An infrared cut-off filter and its preparation method, and a camera module.

By plasma treatment and coating with a polymer resin aqueous solution on the surface of the light-shielding ink of the infrared cut-off filter, a polymer resin film layer is formed, which solves the problem of high water droplet angle on the surface of the light-shielding ink, improves the bonding force between the ink and the adhesive, and enhances the drop reliability of the camera module.

CN123113069APending Publication Date: 2026-11-17ZHEJIANG CRYSTAL OPTECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611579436.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-13
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

The existing infrared cut-off filter has a high water droplet angle on the surface of the light-shielding ink, resulting in poor adhesive wetting and difficulty in bonding with the chip packaging base, which affects the drop reliability of the camera module.

Method used

By plasma treatment of the surface of the light-shielding ink and coating it with a polymer resin aqueous solution, a polymer resin film layer is formed, which enhances the adhesion between the ink and the adhesive.

Benefits of technology

It significantly reduces the water droplet angle on the surface of the light-shielding ink, improves the adhesion between the ink and the encapsulation adhesive, and enhances the drop reliability of the camera module.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123113069A_ABST
    Figure CN123113069A_ABST
Patent Text Reader

Abstract

This invention discloses an infrared cut-off filter, its preparation method, and a camera module, relating to the field of optical technology. The method includes: providing a filter substrate; screen-printing a light-shielding ink on a peripheral area of ​​a first surface of the filter substrate; performing plasma treatment on the surface of the light-shielding ink to introduce polar groups; coating the surface of the light-shielding ink with an aqueous polymer resin solution; and removing the unadhered aqueous polymer resin solution from the surface of the light-shielding ink to form a polymer resin film layer, thereby obtaining the infrared cut-off filter. This infrared cut-off filter, its preparation method, and the camera module, by sequentially performing plasma treatment and aqueous polymer resin coating on the surface of the light-shielding ink to form a polymer resin film layer, persistently reduce the ink droplet angle and enhance its adhesion to adhesives, thereby improving the drop reliability of the camera module.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of optical technology, and more specifically, to an infrared cutoff filter and its preparation method, and a camera module. Background Technology

[0002] In camera modules, to address color distortion issues, an infrared cut-off filter is typically added to the light path of the image sensor. This filter is generally formed by coating a transparent substrate with an infrared cut-off filter film and / or an anti-reflective film to block infrared light from passing through, thus preventing noise from the image sensor. To limit the effective light-transmitting area of ​​the image sensor, a layer of black light-shielding ink is usually screen-printed on the outer periphery of the infrared cut-off filter. During camera module assembly, the light-shielding ink layer of the infrared cut-off filter is adhered to the chip package substrate using adhesive dispensing.

[0003] However, the surface energy of the light-shielding ink on existing commercially available infrared cut-off filters is low after curing, with a droplet angle generally greater than 60°. The ink surface also has low hydrophilicity, which is detrimental to the sufficient wetting and adhesion of adhesives. In drop tests, separation failure easily occurs between the ink and the adhesive layer, failing to meet the overall reliability requirements of the device. While existing technologies employ plasma treatment to modify the surface of objects, such as plasma treatment of the black matrix pattern of color filters to adjust its surface ink repellency, the purpose, target, and subsequent processes of this treatment are irrelevant to the adhesion problem of the light-shielding ink on infrared cut-off filters. Furthermore, although plasma treatment of the light-shielding ink alone can reduce the droplet angle of the ink surface in a short time, the droplet angle will rebound to greater than 60° after the ink surface is coated with a UV anti-adhesion film, failing to meet the demand for a persistently stable low droplet angle in actual production. Summary of the Invention

[0004] The purpose of this invention is to provide an infrared cut-off filter and its preparation method, as well as a camera module. By sequentially performing plasma treatment and coating with a polymer resin aqueous solution on the surface of the light-shielding ink, a polymer resin thin film layer is formed, which can persistently reduce the ink droplet angle and enhance its adhesion to the adhesive, thereby improving the drop reliability of the camera module.

