A high-strength marine organism-proof device with controllable density and its preparation method

By combining M-Zr-MOF modified ultra-high molecular weight polyethylene injection-molded rollers with titanium alloy structures, the problems of impact resistance, density control, and connection strength of marine engineering facilities' anti-biological devices have been solved, achieving high-strength, reliable marine equipment connections and long-term stable suspension.

CN123109124APending Publication Date: 2026-11-17SUN YAT SEN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611299955.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-26
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing marine engineering facilities' anti-biological devices suffer from problems such as poor material impact resistance, inadequate density control, and insufficient connection strength, which limit the stability and lifespan of the equipment.

Method used

The injection roller body of ultra-high molecular weight polyethylene modified with M-Zr-MOF and titanium alloy structure is combined with glue-free braided self-locking connection to achieve controllable density, enhanced mechanical properties and high-strength reliable connection.

Benefits of technology

It enables long-term stable levitation and high-strength connection of marine engineering facilities, improves the wear resistance of equipment and reliability under extreme sea conditions, and reduces operation and maintenance costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123109124A_ABST
    Figure CN123109124A_ABST
Patent Text Reader

Abstract

This invention discloses a high-strength marine biological defense device with controllable density and its preparation method, belonging to the field of marine biological defense equipment technology. It includes an M-Zr-MOF-modified UHMWPE injection-molded roller body, a closed-loop cable protection ring, a UHMWPE load-bearing cable, a closed-loop titanium alloy end ring, a C-type open-loop locking titanium alloy ring, and titanium alloy locking screws; all titanium alloy rings are integral structures without welded seams. The roller body and protection ring are injection-molded from a polymer composition containing 65-75 parts of injection-grade UHMWPE, 12-20 parts of HDPE, and 3-8 parts of M-Zr-MOF. The M-Zr-MOF undergoes a two-step covalent modification involving a polydopamine transition layer and L-leucine amide grafting, resulting in a bulk density of 1.45-1.55 g / cm³. 3 The density of the composition was adjusted to 1.015~1.025 g / cm³. 3 The roller and protective ring are alternately strung on the cable. Both ends of the cable are self-lockingly braided and fixed to titanium alloy end rings without adhesive. The C-rings are locked in place with screws. This invention achieves precise density control and underwater neutral levitation, exhibits excellent mechanical and wear-resistant properties, and provides reliable connections.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of marine biological defense equipment technology, specifically relating to a high-strength marine biological defense device with controllable density and its preparation method. Background Technology

[0002] Offshore wind power plants, offshore oil platforms, and other marine engineering facilities are submerged in seawater for extended periods. Large amounts of marine organisms, such as algae, bacteria, barnacles, and mussels, easily colonize and proliferate on the equipment's surface. This marine organism attachment significantly increases structural fluid resistance, reduces equipment operational stability, substantially raises annual cleaning and maintenance costs, and severely restricts the service life and safety performance of marine engineering equipment.

[0003] Currently, most marine biological defense devices are made of ordinary high-density polyethylene (HDPE) or conventional ultra-high molecular weight polyethylene (UHMWPE). HDPE has poor impact resistance and fatigue resistance, making it prone to cracking and damage under the impact of typhoon surges in the South China Sea and the pressure and friction of sea ice in the north, thus rendering it unsuitable for long-term service. Conventional UHMWPE has a matrix density of only 0.93–0.94 g / cm³. 3 Due to their light weight and inability to achieve neutral suspension underwater, these materials must be modified and densified to match the density of seawater. Existing density control technologies are mainly divided into two categories: inorganic filler modification and fluoropolymer organic modification. Inorganic heavy fillers are prone to precipitation and interfacial peeling after long-term immersion in seawater, resulting in decreased density and mechanical degradation. Fluoropolymer modification systems such as polytetrafluoroethylene (PTFE) and fluorinated ethylene propylene copolymer (FEP) have limited functionality, and high dosages can reduce melt strength, making injection molding prone to cracking.

