A method for preparing a thin-film thermocouple suitable for temperature measurement on metal surfaces
By preparing a glass solder insulating layer and an aluminum oxide nanoparticle protective layer on a nickel-based substrate, the insulation problem of nickel-based high-temperature alloy thin-film thermocouples in aerospace engine combustion chambers was solved, and stable temperature measurement under high-temperature environments was achieved.
Patent Information
- Application Number
- CN202611442893.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-17
- Publication Date
- 2026-11-17
AI Technical Summary
In the existing technology, thin-film thermocouples made of nickel-based high-temperature alloy materials are difficult to effectively insulate in high-temperature hot-end components such as combustion chambers of aerospace engines, leading to electrode short circuits and insulation layer detachment, which affects temperature signal output and service life.
Glass solder is used as the insulating layer, and the glass solder insulating layer is formed on a nickel-based substrate by screen printing technology. Combined with plasma treatment, positive and negative electrode films are then printed on the electrode surface, and an aluminum oxide nanoparticle protective layer is added on the outside to form a high-temperature resistant thin-film thermocouple.
It effectively isolates the nickel-based substrate from the electrode, reduces the risk of short circuits, improves the adhesion and stability of the insulation layer, enhances the electrode's resistance to oxidation and erosion, and extends the service life of the thin-film thermocouple.
Smart Images

Figure CN123111495A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of thin-film thermocouples, surface temperature sensors, and temperature measurement technology for hot-end components of aerospace engines. Specifically, it relates to a method for preparing a thin-film thermocouple suitable for temperature measurement of metal surfaces. Background Technology
[0002] High-temperature hot-end components such as combustion tubes and combustion chamber walls of aerospace engines must withstand the scouring of high-temperature exhaust gases and complex thermal cycling conditions for extended periods during service. To optimize the combustion process, implement thermal protection designs, and assess the lifespan of these components, in-situ, localized, and rapid measurements of their surface temperatures are essential. Thin-film thermocouples, due to their small size, low heat capacity, fast response speed, and ability to closely adhere to the surface of the object being measured, are ideally suited for measuring the surface temperature of these high-temperature components.
[0003] Currently, hot-end components such as combustion chambers are typically made of nickel-based high-temperature alloys, which possess excellent high-temperature mechanical properties and oxidation resistance. However, nickel-based materials are conductive. If the positive and negative electrodes of a thermocouple are directly printed onto the surface of a nickel-based substrate, a short circuit will occur, causing the electrodes to connect with the conductive substrate. This will result in the inability to output a normal temperature signal, or even directly cause the thin-film thermocouple to fail. Therefore, it is essential to place an insulating layer that is both high-temperature resistant and reliably bonded between the conductive nickel-based substrate and the thermocouple electrodes.
[0004] Existing insulation layers typically use prefabricated sheets such as ceramic sheets, mica sheets, and polyimide films, or prefabricated insulating coatings. However, the combustion chamber surface of aerospace engines usually has numerous heat dissipation holes and an overall curved structure. Traditional prefabricated insulating sheets face significant difficulties in fitting to such complex curved surfaces with holes. Not only is it difficult to achieve a proper fit, but they are also prone to peeling or detachment under high-temperature operating environments, leading to damage to the insulation layer.
[0005] On the other hand, since thermocouples need to operate directly in high-temperature fuel gas and oxidizing atmospheres, the outermost positive and negative electrodes and hot junctions are prone to surface oxidation, material particle shedding, and thin-film aging. These problems severely reduce the service life and temperature measurement stability of thin-film thermocouples in high-temperature environments. Therefore, how to construct a firmly bonded and non-detachable insulating layer on such complex curved metal components, and provide effective anti-oxidation and anti-erosion protection for the thermocouple surface, is a technical problem that urgently needs to be solved by those skilled in the art. Summary of the Invention
[0006] The purpose of this invention is to provide a method for preparing a thin-film thermocouple suitable for temperature measurement on metal surfaces, so as to solve the problems mentioned in the background art.