[0005] The embodiments of the present invention are implemented as follows: A first aspect of this invention provides a method for preparing an infrared cutoff filter, the method comprising: A filter substrate is provided, and a light-shielding ink is screen-printed on a peripheral area of ​​a first surface of the filter substrate; The surface of the light-shielding ink is subjected to plasma treatment to introduce polar groups onto the surface of the light-shielding ink; The surface of the light-shielding ink is coated with an aqueous solution of a polymeric resin, wherein the mass percentage of the aqueous solution of the polymeric resin is 0.1% to 10%, and the polymeric resin is one or more selected from acrylic resin, polyurethane resin, polyester resin, modified cellulose, and polyvinyl alcohol with a degree of hydrolysis of 50% to 99%. Remove the unattached aqueous polymer resin from the surface of the light-shielding ink to form a polymer resin film layer on the surface of the light-shielding ink, thereby obtaining an infrared cut-off filter.

[0006] As one possible implementation, in the plasma treatment, the treatment gas is oxygen, or a mixture of oxygen with one or two of argon and nitrogen; the gas flow rate is 50~500 SCCM; the vacuum degree of the plasma cavity is less than 100 Pa; the treatment power is 50~1000 W; and the treatment time is 5~120 seconds.

[0007] As one possible implementation, the mass percentage of the polymer resin aqueous solution is 0.1% to 5%; the polymer resin is polyvinyl alcohol, and the degree of alcoholysis of the polyvinyl alcohol is 85% to 99%, and the degree of polymerization is 1500 to 2000.

[0008] As one possible implementation, the mass percentage of the polymeric resin aqueous solution is 0.1% to 5%; the polymeric resin is carboxymethyl cellulose, and the degree of substitution of the carboxymethyl cellulose is 0.7 to 0.8, and the degree of polymerization is 7000 to 7500.

[0009] As one possible implementation, after plasma treatment of the surface of the light-shielding ink, the method further includes: Rinse the surface of the light-blocking ink with pure water.

[0010] As one possible implementation, the removal of the unadhered polymeric resin aqueous solution from the surface of the light-shielding ink includes: The unadhered polymer resin aqueous solution on the surface of the light-shielding ink is removed by centrifugal drying.

[0011] As one possible implementation, after forming a polymer resin film layer from the aqueous polymer resin adhering to the surface of the light-shielding ink, the method further includes: A UV-resistant anti-adhesion film is coated on the polymer resin film layer.

[0012] As one possible implementation, before screen printing light-blocking ink on the peripheral area of ​​the first surface of the filter substrate, the method further includes: An infrared cut-off filter film is formed on the first surface of the filter substrate, and an anti-reflection film is formed on the second surface of the filter substrate; or, an anti-reflection film is formed on the first surface of the filter substrate, and an infrared cut-off filter film is formed on the second surface of the filter substrate.

[0013] In one possible implementation, the filter substrate includes a plurality of effective light-transmitting areas and a peripheral area, the peripheral area surrounding the periphery of the plurality of effective light-transmitting areas, and one effective light-transmitting area corresponding to one infrared cut-off filter. The method further includes: Laser cutting is performed at the midpoint of the outer region between two adjacent effective light-transmitting areas.

[0014] In a second aspect, an infrared cut-off filter is provided, prepared by the above-described method for preparing an infrared cut-off filter, comprising a filter substrate, a light-shielding ink layer disposed on a peripheral region of a first surface of the filter substrate, and a polymer resin film layer disposed on the surface of the light-shielding ink layer; the polymer resin film layer is made of one or more of acrylic resin, polyurethane resin, polyester resin, modified cellulose, and polyvinyl alcohol with a degree of hydrolysis of 50% to 99%; the water droplet angle on the surface of the light-shielding ink layer is less than or equal to 35°.

[0015] A third aspect of the present invention provides a camera module, including a chip packaging base and the aforementioned infrared cut-off filter, wherein the light-shielding ink layer of the infrared cut-off filter is bonded to the chip packaging base by adhesive.

[0016] The beneficial effects of the embodiments of the present invention include: This application involves sequentially performing plasma treatment and coating with a specific polymer resin aqueous solution at a mass percentage of 0.1% to 10% after screen printing light-shielding ink. This effectively anchors the polar groups introduced by the plasma treatment on the ink surface to the polymer resin film layer, preventing the polar groups from migrating into the ink. As a result, a durable and stable low droplet angle (≤35°) is formed on the surface of the light-shielding ink, significantly enhancing the adhesion between the light-shielding ink and the encapsulation adhesive, and reducing the risk of ink and adhesive layer separation failure in drop tests. Attached Figure Description

[0017] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly introduced below. It should be understood that the following drawings only show some embodiments of the present invention and should not be regarded as a limitation on the scope. For those skilled in the art, other related drawings can be obtained based on these drawings without creative effort.

