A method for determining the interfacial bonding strength of aluminum-magnesium composite plates welded by electromagnetic pulse welding

By observing the morphological characteristics and width of the annular welding zone on the magnesium side of the electromagnetic pulse welded aluminum-magnesium composite plate, the low efficiency and microscopic interpretation difficulties in evaluating the interfacial bonding strength of the electromagnetic pulse welded aluminum-magnesium composite plate in the prior art are solved, and intuitive process optimization guidance is provided.

CN123111941APending Publication Date: 2026-11-17CHONGQING UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611296681.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-25
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In the existing technology, the evaluation method for the interfacial bonding strength of electromagnetic pulse welded aluminum-magnesium composite plates relies on destructive mechanical testing, which is inefficient and difficult to explain the differences in bonding strength at the microscopic level, and cannot intuitively guide process optimization.

Method used

By observing the morphological characteristics of the annular welding area on the magnesium cross-section, the inner weak bonding area, the middle strong bonding area, and the outer weak bonding area are divided. The radial width of each area is measured, and the interface bonding strength is compared and judged by combining the characteristics of thorn pattern and dimple distribution.

Benefits of technology

It enables rapid and intuitive determination of interfacial bonding strength without mechanical testing, improves process screening efficiency, provides microscopic explanations, and guides the process design and optimization of electromagnetic pulse welding aluminum-magnesium composite plates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123111941A_ABST
    Figure CN123111941A_ABST
Patent Text Reader

Abstract

This invention discloses a method for determining the interfacial bonding strength of electromagnetic pulse welded aluminum-magnesium composite plates, comprising the following steps: Step 1: Electromagnetic pulse welding is performed using an aluminum plate as the fly plate and a magnesium plate as the substrate to prepare first and second tensile lap shear specimens for comparison, with the annular welded area located in the middle of the lap area, and a room temperature tensile test is conducted; Step 2: The morphology of the annular welded area on the magnesium side cross-section of the specimen is obtained, and it is divided from the inside to the outside into an inner weak bonding area, a middle strong bonding area, and an outer weak bonding area, and the radial widths W1, W2, and W3 of each area are calculated; Step 3: Based on the thorn pattern morphology and radial width ratio of the inner weak bonding area and the dimple characteristics of the middle strong bonding area, the interfacial bonding strength of the two specimens is compared. This invention is simple to operate and provides intuitive results, which can effectively guide process design and optimization.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a method for evaluating the interfacial bonding strength of metal composite plates, specifically a method for determining the interfacial bonding strength of electromagnetic pulse welded aluminum-magnesium composite plates. Background Technology

[0002] Electromagnetic pulse welding (EPW) is an advanced solid-state joining technology that utilizes the electromagnetic force generated by a pulsed magnetic field to drive a flyer plate to impact a substrate at high speed, achieving metallurgical bonding of dissimilar metals at the collision interface. Compared to fusion welding, EMW effectively suppresses intermetallic compounds (such as Mg) at the interface. 17 Al 12 The formation of a continuous layer of Al3Mg2 phase (Al3Mg2 phase) results in a high-performance aluminum-magnesium composite plate.

[0003] The interfacial bond strength of electromagnetic pulse welded aluminum-magnesium composite plates is typically evaluated using tensile lap shear tests, with key indicators including tensile lap shear force and tensile lap shear work (hereinafter referred to as shear force and shear work, respectively). However, in actual process design and optimization, it is often necessary to compare the interfacial bond strength of multiple samples prepared under different welding parameters to select the optimal process scheme. In existing technologies, this comparison can only rely on mechanical test data, i.e., tensile tests are performed on each sample separately to obtain the values ​​of shear force and shear work before comparison.

[0004] The above method has the following shortcomings: On the one hand, mechanical testing is a destructive test, and testing each sample requires time and cost. When there are a large number of samples to be compared, the efficiency is low. On the other hand, shear force and shear work are only macroscopic mechanical indicators, which are difficult to establish a clear correspondence with the microstructure of the interface. It is impossible to intuitively trace back the welding quality through cross-sectional features, and it is also difficult to explain the reasons for the difference in bonding strength between different samples from a microscopic level. Summary of the Invention

[0005] The purpose of this invention is to provide a method for judging the interfacial bonding strength of electromagnetic pulse welded aluminum-magnesium composite plates. This method can compare and judge the interfacial bonding strength of two samples, is simple to operate, and provides intuitive results. It can effectively guide the process design and optimization of electromagnetic pulse welded aluminum-magnesium composite plates.