[0007] To achieve the above objectives, the present invention provides a method for preparing a thin-film thermocouple suitable for temperature measurement on metal surfaces, comprising the following steps: S1. Clean and dry the surface of the nickel-based substrate; S2. Plasma pretreatment is performed on the surface of the nickel-based substrate in an oxygen-containing gas atmosphere; S3. Glass solder paste is screen-printed onto the surface of the nickel-based substrate to form a wet glass solder film. S4. The glass brazing filler film is sequentially dried, debonded, and sintered to form a glass brazing filler insulating layer. S5. Plasma treatment is performed on the surface of the glass solder insulation layer in an oxygen-containing gas atmosphere; S6. The positive electrode paste and the negative electrode paste are screen-printed onto the glass solder insulating layer, and after curing or sintering, a positive electrode film and a negative electrode film are formed. One end of the positive electrode film and the negative electrode film are connected or overlapped to form a hot junction, and the other end forms a cold junction. S7. The positive electrode film and the negative electrode film are subjected to plasma treatment in a nitrogen-containing gas atmosphere; S8. The aluminum oxide nanoparticle protective slurry is screen-printed onto the outer surface of the positive electrode film, negative electrode film and hot junction, and then cured or sintered to form an aluminum oxide nanoparticle protective layer.
[0008] Furthermore, in S3, the glass solder wet film covers the projected areas of the positive electrode film, negative electrode film, hot junction and cold end, and extends outward by 0.5 mm to 5 mm relative to the edge of the electrode pattern.
[0009] Furthermore, in S4, the sintering conditions are 800±5℃ for 5 to 20 minutes, and the cooling rate after sintering is not higher than 50℃ / min.
[0010] Furthermore, in S2, S5 and S7, the parameters for plasma treatment include: gas flow rate of 20 to 50 SCCM, pulse amplitude of 3.0 to 6.0 kV, pulse frequency of 0.5 to 2 kHz, pulse width of 50 to 150 μs, and treatment time of 5 to 20 minutes.
[0011] Furthermore, the positive electrode slurry contains a positive electrode thermoelectric active material selected from NiCr, PtRh, and La. 0.67 Sr 0.33 The negative electrode slurry contains a negative electrode thermoelectric active material selected from NiSi, Pt, indium oxide, or indium tin oxide, and the positive electrode thermoelectric active material is different from the negative electrode thermoelectric active material.
[0012] The present invention also provides a thin-film thermocouple suitable for temperature measurement on metal surfaces, prepared by the above-described method, comprising: Nickel-based substrate; A glass solder insulating layer is disposed on the surface of the nickel-based substrate; A positive electrode film and a negative electrode film are disposed on the surface of the glass solder insulating layer. One end of the positive electrode film and the negative electrode film are connected or overlapped to form a hot junction, and the other end forms a cold junction. An aluminum oxide nanoparticle protective layer covers the outer surfaces of the positive electrode film, the negative electrode film, and the hot junction. The glass solder insulating layer is located between the nickel-based substrate and the positive electrode film and the negative electrode film.
[0013] Furthermore, the linewidths of the positive electrode film and the negative electrode film are 0.3 mm to 2 mm, and the thicknesses are 1 μm to 100 μm, respectively; the overlap length between the positive electrode film and the negative electrode film at the hot junction is 0.2 mm to 10 mm.
[0014] Furthermore, the aluminum oxide nanoparticle protective layer is formed by sintering and solidifying aluminum oxide nanoparticles with a particle size of 10nm to 200nm, and its thickness is 1μm to 100μm, and the electrical connection area of the cold end is not covered by the protective layer.
[0015] Furthermore, the positive electrode film is made of NiCr, and the negative electrode film is made of NiSi.
[0016] Furthermore, the thin-film thermocouple is attached to the surface of the curved metal component with heat dissipation holes, and the glass solder insulating layer, positive electrode film, negative electrode film and aluminum oxide nanoparticle protective layer are all arranged in the avoidance area between the heat dissipation holes.
[0017] Compared with the prior art, the beneficial effects of the present invention are as follows: In this method for fabricating a thin-film thermocouple suitable for temperature measurement on metal surfaces, a glass solder layer is used as the insulating layer, overcoming the problem that traditional rigid insulating sheets cannot completely adhere to complex curved surfaces. After sintering, the glass solder effectively isolates the conductive nickel-based substrate from the positive and negative electrodes, significantly reducing the risk of short circuits.
[0018] Secondly, this invention employs screen printing technology for patterning of the insulating layer, electrodes, and protective layer. This paste-based preparation process facilitates control over the coverage area and thickness of each film layer, ensuring good process continuity between the insulating layer and the electrodes. It is particularly suitable for avoidance-oriented placement on the curved surface of a combustion cylinder with heat dissipation holes.