[0018] Figure 1This is a schematic diagram illustrating the fabrication process of the infrared cutoff filter provided in an embodiment of the present invention. Figure 2 This is a schematic diagram of the structure of the infrared cut-off filter provided in an embodiment of the present invention; Figure 3 This is a schematic diagram of the structure of an infrared cutoff filter provided in an embodiment of the present invention.

[0019] Icons: 10-Filter substrate; 20-Light-shielding ink layer; 30-Polymer resin film layer; 40-UV anti-adhesion film; 50-Infrared cut-off filter film; 60-Antireflective film. Detailed Implementation

[0020] The embodiments described below represent the information necessary for those skilled in the art to practice the embodiments and illustrate the best mode for practicing the embodiments. After reading the following description with reference to the accompanying drawings, those skilled in the art will understand the concepts of this disclosure and will recognize the application of these concepts not specifically set forth herein. It should be understood that these concepts and applications fall within the scope of this disclosure and the appended claims.

[0021] It should be understood that when an element (such as a layer, region, or substrate) is referred to as "on another element" or "extending to another element," it may be directly on another element or directly extending to another element, or there may be an intermediate element. Similarly, it should be understood that when an element (such as a layer, region, or substrate) is referred to as "on another element" or "extending over another element," it may be directly on another element or directly extending to another element, or there may be an intermediate element.

[0022] The terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit this disclosure. As used herein, the singular forms “a,” “an,” and “the” are intended to include the plural forms as well, unless the context clearly indicates otherwise. It should also be understood that, when used herein, the term “comprising” indicates the presence of the stated feature, integer, step, operation, element, and / or component, but does not exclude the presence or addition of one or more other features, integers, steps, operations, elements, components, and / or groups of the foregoing.

[0023] Unless otherwise defined, all terms used herein (including technical and scientific terms) have the same meaning as commonly understood by one of ordinary skill in the art to which this disclosure pertains. It should also be understood that the terms used herein should be interpreted as having the same meaning as they would in the context of this specification and the relevant field, and not in an idealized or overly formal sense, unless expressly defined herein.

[0024] Please refer to the reference. Figures 1 to 3 In a first aspect, this application provides a method for preparing an infrared cutoff filter, the method comprising: S100: Provide a filter substrate 10 and screen print light-shielding ink on the peripheral area of ​​the first surface of the filter substrate 10. S200. Plasma treatment is performed on the surface of the light-shielding ink to introduce polar groups onto the surface of the light-shielding ink. S300. Coating the surface of a light-shielding ink with a polymer resin aqueous solution, wherein the polymer resin aqueous solution has a mass percentage of 0.1% to 10%, and the polymer resin is one or more of acrylic resin, polyurethane resin, polyester resin, modified cellulose, and polyvinyl alcohol with a degree of alcoholysis of 50% to 99%. S400: Remove the unattached polymer resin aqueous solution from the surface of the light-shielding ink, so that the polymer resin aqueous solution attached to the surface of the light-shielding ink forms a polymer resin film layer 30, thereby obtaining an infrared cut-off filter.

[0025] It should be noted that the method for preparing the infrared cut-off filter provided in this application mainly addresses the problem of insufficient adhesion reliability between the light-shielding ink on the periphery of the infrared cut-off filter and the chip packaging base of the camera module. During the camera module assembly process, the light-shielding ink layer 20 is bonded to the chip packaging base via dispensing. However, the light-shielding ink on existing commercially available infrared cut-off filters has low surface energy after curing, with a droplet angle generally greater than 60°. The ink surface has low hydrophilicity, which is not conducive to sufficient wetting and adhesion of the adhesive. In drop tests, separation failure easily occurs between the ink and the adhesive layer. This application uses a combined process of "plasma treatment and polymer resin aqueous solution coating" to form a polymer resin film layer 30 on the surface of the light-shielding ink, persistently reducing the droplet angle of the ink surface, thereby significantly enhancing the adhesion between the light-shielding ink and the packaging adhesive, and improving the drop reliability of the camera module.

[0026] Specifically, light-shielding ink is first screen-printed on the peripheral area of ​​the first surface of the filter substrate 10. The filter substrate 10 can be a glass substrate, a plastic substrate, or a flexible substrate, preferably a glass substrate with high heat resistance. The light-shielding ink is used to define the effective light-transmitting area of ​​the image sensor. The screen printing process is a conventional screen printing process in the art. After curing, the light-shielding ink forms a light-shielding ink layer 20 on the peripheral area of ​​the first surface. The material and curing conditions of the light-shielding ink layer 20 are well known in the art, and this application does not impose any special limitations on them.