[0004] Meanwhile, existing marine biological control devices mostly use anaerobic adhesives to connect cables to 316L stainless steel. UHMWPE has extremely low surface energy, is difficult to bond, and the bonding interface is prone to peeling and failure, resulting in poor connection strength; 316L stainless steel butt joint structures are prone to crevice corrosion, leading to poor reliability under harsh sea conditions. Summary of the Invention

[0005] To address the aforementioned technical problems, this invention proposes a high-strength marine organism-proof device with controllable density and its preparation method, enabling the simultaneous achievement of precise density control, enhanced mechanical properties, and high-strength reliable connection of the UHMWPE suspended antifouling device.

[0006] To achieve the above objectives, the present invention adopts the following technical solution: First, the present invention provides a high-strength marine organism protection device with controllable density, comprising an M-Zr-MOF modified ultra-high molecular weight polyethylene injection roller and a closed cable protection ring, an ultra-high molecular weight polyethylene load-bearing cable, a closed titanium alloy end ring, a C-type open locking titanium alloy ring, and a titanium alloy locking screw. Both the closed titanium alloy end ring and the C-type open locking titanium alloy ring are integral titanium alloy structures without welding gaps. The injection roller and the closed cable protection ring are made of the same material, both having a coaxial central through hole, and are injection molded from a polymer composition. The polymer composition consists of the following components by weight: 65-75 parts injection-grade ultra-high molecular weight polyethylene, 12-20 parts high-density polyethylene, and 3-8 parts polydopamine-L-leucine covalently modified UiO-66Zr-MOF nanoparticles. The polydopamine-L-leucine covalently modified UiO-66Zr-MOF nanoparticles are M-Zr-MOF with a bulk density of 1.45-1.55 g / cm³. 3 This is used to adjust the overall density of the polymer composition to 1.015~1.025 g / cm³. 3 ; Multiple injection rollers and multiple closed-ended cable protection rings are alternately strung together on the outside of the ultra-high molecular weight polyethylene (UHMWPE) carrying cable, and the axial length of the closed-ended cable protection ring is less than the axial length of the injection roller; both the injection roller and the closed-ended cable protection ring can rotate freely around the circumference of the UHMWPE carrying cable. The two ends of the ultra-high molecular weight polyethylene load-bearing cable are fixed to the connecting handle of the closed titanium alloy end ring by a glue-free pure fiber self-locking braiding process, and the braided connection strength retention rate is not less than 90% of the breaking tensile strength of the cable body; The C-shaped opening locking titanium alloy ring has coaxial titanium alloy locking screws at both ends of its opening. The closed titanium alloy end ring can be inserted into the inner cavity of the C-shaped opening locking titanium alloy ring, and locking is achieved by tightening the titanium alloy locking screws.

[0007] The surface of the M-Zr-MOF nanoparticles has a bilayer modified structure of polydopamine transition layer and L-leucine amide covalent bond. The polydopamine transition layer is coated on the UiO-66 Zr-MOF surface, and the L-leucine is covalently grafted onto the surface of the polydopamine transition layer through amide bonds.

[0008] The viscosity-average molecular weight of the injection-molded ultra-high molecular weight polyethylene is 1.5 million to 2 million.

[0009] The ultra-high molecular weight polyethylene load-bearing cable has a 12-strand braided structure and a diameter of not less than 18 mm.

[0010] The titanium alloy is TC4 titanium alloy or TA2 titanium alloy, and the titanium alloy locking screw is TC4 titanium alloy or TA2 titanium alloy screw.

[0011] The polymer composition does not contain inorganic heavy fillers, nor does it contain polytetrafluoroethylene and fluorinated ethylene propylene copolymer.