[0019] Furthermore, this invention significantly improves the bonding state between layers through staged plasma treatment. The first two oxygen-containing atmosphere treatments improve the wetting and adhesion between the nickel-based substrate and the glass solder layer, and between the glass solder layer and the electrode surface; the final nitrogen-containing atmosphere treatment improves the surface condition of the positive and negative electrodes, thereby enhancing the operational stability of the electrodes.
[0020] Finally, the present invention adds an aluminum oxide nanoparticle protective layer to the outermost side of the electrode and the hot junction. Taking advantage of the high temperature resistance and chemical stability of aluminum oxide, it effectively blocks the scouring and oxidation of high temperature gas, thereby improving the service reliability of the thin film thermocouple in complex thermal cycling environments. Attached Figure Description
[0021] Figure 1 This is a schematic diagram of the planar structure of the glass solder insulating layer, positive and negative electrodes, and aluminum oxide nanoparticle protective layer on the nickel-based sample plate of the present invention. Figure 2 This is a physical image of the glass solder insulation layer and electrode pattern fabricated on a nickel-based sample plate in an embodiment of the present invention. Figure 3 This is a schematic diagram showing the arrangement of electrodes and glass brazing insulation layer on a combustion cylinder with heat dissipation holes in the curved surface application of the present invention. Figure 4 This is a schematic diagram of the second arrangement of the electrodes and glass brazing filler metal insulation layer on the combustion cylinder with heat dissipation holes in the curved surface application of the present invention; Figure 5 This is a schematic diagram of the plasma discharge processing device and wiring of the present invention.
[0022] Explanation of reference numerals in the attached diagram: 1. Hot junction; 2. Nickel-based substrate; 3. Glass solder insulation layer; 4. Negative electrode; 5. Positive electrode; 6. Cold junction; 7. Alumina nanoparticle protective layer; 8. Combustion chamber; 12. Heat dissipation hole; 20. Pulsed high-voltage power supply; 21. Flow controller; 22. High-voltage electrode lead; 23. Low-voltage electrode lead; 24. Thermocouple; 25. Gas source; 26. Shielding cover. Detailed Implementation
[0023] The technical solutions in the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0024] I. Structural components of a thin-film thermocouple: like Figure 1 and Figure 2As shown, the present invention provides a thin-film thermocouple suitable for temperature measurement on metal surfaces. The overall structure mainly includes: a nickel-based substrate 2, a glass solder insulating layer 3, a negative electrode 4, a positive electrode 5, and an aluminum oxide nanoparticle protective layer 7.
[0025] The nickel-based substrate 2 uses a nickel-based sample sheet (corresponding to the wall surface of metal components such as the combustion chamber of aerospace engines in practical applications). A glass solder insulating layer 3 is disposed on the surface of the nickel-based substrate 2, with a projected area larger than the area of the electrode pattern, extending outwards by 0.5mm to 5mm relative to the electrode edge to ensure that all subsequently printed electrodes are located within the insulating area. The positive electrode 5 and negative electrode 4 are disposed on the glass solder insulating layer 3, with one end overlapping to form a hot junction 1, and the other ends extending to form cold junctions 6. An aluminum oxide nanoparticle protective layer 7 covers the outer surfaces of the positive electrode 5, negative electrode 4, and hot junction 1; to facilitate subsequent wiring or data acquisition, the electrical connection area of the cold junction 6 is not covered by the protective layer, remaining partially exposed.
[0026] like Figure 5 As shown, the plasma discharge processing apparatus used in the preparation process of this invention includes: a pulsed high-voltage power supply 20, a flow controller 21, a high-voltage electrode wire 22, a low-voltage electrode wire 23, a thermocouple 24, a gas source 25, and a shield 26. The gas source 25 is used to supply oxygen-containing gas or nitrogen-containing gas into the shield 26; the high-voltage electrode wire 22 connects the high-voltage output terminal to the high-voltage electrode metal sheet inside the shield 26; the low-voltage electrode wire 23 connects the low-voltage terminal to the sample to be processed (such as the electrode end of the thermocouple 24).