[0027] Secondly, the surface of the opaque ink undergoes plasma treatment. The purpose of plasma treatment is to ionize the treatment gas into plasma using a high-voltage electric field. This plasma contains high-energy particles such as ions, electrons, and free radicals. These high-energy particles react with the non-polar groups on the surface of the opaque ink, introducing polar groups such as hydroxyl, carbonyl, and carboxyl groups, thereby increasing the surface energy of the ink and transforming its surface from hydrophobic to hydrophilic. Simultaneously, plasma treatment also cleans and roughens the ink surface, removing organic contaminants and forming a micro-rough structure, providing more anchoring points for the subsequent adhesion of the polymer resin film layer 30.

[0028] However, while plasma treatment alone can significantly reduce the water droplet angle of light-shielding ink to below 60° in a short period, the angle rebounds to above 60° after UV-resistant adhesive tape is applied to the ink surface. This is because the polar groups (hydroxyl, carbonyl, carboxyl, etc.) introduced into the ink surface after plasma treatment are in a high-energy state and tend to migrate and rearrange into the ink interior. According to the polar group inversion model, these polar groups gradually migrate into the material, reducing surface energy and causing the plasma treatment effect to gradually disappear. Therefore, plasma treatment alone cannot meet the demand for a persistently stable low water droplet angle in actual production.

[0029] For the reasons mentioned above, this application further utilizes a polymer resin aqueous solution to coat the surface of the light-shielding ink after plasma treatment. The polymer resin in the aqueous solution is firmly anchored to the plasma-activated ink surface through hydrogen bonding, van der Waals forces, or chemical bonding between polar groups, forming an extremely thin polymer resin film layer 30 on the ink surface. This polymer resin film layer 30, on the one hand, "locks in" the polar groups such as hydroxyl, carbonyl, and carboxyl groups formed on the ink surface after plasma treatment, preventing their migration into the ink interior, thereby maintaining a low water droplet angle on the ink surface; on the other hand, the polymer resin film layer 30 itself is rich in polar groups, and its exposed polar groups can chemically crosslink or strongly interact with the active groups in the subsequently coated encapsulating adhesive, forming a "molecular bridge" between the ink and the adhesive, thereby significantly enhancing the bonding force between the light-shielding ink and the encapsulating adhesive.

[0030] Furthermore, this application only treats the surface of the light-shielding ink without altering its intrinsic chemical structure, weather resistance, or adhesion to the filter substrate 10. Compared to replacing existing inks with more hydrophilic inks, this application reduces the water droplet angle on the ink surface while retaining the excellent weather resistance of existing inks.

[0031] The mass percentage of the polymer resin aqueous solution is 0.1% to 10%. If the concentration is too low, a complete and uniform resin film layer cannot be formed on the ink surface, resulting in insufficient anchoring effect on polar groups; if the concentration is too high, the resin film layer will be too thick, which may affect the optical properties and appearance of the light-shielding ink and cause waste of raw materials. The polymer resin is selected from one or more of acrylic resin, polyurethane resin, polyester resin, modified cellulose, and polyvinyl alcohol with a degree of hydrolysis of 50% to 99%. The above-mentioned polymer resins all have abundant polar groups (such as hydroxyl, carboxyl, amino, etc.), which can form a stable film layer on the ink surface and form a strong bond with the encapsulating adhesive. Among them, the degree of hydrolysis of polyvinyl alcohol is 50% to 99%. The higher the degree of hydrolysis, the higher the hydroxyl content on the molecular chain, the stronger the polarity, and the stronger the binding force with the polar groups on the ink surface; however, excessively high hydrolysis may lead to a decrease in water solubility, so a degree of hydrolysis of 85% to 99% is preferred.

[0032] The coating method can be brushing, soaking, spraying, roller coating, or spin coating, as long as the polymer resin aqueous solution can fully wet and cover the surface of the opaque ink. After coating, the unadhered polymer resin aqueous solution on the surface of the opaque ink is removed, allowing the polymer resin aqueous solution adhering to the ink surface to form a polymer resin film layer 30. Removal methods can include centrifugal drying, air knife blowing, natural air drying, or heat drying. By removing the unadhered solution, the uniformity and controllable thickness of the polymer resin film layer 30 can be ensured, avoiding uneven film thickness or ink surface contamination caused by solution residue.