[0012] Secondly, the present invention also provides a method for preparing the above-mentioned device, comprising the following steps: S1. Preparation of M-Zr-MOF nanofillers: S11. Zirconium tetrachloride and terephthalic acid were dissolved in N,N-dimethylformamide, glacial acetic acid was added, and after ultrasonic dissolution, the mixture was solvothermal reacted at 120 °C for 24 h. After centrifugation, washing and drying, native UiO-66 powder with a particle size of 100~200 nm was obtained. S12. The original UiO-66 powder was dispersed in a tris(hydroxymethyl)aminomethane hydrochloride buffer solution at pH=8.5, dopamine hydrochloride was added, and the mixture was stirred and polymerized at room temperature for 16 h. After centrifugation, washing and drying, UiO-66@PDA intermediate was obtained. S13. L-leucine, 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride and N-hydroxysuccinimide were dissolved in anhydrous N,N-dimethylformamide, activated in the dark, and then triethylamine was added. The UiO-66@PDA powder was then added and stirred in the dark at 60 °C for 12 h. After centrifugation, washing and drying, M-Zr-MOF nanofiller was obtained. S2. Weigh injection-grade ultra-high molecular weight polyethylene, high-density polyethylene and the M-Zr-MOF nanofiller according to the formula, mix them, melt-blend them through a twin-screw extruder, granulate them and dry them to obtain injection-molded granules; S3. Inject the injection molding granules to obtain the roller body and the closed cable protection ring; S4. The titanium alloy sheet is processed into the closed titanium alloy end ring and the C-type open locking titanium alloy ring, and the titanium alloy locking screw is processed accordingly. S5. After splitting the fibers at both ends of the ultra-high molecular weight polyethylene carrying cable, it is self-lockingly braided and fixed to the connecting handle of the closed titanium alloy end ring without using adhesive. S6. Alternately string the injection roller and the closed cable protection ring onto the ultra-high molecular weight polyethylene carrying cable, insert the closed titanium alloy end ring into the inner cavity of the C-shaped opening locking titanium alloy ring, and tighten the titanium alloy locking screw to complete the locking.

[0013] In step S12, based on 100 g of the original UiO-66 powder, a coating reaction was carried out using 2 L of the 10 mM, pH 8.5 tris(hydroxymethyl)aminomethane hydrochloride buffer and 8 g of the dopamine hydrochloride.

[0014] In S13, based on 100 g of the original UiO-66 powder, the amount of L-leucine is 12 g, the amount of 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride is 7.5 g, the amount of N-hydroxysuccinimide is 4.2 g, the amount of anhydrous N,N-dimethylformamide is 500 mL, and the amount of triethylamine is 3 mL.

[0015] The injection molding conditions in S3 are as follows: the injection granules are pre-dried at 80 ℃ for 2 h, the injection molding machine barrel temperature is 210~220 ℃, the mold temperature is 50 ℃, the injection pressure is 90 MPa, the holding pressure is 60 MPa, and the mold is demolded after cooling for 40 s.

[0016] Compared with the prior art, the beneficial effects of the present invention are: (1) A novel two-step covalent modification system for UiO-66 Zr abandons conventional modification routes such as barium sulfate and other inorganic fillers, PTFE / FEP fluororesin, and silane-modified MOF; and adopts a polydopamine transition layer covalent grafting L-leucine bilayer modification strategy. Polydopamine serves as an intermediate covalent bridge, making the L-leucine grafting firm and preventing it from falling off during high-temperature injection molding and long-term seawater immersion; the bio-based amino acid is fluorine-free, low-toxicity, and environmentally friendly to the marine environment, while achieving a triple synergistic function of hydrophobicity, antibacterial properties, and interface compatibilization, thus solving the inherent defects of one-step modification such as low grafting density, easy desorption during high-temperature processing, and nanoparticle aggregation; (2) Stable interfacial bonding and comprehensive improvement in mechanical and wear resistance. The double-layer covalently modified structure firmly encapsulates the MOF particles and does not fall off during high-temperature melt processing; the outer alkyl chain improves wettability with the polyolefin matrix and significantly reduces interfacial defects. The tensile strength, low-temperature impact toughness and wear resistance of the composite material of this invention are significantly improved, and it can withstand long-term sea ice compression and wave cyclic impact.