[0006] To achieve the above objectives, the technical solution adopted by the present invention is as follows:

[0007] A method for determining the interfacial bonding strength of aluminum-magnesium composite plates welded by electromagnetic pulse welding includes the following steps:

[0008] Step 1: Select an aluminum plate as the fly plate and a magnesium plate as the base plate, and connect the aluminum plate and the magnesium plate using electromagnetic pulse welding; prepare the first and second samples to be compared respectively. Each sample is an aluminum-magnesium composite plate tensile lap shear test sample, so that the annular welding area of ​​the sample is located in the middle of the lap area of ​​the sample, and perform room temperature tensile tests on each sample respectively.

[0009] Step 2: Obtain the morphological characteristics of the annular welded area on the magnesium side section of each sample. The annular welded area is divided into three regions from the inside to the outside: the inner weak bonding area, the middle strong bonding area, and the outer weak bonding area. The radial widths W1, W2, and W3 of each region are calculated respectively.

[0010] Step 3: Based on the distribution morphology of the thorn pattern in the weak bonding area on the inner side of each sample, the radial width ratio, and the dimple distribution characteristics in the strong bonding area in the middle, the interfacial bonding strength of the first and second samples is compared and judged.

[0011] Preferably, in step one, the length ratio of the annular welding area to the lap area of ​​the aluminum-magnesium composite plate tensile lap shear specimen is 0.3~0.5, and the width ratio is 0.5~0.8.

[0012] Preferably, in step two, the inner weak bonding area includes tear grooves and a mesh-like thorn pattern that are radially parallel to each other along the annular welding area; the middle strong bonding area includes multiple dimple areas; and the outer weak bonding area includes tear grooves and dispersed tear blocks that are radially parallel to each other along the annular welding area.

[0013] Preferably, in step three, when the thorn pattern in the inner weak bonding area of ​​the first sample is distributed in a discontinuous network and its radial width satisfies W2 / (W1+W2+W3)≥0.45, it is determined that the interfacial bonding strength of the first sample is higher than that of the second sample.

[0014] Preferably, in step three, when the thorny pattern in the inner weak bonding area of ​​the first sample is distributed in a continuous network and its radial width simultaneously satisfies W2 / (W1+W2+W3)≥0.45 and W2 / W1≥2, it is determined that the interfacial bonding strength of the first sample is higher than that of the second sample.

[0015] Preferably, in step three, when the distribution of thorn patterns in the weak bonding area on the inner side of the first and second samples is similar, and the radial width relationships W2 / (W1+W2+W3) and W2 / W1 are similar, the distribution of dimples in the strong bonding area between the two samples is compared. The sample with more dimples and larger size has a higher interfacial bonding strength.

[0016] Preferably, in step two, the radial width of each region is calculated as follows: the radial width W1 of the inner weak bonding region is the average distance from the inner boundary of the annular welding area to the end of the tear groove and the extension of the thorn pattern; the radial width W2 of the middle strong bonding region is the average distance from the outer boundary of the inner weak bonding region to the end of the dimple distribution; the radial width W3 of the outer weak bonding region is the average distance from the outer boundary of the middle strong bonding region to the end of the tear groove and the extension of the tear block.

[0017] Compared with the prior art, the present invention has the following beneficial effects:

[0018] 1. This invention can compare and determine the interfacial bonding strength by acquiring and comparing the morphological characteristics of the annular welding area on the magnesium cross-section of two samples. It does not rely on mechanical test data, is easy to operate, and provides intuitive results, which can significantly improve the efficiency of process screening.

[0019] 2. This invention establishes the correspondence between the morphological characteristics of the annular welding zone of the magnesium side section of electromagnetic pulse welded aluminum-magnesium composite plates (including the distribution of thorn patterns in the inner weak bonding zone, the radial width ratio of the three regions, and the dimple distribution characteristics in the middle strong bonding zone) and the interfacial bonding strength. It can explain the reasons for the difference in bonding strength between different samples from the microstructure level, and provides a more intuitive and reliable basis for the process design and optimization of electromagnetic pulse welded aluminum-magnesium composite plates. Attached Figure Description

[0020] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention.

[0021] Figure 1 This is a schematic diagram of the lap joint area of ​​the magnesium side section of an aluminum-magnesium composite plate welded by electromagnetic pulse welding.

