, generate instructions for implementing the flowchart... Figure 1 One or more processes and / or boxes Figure 1 A device that provides the functions specified in one or more boxes.

[0177] These computer program instructions may also be stored in a computer-readable storage medium that can direct a computer or other programmable data processing device to function in a particular manner, such that the instructions stored in the computer-readable storage medium produce an article of manufacture including instruction means, which are implemented in a process Figure 1 One or more processes and / or boxes Figure 1 The function specified in one or more boxes.

[0178] These computer program instructions may also be loaded onto a computer or other programmable data processing equipment to cause a series of operational steps to be performed on the computer or other programmable equipment to produce a computer-implemented process, thereby providing instructions that execute on the computer or other programmable equipment for implementing the process. Figure 1 One or more processes and / or boxes Figure 1 The steps of the function specified in one or more boxes.

[0179] Computer-readable media includes both permanent and non-permanent, removable and non-removable media that can store information using any method or technology. Information can be computer-readable instructions, data structures, modules of programs, or other data. Examples of computer storage media include, but are not limited to, phase-change memory (PRAM), static random access memory (SRAM), dynamic random access memory (DRAM), other types of random access memory (RAM), read-only memory (ROM), electrically erasable programmable read-only memory (EEPROM), flash memory or other memory technologies, CD-ROM, digital versatile optical disc (DVD) or other optical storage, magnetic tape, magnetic disk storage or other magnetic storage devices, or any other non-transferable medium that can be used to store information accessible by a computing device. As defined herein, computer-readable media does not include transient computer-readable media, such as modulated data signals and carrier waves.

[0180] Those skilled in the art will understand that the embodiments of this specification can be provided as methods, systems, or computer program products. Therefore, the embodiments of this specification can take the form of entirely hardware embodiments, entirely software embodiments, or embodiments combining software and hardware aspects. Furthermore, the embodiments of this specification can take the form of computer program products implemented on one or more computer-usable storage media (including, but not limited to, disk storage, CD-ROM, optical storage, etc.) containing computer-usable program code.

[0181] The various embodiments in this specification are described in a progressive manner. Similar or identical parts between embodiments can be referred to mutually. Each embodiment focuses on describing the differences from other embodiments. In particular, system embodiments are basically similar to method embodiments, so the description is relatively simple; relevant parts can be referred to the descriptions in the method embodiments. In the description of this specification, the terms "one embodiment," "some embodiments," "example," "specific example," or "some examples," etc., refer to specific features, structures, materials, or characteristics described in connection with that embodiment or example, which are included in at least one embodiment or example of the embodiments in this specification. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described can be combined in any suitable manner in one or more embodiments or examples. Moreover, without contradiction, those skilled in the art can combine and integrate the different embodiments or examples described in this specification and the features of different embodiments or examples.

[0182] The above description is merely an embodiment of this application and is not intended to limit the scope of this application. Various modifications and variations can be made to this application by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the scope of the claims of this application.

Claims

1. A method for preparing modified insulating paper, characterized in that, include: In a composite solvent comprising an amide-based polar solvent and a co-solvent, an aromatic diamine monomer and an aromatic diacyl chloride monomer are subjected to a polycondensation reaction to obtain a polymerization solution for aramid fibers; the co-solvent comprises a metal chloride. The polymer solution of aramid is coated onto the surface of insulating paper, so that the dry basis loading of aramid is 2~10wt%; The coated insulating paper undergoes a first drying process to form a coating layer of aramid on the surface of the cellulose fibers of the insulating paper. The insulating paper after the first drying treatment is soaked or rinsed to remove metal chlorides; The insulating paper after removing metal chlorides is subjected to a second drying treatment to obtain modified insulating paper.

2. The method according to claim 1, characterized in that, The amide polar solvent includes one or more of N,N-dimethylacetamide, N-methylpyrrolidone, and dimethylformamide; the metal chloride includes one or more of lithium chloride, calcium chloride, and zinc chloride.

3. The method according to claim 1, characterized in that, The aromatic diamine monomer includes p-phenylenediamine, and the aromatic diacyl chloride monomer includes terephthaloyl chloride.

4. The method according to claim 1, characterized in that, The molar ratio of the aromatic diamine monomer to the aromatic diacyl chloride monomer is 0.98:1 to 1.02:

1.

5. The method according to claim 1, characterized in that, The polycondensation reaction is carried out at a temperature of -5 to 5°C for 0.5 to 3 hours; the solid content of the polymerization solution of the aramid is 2 to 20 wt%.

6. The method according to claim 1, characterized in that, The coating includes single-sided coating and double-sided coating; in the double-sided coating, the dry basis loading of aramid on each side is 2~10wt%.

7. The method according to claim 1, characterized in that, The temperature of the first drying treatment is 80~110℃, and the time is 10~25min; The first drying treatment of the coated insulating paper, which forms a coating layer of aramid on the surface of the cellulose fibers of the insulating paper, includes: The coated insulating paper is placed in a hot air oven for a first drying treatment, which causes the solvent in the aramid polymerization solution to evaporate. The solvent evaporation causes phase separation of the aramid on the surface of the cellulose fiber, forming a continuous coating layer. The molecular chain of the aramid includes amide groups, and the surface of the cellulose fiber includes hydroxyl groups. The coating layer is attached to the surface of the cellulose fiber through hydrogen bonds between the amide groups and the hydroxyl groups.

8. The method according to claim 1, characterized in that, The soaking or rinsing of the insulating paper after the first drying treatment to remove metal chlorides includes: The insulating paper after the first drying treatment was repeatedly soaked or rinsed with a displacement solvent to remove impurities from the aramid polymerization solution. The replacement solvent is water, ethanol, or a mixture of water and ethanol.

9. The method according to claim 1, characterized in that, The second drying process is performed at a temperature of 100-130°C for 10-60 minutes. The second drying treatment of the insulating paper after removing metal chlorides yields modified insulating paper, comprising: The insulating paper after removing metal chlorides is dried by hot air or vacuum to remove the solvents introduced by soaking or rinsing.

10. A modified insulating paper, characterized in that, The modified insulating paper is prepared using the method for preparing modified insulating paper according to any one of claims 1 to 9.