[0017] (3) The density is precisely controllable and the underwater suspension is stable over a long period of time. Only 3 to 8 parts of modified MOF are needed to precisely control the density of the composite material to 1.015 to 1.025 g / cm³. 3 Seawater compatibility range; the system does not contain inorganic fillers, and there is no filler precipitation or interface peeling during long-term immersion in seawater, and there will be no density drift. The device remains in a stable neutral suspension state for a long time.

[0018] (4) The adhesive-free braided self-locking connection, combined with the all-titanium alloy butt joint structure, ensures high reliability under extreme working conditions. The cable braided self-locking connection retains no less than 90% of the cable body strength, completely solving the problem of UHMWPE bonding failure; the titanium alloy is formed by milling and wire cutting of a whole plate, resulting in high strength and completely eliminating the risk of crevice corrosion and pitting of 316L stainless steel, making it suitable for multiple harsh sea conditions such as high temperature and high salinity in the South China Sea and low temperature and sea ice in the North.

[0019] (5) The roller body and the protective ring are arranged flexibly in alternation, which disperses the load and reduces wear. The large roller body and the small protective ring of the same material are connected in series alternately to improve the overall bending flexibility of the roller chain, evenly disperse the surge and sea ice impact load, reduce the stress concentration and friction loss on the end face of the roller body, effectively extend the service life of the device and reduce the operation and maintenance replacement cost. Attached Figure Description

[0020] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the description of the embodiments are briefly introduced below.

[0021] Figure 1 This is a schematic diagram of the connection of the marine organism prevention device of the present invention; Figure 2 This is a schematic diagram of the C-type titanium alloy open ring, closed titanium alloy end ring, and titanium alloy screw connection of the present invention.

[0022] The meanings of the markings in the diagram are as follows: 1. Injection roller body; 2. Closed cable protection ring; 3. UHMWPE load-bearing cable; 4. Closed titanium alloy end ring; 5. C-type open locking titanium alloy ring; 6. Titanium alloy locking screw. Detailed Implementation

[0023] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be described in detail below with reference to the accompanying drawings and specific embodiments.

[0024] Test methods and standards (1) Density test: The immersion drainage method was adopted and performed in accordance with GB / T 1033.1-2008 standard.

[0025] (2) Low temperature simply supported beam notched impact strength: in accordance with GB / T 1043.1-2008 standard.

[0026] (3) Tensile strength: in accordance with GB / T 1040.1-2018 standard.

[0027] (4) Sliding friction wear resistance: in accordance with GB / T 3960-2016 standard.

[0028] (5) Tensile breaking strength: Performed in accordance with GB / T 39289-2020 "Determination of adhesive bonding strength of metals and plastics".

[0029] Example 1 The raw materials of the composition in this embodiment, by weight, are: 72 parts of injection molding grade ultra-high molecular weight polyethylene with a viscosity-average molecular weight of 1.5 million to 2 million, 20 parts of high-density polyethylene, and 3 parts of M-Zr-MOF nanoparticles.