[0027] II. Preparation method of thin-film thermocouples: The preparation process of this invention mainly includes the following steps: S1. Substrate cleaning: Select a rectangular nickel-based sample sheet as nickel-based substrate 2, and perform surface polishing, degreasing, anhydrous ethanol cleaning, deionized water rinsing, and drying at room temperature or in an oven.
[0028] S2. Substrate Plasma Pretreatment: The dried nickel-based substrate 2 is placed inside a shield 26, and oxygen-containing gas (such as oxygen or air) is introduced for pretreatment under a plasma discharge device. This step aims to improve the adhesion of the substrate surface, allowing the subsequent printed glass solder paste to spread better.
[0029] S3. Printed Glass Solder Insulation Layer: After uniformly mixing the lead-free glass solder slurry, a wet glass solder film is printed on the surface of the nickel-based substrate 2 using a screen printing process. The patterned area of the wet film covers the design areas of the positive electrode 5, negative electrode 4, hot junction 1, and cold junction 6.
[0030] S4. Drying and sintering: The substrate with the wet film of glass brazing filler is sent into the heating furnace and dried at 120±5℃ for 5 to 20 minutes; then the binder is removed at 400±5℃ for 20 to 40 minutes; finally, the substrate is sintered at 800±5℃ for 5 to 20 minutes and cooled to room temperature with the furnace at a rate not exceeding 50℃ / min to form a dense glass brazing filler insulating layer 3.
[0031] S5. Insulation layer plasma treatment: The sintered sample is placed back into the shield 26 and plasma discharge treatment is performed on the surface of the glass solder insulation layer 3 in an oxygen-containing gas atmosphere, thereby improving the adhesion of the subsequent electrode paste to the surface of the insulation layer.
[0032] S6. Electrode slurry preparation: According to the required thermocouple type 24, weigh the positive electrode thermoelectric active material powder and the negative electrode thermoelectric active material powder respectively, add organic carrier (such as terpineol), resin binder and dispersant, and prepare positive electrode slurry and negative electrode slurry by mixing and grinding.
[0033] S7. Electrode Pattern Printing: Using screen printing, the negative electrode paste is first printed onto the glass solder insulating layer 3 to form the negative electrode 4; then the positive electrode paste is printed to form the positive electrode 5, so that the positive and negative electrodes overlap at a set position to form a hot junction 1. The overlap length is controlled between 0.2 mm and 10 mm, the linewidth of the positive and negative electrode films is controlled between 0.3 mm and 2 mm, and the thickness is controlled between 1 μm and 100 μm. Subsequently, it is pre-dried at 80 to 150 °C and sintered and cured under a protective atmosphere.
[0034] S8. Electrode nitrogen plasma treatment: The formed thermocouple 24 is placed inside the shield 26, and nitrogen-containing gas (such as nitrogen or nitrogen-argon mixture) is introduced. The pulse high voltage power supply 20 is turned on to perform plasma discharge treatment on the positive and negative electrode surfaces to improve the surface working stability of the electrodes.
[0035] S9. Printing the outer protective layer: Alumina nanoparticles with a particle size ranging from 10nm to 200nm are mixed with a binder and an organic carrier and ground into a protective slurry. This slurry is then screen-printed onto the outer sides of the positive electrode 5, negative electrode 4, and hot junction 1, avoiding the wiring area of the cold end 6. After drying and sintering, an alumina nanoparticle protective layer 7 with a thickness of 1μm to 100μm is formed. III. Specific Implementation Examples: Example 1: A rectangular nickel-based sample sheet with dimensions of 60mm × 40mm × 2mm was selected as the substrate for a standard-sized NiCr / NiSi thin-film thermocouple. After cleaning and drying, it underwent plasma pretreatment in an oxygen-containing atmosphere (gas flow rate 30 SCCM, pulse amplitude 4.5 kV, pulse frequency 1 kHz, pulse width 100 μs, treatment time 10 minutes). After screen printing glass solder paste, it was dried at 120℃ for 10 minutes, debonded at 400℃ for 30 minutes, sintered at 800℃ for 10 minutes, and cooled at a rate of 40℃ / min. After another oxygen-containing plasma treatment, NiSi negative electrode paste and NiCr positive electrode paste were printed respectively. The electrode linewidth was set to 1 mm, and the film thickness was approximately 30 μm, forming negative electrode 4 and positive electrode 5, with a thermal junction overlap length of 3 mm. After curing, it underwent plasma treatment in a nitrogen-containing atmosphere (parameters as above, treatment time 15 minutes). Finally, a paste was prepared using aluminum oxide particles with a particle size of 50 nm and printed on the outside of the electrode. After sintering, an aluminum oxide nanoparticle protective layer with a thickness of about 20 μm was formed.