[0033] As one possible implementation method, in plasma treatment, the treatment gas is oxygen, or a mixture of oxygen with one or two of argon and nitrogen; the gas flow rate is 50~500 SCCM; the vacuum degree of the plasma cavity is less than 100 Pa; the treatment power is 50~1000 W; the treatment time is 5~120 seconds; and the plasma treatment is carried out using vacuum plasma at room temperature.

[0034] It should be noted that oxygen or an oxygen-containing mixture is chosen as the treatment gas because oxygen can generate a large number of oxygen free radicals and ozone in the plasma state. These active species can react with the non-polar groups on the ink surface to efficiently introduce polar groups such as hydroxyl, carbonyl, and carboxyl groups, thereby significantly improving the hydrophilicity and surface energy of the ink surface. Argon, as an inert gas, mainly physically roughens the ink surface through ion bombardment in the plasma state, increasing surface roughness and active sites; nitrogen can introduce nitrogen-containing polar groups such as amino groups on the ink surface. Therefore, a mixture of oxygen and argon and / or nitrogen can have both chemical activation and physical roughening effects, further enhancing the plasma treatment effect. The gas flow rate is 50~500 SCCM. If the flow rate is too low, the plasma concentration will be insufficient, and the treatment effect will be limited; if the flow rate is too high, it will waste gas and may cause excessive etching to the ink surface. The vacuum degree of the plasma chamber is less than 100 Pa. If the vacuum degree is too high, it will be difficult to generate plasma stably; if the vacuum degree is too low, the plasma density will be insufficient. The processing power is 50~1000W. If the power is too low, the plasma energy will be insufficient and the ink surface cannot be effectively activated; if the power is too high, it may lead to excessive etching or even damage to the ink surface. The processing time is 5~120 seconds. If the time is too short, the processing will be insufficient; if the time is too long, the efficiency will decrease and the ink surface may age. Vacuum plasma is used at room temperature, and the process conditions are mild, which will not cause thermal damage to the infrared cut-off filter film 50, antireflection film 60, and light-shielding ink layer 20 on the filter substrate 10, thus ensuring the optical performance and structural integrity of the filter.

[0035] As one possible implementation method, the mass percentage of the polymer resin aqueous solution is 0.1% to 5%; the polymer resin is polyvinyl alcohol, the degree of alcoholysis of polyvinyl alcohol is 85% to 99%, and the degree of polymerization is 1500 to 2000.

[0036] It should be noted that polyvinyl alcohol (PVA) is a water-soluble polymer with a large number of hydroxyl groups in its molecular chain, exhibiting excellent film-forming properties and a high density of polar groups. PVA with a degree of hydrolysis of 85%–99% has a high hydroxyl content and abundant polar groups in its molecular chain, enabling it to form strong hydrogen bonds on the ink surface. Simultaneously, the exposed hydroxyl groups can chemically cross-link with the epoxy and hydroxyl groups in the encapsulating adhesive, forming a strong interfacial bond. PVA with a degree of polymerization of 1500–2000 has a moderate molecular chain length, which allows for the formation of a continuous and uniform film layer without causing excessively high viscosity of the aqueous solution and difficulties in coating due to excessively long molecular chains. A PVA aqueous solution with a mass percentage of 0.1%–5% has a moderate concentration, ensuring the formation of a complete film layer on the ink surface without causing an excessively thick film layer due to excessive concentration, which would affect the optical properties of the ink. Experiments show that treating the ink surface with a 1% (w / w) aqueous solution of polyvinyl alcohol with a 99% degree of hydrolysis and a 1700 degree of polymerization can reduce the water droplet angle of the ink surface to 30°; treating the ink surface with a 0.1% (w / w) aqueous solution of polyvinyl alcohol with an 88% (w / w) degree of hydrolysis and a 1700 degree of polymerization can reduce the water droplet angle of the ink surface to 32°.

[0037] As one possible implementation method, the mass percentage of the polymer resin aqueous solution is 0.1% to 5%; the polymer resin is carboxymethyl cellulose, the degree of substitution of carboxymethyl cellulose is 0.7 to 0.8, and the degree of polymerization is 7000 to 7500.