[0030] Step 1: Preparation of M-Zr-MOF hydrophobically modified nanofiller. 58.3 g of zirconium tetrachloride and 41.5 g of terephthalic acid were dissolved in 700 mL of DMF, and 40 mL of glacial acetic acid was added. The mixture was sonicated for 30 min until fully dissolved. The solution was transferred to a polytetrafluoroethylene-lined reactor and subjected to a solvothermal reaction at 120 °C for 24 h. After cooling, the mixture was centrifuged at 8000 r / min, washed three times with DMF, and exchanged three times with methanol solvent. The mixture was then vacuum dried at 80 °C for 12 h to obtain virgin UiO-66 powder with a particle size of 100–200 nm. 2 L of 10 mM Tris-HCl buffer (pH=8.5) was prepared, and 100 g of virgin UiO-66 powder was dispersed in the buffer. 8 g of dopamine hydrochloride was added, and the mixture was stirred and oxidatively polymerized at room temperature for 16 h. The mixture was centrifuged and washed until the filtrate was colorless, and then vacuum dried at 50 °C for 6 h to obtain the UiO-66@PDA intermediate. 12 g L-leucine, 7.5 g EDC·HCl, and 4.2 g NHS were dissolved in 500 mL anhydrous DMF and activated in the dark for 1 h. Then, 3 mL of triethylamine was added dropwise. All UiO-66@PDA powder was added, and the mixture was sonicated for 20 min and stirred in an oil bath at 60 ℃ in the dark for 12 h. After centrifugation, the powder was washed 4 times with anhydrous DMF and 3 times with ethanol, and then vacuum dried at 70 ℃ for 18 h to obtain M-Zr-MOF powder with a bulk density of 1.48 g / cm³. 3 .

[0031] Step 2: Composite material blending and granulation. Weigh 720 g UHMWPE, 200 g HDPE, and 30 g M-Zr-MOF according to the formula; mix the polyethylene matrix in a high-speed mixer for 5 min, add the modified MOF powder in batches, and stir at high speed for 10 min to obtain a uniform premix; put it into a co-rotating twin-screw extruder with a screw length-to-diameter ratio of 40:1, a temperature of 190~210 ℃ in each section, and a screw speed of 220 r / min for melt extrusion, water cooling and pelletizing, and hot air drying at 60 ℃ for 4 h to obtain injection molding granules.

[0032] Step 3: Injection molding roller 1 and closed cable protection ring 2. The granules are dried at 80℃ for 2 hours; the injection molding machine barrel temperature is 210~220℃, the mold temperature is constant at 50℃, the injection pressure is 90 MPa, the holding pressure is 60 MPa, and the product is demolded after cooling for 40 seconds; the flash is removed from the product, and the density is measured to be 1.016 g / cm³ using the drainage method. 3 .

[0033] Step 4: Machining and overall assembly of titanium alloy parts. For example... Figures 1 to 2As shown, the TC4 titanium alloy plate is milled and wire-cut to form a closed titanium alloy end ring 4 and a C-shaped open locking titanium alloy ring 5, polished and degreased, and fitted with M8 titanium alloy locking screws 6. A 18 mm diameter, 12-strand braided UHMWPE load-bearing cable 3 is selected, with the fibers at both ends self-locking and fixed to the connecting handle of the closed titanium alloy end ring 4 without glue. The injection roller body 1 and the closed cable protection ring 2 are alternately strung on the UHMWPE load-bearing cable 3, and the closed titanium alloy end ring 4 is inserted into the C-shaped open locking titanium alloy ring 5 and tightened with M8 titanium alloy locking screws 6 to obtain the finished device.

[0034] Example 2 The formulation, by weight, is: 70 parts injection molding grade UHMWPE, 17 parts HDPE, and 5 parts M-Zr-MOF. The rest is the same as in Example 1. The density, tested by the water displacement method, is 1.020 g / cm³. 3 .

[0035] Example 3 The formulation, by weight, is: 65 parts injection molding grade UHMWPE, 12 parts HDPE, and 8 parts M-Zr-MOF. The rest is the same as in Example 1. The density, tested by the water displacement method, is 1.025 g / cm³. 3 .

[0036] Comparative Example 1 100 parts of injection-grade UHMWPE were directly granulated and injection molded without the addition of HDPE and modified MOF. The rest was the same as in Example 1.

[0037] Comparative Example 2 The matrix formulation is the same as in Example 2, except that unmodified native UiO-66 Zr-MOF is used instead of the modified M-Zr-MOF, with an addition amount of 5 parts. The rest is the same as in Example 1.