[0037] Example 2: Using the same nickel-based substrate and the same process flow as Example 1, the main difference was that a fine-linewidth screen printing plate was used for electrode screen printing, controlling the linewidth of the positive electrode 5 film and the negative electrode 4 film to 0.3 mm, and the film thickness to a relatively thin 1 μm. The overlap length of the hot junction 1 was 0.2 mm. In preparing the alumina nanoparticle protective layer 7, alumina nanoparticles with a particle size of 10 nm were selected, and the number of printing passes was controlled to ensure that the final sintered alumina nanoparticle protective layer 7 had a thickness of 1 μm. Testing showed that the thin-film thermocouple 24 under these parameters still exhibited good insulation performance and temperature response.
[0038] Example 3: Using the same nickel-based substrate and preparation process, in step S6, the positive electrode thermoelectric active material was replaced with PtRh powder, and the negative electrode thermoelectric active material was replaced with Pt powder. Due to the sintering characteristics of the platinum-rhodium alloy, the sintering temperature in step S7 was adjusted to 850°C. The preparation parameters for the remaining plasma treatment, glass solder insulation layer 3, and alumina nanoparticle protective layer 7 were consistent with those in Example 1. The resulting PtRh / Pt thin-film thermocouple 24 could also be stably attached to the glass solder insulation layer, meeting the measurement requirements in higher temperature regions.
[0039] IV. Practical Application Layout of Curved Surface Components: In a preferred practical application scenario, the thin-film thermocouple of the present invention can be directly deployed on the curved surface of the combustion tube of an aerospace engine with heat dissipation holes to achieve in-situ temperature monitoring of the hot end components.
[0040] like Figure 3In the layout shown, the combustion chamber 8 has multiple heat dissipation holes 12 arrayed on its curved wall. Since both the glass solder paste and electrode paste are screen-printed on a curved surface using a flexible screen, the glass solder insulation layer 3 can be designed within the clearance gaps between the heat dissipation holes 12. The negative electrode 4 and positive electrode 5 run along the glass solder insulation layer 3 and converge at the designated temperature measurement point to form a hot junction 1. The outer aluminum oxide nanoparticle protective layer also conforms to the curved shape and covers the electrodes.
[0041] like Figure 4 In the second layout shown, to accommodate heat dissipation holes 12 with different spacing and different temperature measurement lead-out directions, the glass solder insulation layer 3 and the positive and negative electrodes on the surface of the combustion cylinder 8 have been adaptively adjusted. The negative electrode 5 and the positive electrode 5 have changed their bending angle and wiring path while avoiding the heat dissipation holes 12, and a hot junction 1 is formed in the target temperature measurement area.
[0042] The above application layout demonstrates that the full-slurry screen printing process adopted in this invention is not limited by the inability of rigid insulating sheets to bend and fit, and can flexibly avoid holes or structural interference areas on the curved surface of metal, thus meeting the actual temperature measurement requirements of complex curved high-temperature components.
[0043] The foregoing has shown and described the basic principles, main features, and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The embodiments and descriptions in the specification are merely preferred examples of the present invention and are not intended to limit the invention. Various changes and modifications can be made to the present invention without departing from its spirit and scope, and all such changes and modifications fall within the scope of the present invention as claimed. The scope of protection of the present invention is defined by the appended technical solutions and their equivalents.
Claims
1. A method for preparing a thin-film thermocouple suitable for temperature measurement on metal surfaces, characterized in that, Includes the following steps: S1. Clean and dry the surface of the nickel-based substrate (2); S2. Plasma pretreatment is performed on the surface of the nickel-based substrate (2) in an oxygen-containing gas atmosphere; S3. Glass solder paste is screen-printed onto the surface of the nickel-based substrate (2) to form a wet glass solder film; S4. The glass brazing film is dried, debonded and sintered in sequence to form a glass brazing insulation layer (3). S5. Plasma treatment is performed on the surface of the glass solder insulation layer (3) in an oxygen-containing gas atmosphere; S6. The positive electrode paste and the negative electrode paste are screen printed on the glass solder insulating layer (3). After curing or sintering, a positive electrode (5) film and a negative electrode (4) film are formed. One end of the positive electrode (5) film and the negative electrode (4) film are connected or overlapped to form a hot junction (1), and the other end forms a cold end (6). S7. Plasma treatment is performed on the positive electrode (5) film and the negative electrode (4) film in a nitrogen-containing gas atmosphere; S8. The aluminum oxide nanoparticle protective slurry is screen printed on the outer surface of the positive electrode (5) film, the negative electrode (4) film and the hot junction (1), and then cured or sintered to form an aluminum oxide nanoparticle protective layer (7).