[0022] Figure 2 This is a schematic diagram of the microstructure of the annular welding zone on the magnesium side section of an electromagnetic pulse welded aluminum-magnesium composite plate, showing the distribution of the inner weak bonding zone, the middle strong bonding zone, and the outer weak bonding zone.

[0023] Figure 3 This is a microstructure diagram of the annular weld zone on the magnesium side section of an aluminum-magnesium composite plate welded by electromagnetic pulse welding with a discharge energy of 26kJ.

[0024] Figure 4 This is a microstructure diagram of the annular weld zone on the magnesium side section of an aluminum-magnesium composite plate welded by electromagnetic pulse welding with a discharge energy of 28kJ.

[0025] Figure 5This is a microstructure diagram of the annular weld zone on the magnesium side section of an aluminum-magnesium composite plate subjected to electromagnetic pulse welding with a discharge energy of 30kJ. Detailed Implementation

[0026] The present invention will now be described in further detail with reference to the accompanying drawings and specific embodiments, so that those skilled in the art can better understand the present invention.

[0027] This invention provides a method for determining the interfacial bonding strength of electromagnetic pulse welded aluminum-magnesium composite plates. The core of this method lies in establishing a correspondence between the microstructure characteristics of the annular welding zone on the magnesium side section and the interfacial bonding strength.

[0028] General sample preparation and observation methods:

[0029] An aluminum plate was selected as the fly plate, and a magnesium plate as the substrate. The aluminum and magnesium plates were joined using electromagnetic pulse welding. Tensile lap shear specimens of the aluminum-magnesium composite plate were prepared, ensuring that the annular weld zone of the specimen was located in the center of the lap zone. Figure 1 As shown. Preferably, the length ratio of the annular welded area to the overlap area of ​​the specimen is 0.3~0.5, and the width ratio is 0.5~0.8. After performing room temperature tensile tests on each specimen, the morphological characteristics of the annular welded area on the magnesium cross-section are obtained. The annular welded area is divided into three regions from the inside to the outside: an inner weak bonding area, a middle strong bonding area, and an outer weak bonding area, as shown. Figure 2 As shown. The inner weak bonding zone includes tear grooves and a mesh-like thorn pattern that are radially parallel to each other along the annular welding zone; the middle strong bonding zone includes multiple dimple zones; and the outer weak bonding zone includes tear grooves and dispersed tear blocks that are radially parallel to each other along the annular welding zone.

[0030] The formation mechanism of the above three regions is as follows: Electromagnetic pulse welding relies on the instantaneous discharge of the capacitor bank and the coupling effect of induced eddy currents to generate a strong Lorentz force on the workpiece, driving the workpiece to collide, causing plastic deformation and jet formation on the workpiece surface, thus achieving bonding. During electromagnetic pulse welding, there is an angle between the aluminum plate and the magnesium plate, meaning the collision is not perpendicular but oblique, resulting in an effective collision angle range for a strong connection between the aluminum and magnesium plates. In the initial stage of welding, due to the small collision angle, the energy waves generated at the aluminum / magnesium interface collision point do not propagate completely homogeneously in the same direction. The energy superposition has certain disordered characteristics, forming an inner weak bonding zone, manifested as a magnesium side cross-section consisting of radially parallel tear grooves and a mesh-like thorn pattern along the annular welding area. As the welding process continues, the collision angle enters the effective range, and the aluminum / magnesium interface begins to produce severe shear deformation and metal jet formation, forming an intermediate strong bonding zone, manifested as a magnesium side cross-section consisting of dimples. In the later stages of welding, due to the excessive collision angle and energy dissipation, the shear deformation and metal jet at the aluminum / magnesium interface are significantly weakened, with strong bonding only existing in localized areas, forming a weak bonding zone on the outer side. This manifests as the magnesium side cross-section consisting of radially parallel tear grooves and dispersed tear blocks along the annular welding zone.

[0031] During the judgment process, the radial widths W1, W2, and W3 of each region need to be measured separately. Specifically, W1 (radial width of the inner weak bonding zone) is the average distance from the inner boundary of the annular weld zone to the end of the tear groove and the extension of the thorn pattern; W2 (radial width of the middle strong bonding zone) is the average distance from the outer boundary of the inner weak bonding zone to the end of the dimple distribution; and W3 (radial width of the outer weak bonding zone) is the average distance from the outer boundary of the middle strong bonding zone to the end of the tear groove and the extension of the tear block. It should be noted that the aforementioned "average distance" refers to multiple measurements taken at different locations within the annular weld zone (e.g., multiple points selected along the circumference), and the arithmetic mean of these measurements is calculated to eliminate errors caused by local non-uniformity.