[0038] Comparative Example 3 The rest of the formulation and process are the same as in Example 2, except that the amount of modified MOF added is adjusted to 2 parts.

[0039] Comparative Example 4 The rest of the formulation and process are the same as in Example 2, except that the amount of modified MOF added is adjusted to 10 parts.

[0040] Comparative Example 5 UiO-66 is only PDA coated and not grafted with L-leucine. The amount added is 5 parts, and the rest is the same as in Example 2.

[0041] Comparative Example 6 Without setting a polydopamine intermediate layer, L-leucine directly coordinates and binds to the metal sites on the surface of UiO-66. The amount added is 5 parts, and the rest is the same as in Example 2.

[0042] Comparative Example 7 The matrix formulation is the same as in Example 2, except that 13 parts of PTFE ultrafine powder are used to replace the modified MOF.

[0043] Comparative Example 8 The UHMWPE cable is fixed by anaerobic adhesive using 316L stainless steel butt joints, without braiding. The rest is the same as in Example 2.

[0044] Comparative Example 9 The UHMWPE cable was fixed by bonding with anaerobic adhesive using TC4 titanium alloy butt welding method, without braiding process, and otherwise the same as in Example 2.

[0045] Performance test results The performance test results of each embodiment and comparative example are shown in Table 1.

[0046] Table 1 Performance Comparison Table of Examples and Comparative Examples ; Examples 1-3 all used M-Zr-MOF prepared by the complete two-step covalent modification of this invention as the functional filler, with only the M-Zr-MOF addition amount adjusted in a gradient manner to 3 parts, 5 parts, and 8 parts, respectively. The densities of the three groups of samples were 1.016 g / cm³, respectively. 3 1.020 g / cm 3 1.025 g / cm 3 The concentration ranges from 1.015 to 1.025 g / cm³. 3 Within the neutral suspension range; low-temperature simply supported beam notched impact strength: 71~76 kJ / m 2 Tensile strength 34.2~36.8 MPa, wear volume 1.75~2.12 mm. 3 All mechanical abrasion resistance indicators are significantly better than all comparative examples; the 18 mm UHMWPE load-bearing cable with a non-adhesive braided joint stably achieves a tensile breaking force of over 249 kN, and the connection strength retention rate meets the requirement of not less than 90%. Among them, Example 2 has the best overall performance with a filler content of 5 parts, Example 1 has better processing fluidity and lower cost, and Example 3 has the highest density and is suitable for high-salinity deep sea. The three examples together verify that the addition of 3 to 8 parts of M-Zr-MOF combined with the polydopamine-L-leucine double-layer covalent modification process can simultaneously achieve multiple technical effects such as precise density control, enhanced mechanical abrasion resistance, and high-strength non-adhesive cable connection.

[0047] Comparative Example 1 used only pure UHMWPE, with a density of only 0.936 g / cm³. 3Unable to achieve neutral suspension, the samples exhibited the worst mechanical and abrasion resistance among all specimens, demonstrating that the combination of HDPE and M-Zr-MOF is fundamental for achieving density control and performance enhancement. Comparative Example 2 used unmodified native UiO-66, Comparative Example 5 had only a single-layer PDA coating, and Comparative Example 6 directly coordinated L-leucine without a PDA transition layer. All three filler modification processes differed from the two-step covalent modification scheme of this invention, resulting in a significant decrease in mechanical properties. This verifies that the double-layer modification of the polydopamine transition layer with amide grafting of L-leucine is the core innovative step. Comparative Examples 3 and 4 had M-Zr-MOF additions of 2 and 10 parts respectively, deviating from the 3-8 part range; the former had a density less than 1.015 g / cm³. 3 The inability to stably suspend the material and the weak modification and enhancement effects, coupled with excessive filler agglomeration and deterioration of mechanical properties in the latter, demonstrate that 3-8 parts represent an effective filling window. Comparative Example 7, which uses PTFE fluoropolymer to replace M-Zr-MOF, exhibits lower mechanical properties, highlighting the advantages of the M-Zr-MOF hybrid system of this invention. Comparative Examples 8 and 9 retain the optimal modified composite material roller body, only replacing the connection structure with anaerobic adhesive bonding of 316L stainless steel and TC4 titanium alloy. The tensile breaking strength of the cable joints in these examples is only 25 kN and 23 kN, respectively, far lower than the 250 kN or more in the example. Even replacing the substrate with corrosion-resistant titanium alloy cannot solve the defect of easy peeling at the UHMWPE bonding interface, fully demonstrating that the combination of adhesive-free braided self-locking cable connection and all-titanium alloy locking structure is a key improvement to ensure high strength and high reliability of the connection under extreme sea conditions. All nine comparative examples demonstrate from different perspectives that the formulation range, filler modification process, and cable assembly structure of this invention work synergistically to achieve unexpected comprehensive service performance.