2. The method for preparing a thin-film thermocouple suitable for temperature measurement on a metal surface according to claim 1, characterized in that, In S3, the glass brazing film covers the projection areas of the positive electrode (5) film, the negative electrode (4) film, the hot junction (1) and the cold end (6), and extends outward by 0.5 mm to 5 mm relative to the edge of the electrode pattern.
3. The method for preparing a thin-film thermocouple suitable for temperature measurement on a metal surface according to claim 1, characterized in that, In S4, the sintering conditions are 800±5℃ for 5 to 20 minutes, and the cooling rate after sintering is not higher than 50℃ / min.
4. The method for preparing a thin-film thermocouple suitable for temperature measurement on a metal surface according to claim 1, characterized in that, In S2, S5 and S7, the parameters for plasma treatment include: gas flow rate of 20 to 50 SCCM, pulse amplitude of 3.0 to 6.0 kV, pulse frequency of 0.5 to 2 kHz, pulse width of 50 to 150 μs, and treatment time of 5 to 20 minutes.
5. The method for preparing a thin-film thermocouple suitable for temperature measurement on a metal surface according to claim 1, characterized in that, The positive electrode slurry contains a positive electrode thermoelectric active material selected from NiCr, PtRh, and La. 0.67 Sr 0.33 The negative electrode slurry contains a negative electrode thermoelectric active material selected from NiSi, Pt, indium oxide, or indium tin oxide, and the positive electrode thermoelectric active material is different from the negative electrode thermoelectric active material.
6. A thin-film thermocouple suitable for temperature measurement on metal surfaces, characterized in that, Prepared using the method described in any one of claims 1 to 5, comprising: Nickel-based substrate (2); A glass solder insulating layer (3) is disposed on the surface of the nickel-based substrate (2); A positive electrode (5) film and a negative electrode (4) film are disposed on the surface of the glass solder insulating layer (3). One end of the positive electrode (5) film and the negative electrode (4) film are connected or overlapped to form a hot junction (1), and the other end forms a cold end (6). A protective layer of aluminum oxide nanoparticles (7) is applied to the outer surfaces of the positive electrode (5) film, the negative electrode (4) film and the hot junction (1); The glass solder insulating layer (3) is located between the nickel-based substrate (2) and the positive electrode (5) film and the negative electrode (4) film.
7. The thin-film thermocouple suitable for temperature measurement of metal surfaces according to claim 6, characterized in that, The linewidths of the positive electrode (5) film and the negative electrode (4) film are 0.3 mm to 2 mm and the thicknesses are 1 μm to 100 μm, respectively; the overlap length of the positive electrode (5) film and the negative electrode (4) film at the hot junction (1) is 0.2 mm to 10 mm.
8. The thin-film thermocouple suitable for temperature measurement of metal surfaces according to claim 6, characterized in that, The aluminum oxide nanoparticle protective layer (7) is formed by sintering and solidifying aluminum oxide nanoparticles with a particle size of 10nm to 200nm, and its thickness is 1μm to 100μm. The electrical connection area of the cold end (6) is not covered by the protective layer.
9. The thin-film thermocouple suitable for temperature measurement of metal surfaces according to claim 6, characterized in that, The positive electrode (5) film is made of NiCr, and the negative electrode (4) film is made of NiSi.
10. The thin-film thermocouple suitable for temperature measurement of metal surfaces according to claim 6, characterized in that, The thin-film thermocouple is attached to the surface of the metal curved component with heat dissipation holes (12), and the glass solder insulation layer (3), the positive electrode (5) film, the negative electrode (4) film and the aluminum oxide nanoparticle protective layer (7) are all arranged in the avoidance area between the heat dissipation holes (12).