[0032] The following analysis uses three examples with different discharge energies as examples:

[0033] Example 1: Electromagnetic pulse welding was performed using a discharge energy of 26kJ. Observation of the magnesium cross-section revealed that the thorny texture in the inner weak bonding zone was distributed in a discontinuous network pattern, such as... Figure 3 As shown. Measurements revealed the following radial widths for each region: inner weak bonding region W1 = 443 μm, middle strong bonding region W2 = 610 μm, and outer weak bonding region W3 = 673 μm.

[0034] According to the judgment criteria of this invention, when the thorn pattern is distributed in a discontinuous network, the proportion of the intermediate strong bonding zone needs to be examined. The proportion of the intermediate strong bonding zone is calculated as: W2 / (W1+W2+W3)=610 / (443+610+673)≈0.35. Since this ratio is less than the critical value of 0.45, and observation shows that the number and size of dimples in the intermediate strong bonding zone are small, the interfacial bonding strength of this sample is judged to be low.

[0035] Analysis of the welding mechanism shows that the energy of 26 kJ is relatively low, resulting in insufficient impact velocity of the flyer plate. In the initial stage of welding, the collision angle is small, and the interface energy wave propagation is disordered, failing to form an effective metal jet. This leads to a large and loosely bonded area on the inner side. Due to insufficient overall energy, the time to enter the effective collision angle range is short, resulting in a low proportion of the strong bond area in the middle. The measured average shear force is 859 N, and the average shear work is 0.831 J, verifying the accuracy of the above judgment.

[0036] Example 2: Electromagnetic pulse welding was performed using a discharge energy of 28kJ. Observation of the magnesium cross-section revealed that the thorny texture in the inner weak bonding zone exhibited a partially continuous network distribution, such as... Figure 4 As shown. Measurements revealed the following radial widths for each region: W1 = 471 μm for the inner weak bonding region, W2 = 1158 μm for the middle strong bonding region, and W3 = 720 μm for the outer weak bonding region.

[0037] The proportion of the strong bonding region in the middle was calculated as: W2 / (W1+W2+W3)=1158 / (471+1158+720)≈0.49. This ratio is greater than the critical value of 0.45. Simultaneously, observations revealed a greater number and larger size of dimples in the strong bonding region in the middle, and W2 / W1=1158 / 471≈2.46, meaning W2 is significantly larger than W1. In conclusion, the sample prepared in Example 2 exhibits higher interfacial bonding strength compared to the sample in Example 1.

[0038] Analysis of the welding mechanism shows that the 28kJ energy allowed the flyboard to achieve its optimal speed range. During the mid-welding stage, the collision angle entered its effective range, resulting in intense shear deformation and a continuous metal jet at the interface. This removed the surface oxide film and formed a broad and densely bonded intermediate strong bonding zone. The measured average shear force was 1559N, and the average shear work was 1.368J, the highest among the three groups, verifying the accuracy of the above assessment.

[0039] Example 3: Electromagnetic pulse welding was performed using a discharge energy of 30kJ. Observation of the magnesium cross-section revealed that the thorny patterns in the inner weak bonding zone were distributed in a continuous network, such as... Figure 5As shown. Measurements revealed the following radial widths for each region: inner weak bonding region W1 = 435 μm, middle strong bonding region W2 = 818 μm, and outer weak bonding region W3 = 784 μm.

[0040] When the thorn pattern is distributed in a continuous network, the judgment criteria are more stringent, requiring both W2 / (W1+W2+W3)≥0.45 and W2 / W1≥2 to be satisfied simultaneously. The proportion of the strong bonding zone in the middle is calculated as: W2 / (W1+W2+W3)=818 / (435+818+784)≈0.40, which is less than the critical value of 0.45. Simultaneously, W2 / W1=818 / 435≈1.88, which is less than the critical value of 2. Although observations revealed a large number and size of dimples in the strong bonding zone in the middle, the overall assessment indicates that the interfacial bonding strength is lower than that of the sample prepared in Example 2 due to the decreased proportion of the strong bonding zone.