[0048] The preferred embodiments of the present invention disclosed above are merely illustrative of the invention. These preferred embodiments do not describe all details exhaustively, nor do they limit the invention to the specific implementations described. Clearly, many modifications and variations can be made based on the content of this specification.

Claims

1. A high-strength marine organism controllable density device, characterized in that, It includes an M-Zr-MOF modified ultra-high molecular weight polyethylene injection roller (1), a closed cable protection ring (2), an ultra-high molecular weight polyethylene load-bearing cable (3), a closed titanium alloy end ring (4), a C-type open locking titanium alloy ring (5), and a titanium alloy locking screw (6). The closed titanium alloy end ring (4) and the C-type open locking titanium alloy ring (5) are both integral titanium alloy structures without welding gaps. The injection roller (1) and the closed cable protection ring (2) are made of the same material, both having a coaxial central through hole, and are injection molded from a polymer composition. The polymer composition consists of the following components by mass: 65-75 parts of injection-grade ultra-high molecular weight polyethylene, 12-20 parts of high-density polyethylene, and 3-8 parts of polydopamine-L-leucine covalently modified UiO-66 Zr-MOF nanoparticles. The polydopamine-L-leucine covalently modified UiO-66 Zr-MOF nanoparticles are M-Zr-MOF with a bulk density of 1.45-1.55 g / cm³. 3 This is used to adjust the overall density of the polymer composition to 1.015~1.025 g / cm³. 3 ; Multiple injection rollers (1) and multiple closed cable protection rings (2) are alternately strung together on the outside of the ultra-high molecular weight polyethylene carrying cable (3), and the axial length of the closed cable protection ring (2) is less than the axial length of the injection roller (1); both the injection roller (1) and the closed cable protection ring (2) can rotate freely around the circumference of the ultra-high molecular weight polyethylene carrying cable (3); The two ends of the ultra-high molecular weight polyethylene load-bearing cable (3) are fixed to the connecting handle of the closed titanium alloy end ring (4) by a glue-free pure fiber self-locking braiding process, and the braided connection strength retention rate is not less than 90% of the breaking tensile strength of the cable body; The C-shaped opening locking titanium alloy ring (5) is equipped with coaxial titanium alloy locking screws (6) at both ends of the opening. The closed titanium alloy end ring (4) can be inserted into the inner cavity of the C-shaped opening locking titanium alloy ring (5) and locking is achieved by tightening the titanium alloy locking screws (6).

2. The high-strength marine organism controllable device according to claim 1, characterized in that: The surface of the M-Zr-MOF nanoparticles has a bilayer modified structure of polydopamine transition layer and L-leucine amide covalent bond. The polydopamine transition layer is coated on the UiO-66 Zr-MOF surface, and the L-leucine is covalently grafted onto the surface of the polydopamine transition layer through amide bonds.

3. The high-strength marine organism controllable device according to claim 1, characterized in that: The viscosity-average molecular weight of the injection-molded ultra-high molecular weight polyethylene is 1.5 million to 2 million.

4. The high-strength marine organism controllable device according to claim 1, characterized in that: The ultra-high molecular weight polyethylene load-bearing cable (3) has a 12-strand braided structure and a diameter of not less than 18 mm.

5. The high-strength marine organism controllable device according to claim 1, characterized in that: The titanium alloy is TC4 titanium alloy or TA2 titanium alloy, and the titanium alloy locking screw (6) is TC4 titanium alloy or TA2 titanium alloy screw.

6. The high-strength marine organism controllable device according to claim 1, characterized in that: The polymer composition does not contain inorganic heavy fillers, nor does it contain polytetrafluoroethylene and fluorinated ethylene propylene copolymer.

7. A method for preparing a high-strength marine organism-resistant device with controllable density as described in any one of claims 1 to 6, characterized in that, Includes the following steps: S1. Preparation of M-Zr-MOF nanofillers: S11. Zirconium tetrachloride and terephthalic acid were dissolved in N,N-dimethylformamide, glacial acetic acid was added, and after ultrasonic dissolution, the mixture was solvothermal reacted at 120 °C for 24 h. After centrifugation, washing and drying, native UiO-66 powder with a particle size of 100~200 nm was obtained. S12. The original UiO-66 powder was dispersed in a tris(hydroxymethyl)aminomethane hydrochloride buffer solution at pH=8.5, dopamine hydrochloride was added, and the mixture was stirred and polymerized at room temperature for 16 h. After centrifugation, washing and drying, UiO-66@PDA intermediate was obtained. S13. L-leucine, 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride and N-hydroxysuccinimide were dissolved in anhydrous N,N-dimethylformamide, activated in the dark, and then triethylamine was added. The UiO-66@PDA powder was then added and stirred in the dark at 60°C for 12 h. After centrifugation, washing and drying, M-Zr-MOF nanofiller was obtained. S2. Weigh injection-grade ultra-high molecular weight polyethylene, high-density polyethylene and the M-Zr-MOF nanofiller according to the formula, mix them, melt-blend them through a twin-screw extruder, granulate them and dry them to obtain injection-molded granules; S3. Inject the injection molding granules to obtain the roller body and the closed cable protection ring; S4. The titanium alloy sheet is processed into the closed titanium alloy end ring and the C-type open locking titanium alloy ring, and the titanium alloy locking screw is processed accordingly. S5. After splitting the fibers at both ends of the ultra-high molecular weight polyethylene carrying cable, it is self-lockingly braided and fixed to the connecting handle of the closed titanium alloy end ring without using adhesive. S6. Alternately string the injection roller and the closed cable protection ring onto the ultra-high molecular weight polyethylene carrying cable, insert the closed titanium alloy end ring into the inner cavity of the C-shaped opening locking titanium alloy ring, and tighten the titanium alloy locking screw to complete the locking.

8. The preparation method according to claim 7, characterized in that: In step S12, based on 100 g of the original UiO-66 powder, a coating reaction was carried out using 2 L of the 10 mM, pH 8.5 tris(hydroxymethyl)aminomethane hydrochloride buffer and 8 g of the dopamine hydrochloride.

9. The preparation method according to claim 7, characterized in that: In S13, based on 100 g of the original UiO-66 powder, the amount of L-leucine is 12 g, the amount of 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride is 7.5 g, the amount of N-hydroxysuccinimide is 4.2 g, the amount of anhydrous N,N-dimethylformamide is 500 mL, and the amount of triethylamine is 3 mL.

10. The preparation method according to claim 7, characterized in that: The injection molding conditions in S3 are as follows: the injection granules are pre-dried at 80 ℃ for 2 h, the injection molding machine barrel temperature is 210~220 ℃, the mold temperature is 50 ℃, the injection pressure is 90 MPa, the holding pressure is 60 MPa, and the mold is demolded after cooling for 40 s.