[0041] Analysis of the welding mechanism shows that the energy of 30kJ is too high, resulting in an excessively large collision angle and severe energy dissipation in the later stages of welding. Although a continuous network of thorny patterns is formed in the initial stage of welding, the excessive energy may lead to localized overburning at the interface or collision angles exceeding the effective range, causing the outer weak bonding zone to widen and compressing the proportion of the middle strong bonding zone, resulting in a decrease in overall bonding performance. The measured average shear force was 1373N and the average shear work was 1.288J, which is indeed lower than that of Example 2, verifying the accuracy of the above judgment.

[0042] The test data and judgment results for each embodiment are shown in Table 1.

[0043] Table 1. Test data and judgment results of interfacial bonding strength of electromagnetic pulse welded aluminum-magnesium composite plates.

[0044]

[0045] As can be seen from the above embodiments, the method provided by the present invention can quickly and accurately determine the interfacial bonding strength of electromagnetic pulse welded aluminum-magnesium composite plates by observing the morphological characteristics of the annular welding zone on the magnesium side section and measuring the radial width of the three regions, and can explain the microscopic mechanism of strength change, which has significant practical value.

[0046] It should be noted that this method can be used for both relative comparisons between samples and for determining the absolute mass based on standard samples.

Claims

1. A method for judging the interface bonding strength of an electromagnetic pulse welded aluminum magnesium composite plate, characterized by, Includes the following steps: Step 1: Select an aluminum plate as the fly plate and a magnesium plate as the base plate, and connect the aluminum plate and the magnesium plate using electromagnetic pulse welding; prepare the first and second samples to be compared respectively. Each sample is an aluminum-magnesium composite plate tensile lap shear test sample, so that the annular welding area of ​​the sample is located in the middle of the lap area of ​​the sample, and perform room temperature tensile tests on each sample respectively. Step 2: Obtain the morphological characteristics of the annular welded area on the magnesium side section of each sample. The annular welded area is divided into three regions from the inside to the outside: the inner weak bonding area, the middle strong bonding area, and the outer weak bonding area. The radial widths W1, W2, and W3 of each region are calculated respectively. Step 3: Based on the distribution morphology of the thorn pattern in the weak bonding area on the inner side of each sample, the radial width ratio, and the dimple distribution characteristics in the strong bonding area in the middle, the interfacial bonding strength of the first and second samples is compared and judged.

2. The method of claim 1, wherein: In step one, the length ratio of the annular welding area to the lap area of ​​the aluminum-magnesium composite plate tensile lap shear specimen is 0.3~0.5, and the width ratio is 0.5~0.

8.

3. The method of claim 1, wherein: In step two, the inner weak bonding area includes tear grooves and a mesh-like thorn pattern that are radially parallel to each other along the annular welding area; the middle strong bonding area includes multiple dimple areas; and the outer weak bonding area includes tear grooves and dispersed tear blocks that are radially parallel to each other along the annular welding area.

4. The method of claim 3, wherein: In step three, when the thorn pattern in the inner weak bonding area of ​​the first sample is distributed in a discontinuous network and its radial width satisfies W2 / (W1+W2+W3)≥0.45, it is determined that the interfacial bonding strength of the first sample is higher than that of the second sample.

5. The method of claim 3, wherein: In step three, when the thorny pattern in the inner weak bonding area of ​​the first sample is distributed in a continuous network and its radial width simultaneously satisfies W2 / (W1+W2+W3)≥0.45 and W2 / W1≥2, it is determined that the interfacial bonding strength of the first sample is higher than that of the second sample.

6. The method of claim 3, wherein: In step three, when the distribution of thorn patterns in the weak bonding areas of the first and second samples is similar, and the radial width relationships W2 / (W1+W2+W3) and W2 / W1 are similar, the distribution of dimples in the strong bonding areas of the two samples is compared. The sample with more dimples and larger sizes has a higher interfacial bonding strength.

7. The method of claim 1, wherein: In step two, the method for calculating the radial width of each region is as follows: The radial width W1 of the inner weak bonding area is the average distance from the inner boundary of the annular welding area to the end of the tear groove and the extension of the thorn pattern. The radial width W2 of the intermediate strong bonding zone is the average distance from the outer boundary of the inner weak bonding zone to the end of the dimple distribution; The radial width W3 of the outer weak bonding zone is the average distance from the outer boundary of the middle strong bonding zone to the extension end of the tear groove and the tear block.