[0038] It should be noted that carboxymethyl cellulose is a water-soluble polymer obtained by carboxylation modification of cellulose, and its molecular chain contains a large number of carboxymethyl groups (-CH2COO). - Carboxymethyl cellulose (CMC) contains hydroxyl groups, exhibiting excellent hydrophilicity and film-forming properties. With a degree of substitution of 0.7–0.8, an average of 0.7–0.8 hydroxyl groups are replaced by carboxymethyl groups on each glucose unit. This moderate density of polar groups ensures both good water solubility and sufficient polar groups to form a strong bond with the ink surface and adhesive. CMC with a degree of polymerization of 7000–7500 has a longer molecular chain, enabling the formation of a continuous and dense film layer, resulting in better anchoring of polar groups on the ink surface. Experiments show that treating the ink surface with a 1% (w / w) aqueous solution of CMC with a degree of substitution of 0.7–0.8 and a degree of polymerization of 7200 can reduce the water droplet angle of the ink surface to 35°.

[0039] As one possible implementation, after plasma treatment of the surface of the light-shielding ink in step S200, the method further includes: S500: Use pure water to rinse the surface of the opaque ink.

[0040] It should be noted that after plasma treatment, some loose particles, low-molecular-weight fragments, or unreacted byproducts generated during the plasma treatment process may remain on the ink surface. If these residues are not removed, they may affect the effective contact between the subsequent polymer resin aqueous solution and the ink surface, reducing the adhesion quality of the resin film layer. Rinsing the ink surface with pure water can effectively remove these residues, keeping the ink surface clean and ensuring that the polymer resin aqueous solution can fully wet the ink surface and form a strong bond with the polar groups on the ink surface. Pure water rinsing can be done by spraying, soaking, or ultrasonic cleaning. After rinsing, it can be dried with compressed air or allowed to air dry naturally.

[0041] As one possible implementation, S400, removing the unadhered polymeric resin aqueous solution from the surface of the light-shielding ink, includes: S401. Use centrifugal drying to remove unadhered polymer resin aqueous solution from the surface of the light-shielding ink.

[0042] It should be noted that centrifugal drying is a highly efficient and uniform removal method. The centrifugal force generated by high-speed rotation removes the unattached polymer resin aqueous solution from the ink surface, while the polymer resin aqueous solution adhering to the ink surface forms a uniform, extremely thin film layer under the combined action of centrifugal force and surface tension. The centrifugal speed and time can be adjusted according to the concentration and viscosity of the polymer resin aqueous solution; for example, the speed can be 1000~5000 rpm, and the time can be 10~60 seconds. After centrifugal drying, there is no liquid accumulation or dripping on the ink surface, and the film layer thickness is uniform, which helps ensure the uniformity and consistency of the water droplet angle on the ink surface. Furthermore, centrifugal drying can be used in conjunction with heating drying to accelerate the drying and curing of the film layer.

[0043] like Figure 2 and Figure 3 As shown, in one possible implementation, after forming a polymer resin film layer 30 from the polymer resin aqueous solution adhering to the surface of the light-shielding ink in step S400, the method further includes: S600, A UV anti-adhesion film 40 is coated on the polymer resin film layer 30.

[0044] It should be noted that the UV anti-adhesion film 40 is a pressure-sensitive tape whose tackiness decreases after ultraviolet irradiation. It is mainly used to protect the polymer resin film layer 30 on the ink surface during filter cutting, transportation, and storage, preventing scratches, contamination, or damage to the film layer. After applying the UV anti-adhesion film 40, its tackiness can be reduced by ultraviolet irradiation during subsequent filter use, making it easy to peel off from the film layer surface without damaging the polymer resin film layer 30. The inventors discovered that if the ink is only subjected to plasma treatment without polymer resin aqueous solution treatment, the water droplet angle on the ink surface after applying the UV anti-adhesion film 40 will rebound to greater than 60°; however, after polymer resin aqueous solution treatment, the water droplet angle on the ink surface after applying the UV anti-adhesion film 40 remains stable at around 30°, far less than 60°, indicating that the polymer resin film layer 30 can effectively resist the migration of polar groups and surface energy rebound caused by the UV anti-adhesion film 40.

[0045] like Figure 2 and Figure 3 As shown, in one possible implementation, before screen printing light-shielding ink on the peripheral area of ​​the first surface of the filter substrate 10 in step S100, the method further includes: S700, an infrared cut-off filter film 50 is formed on the first surface of the filter substrate 10, and an anti-reflection film 60 is formed on the second surface of the filter substrate 10; or, an anti-reflection film 60 is formed on the first surface of the filter substrate 10, and an infrared cut-off filter film 50 is formed on the second surface of the filter substrate 10.

[0046] It should be noted that the infrared cut-off filter 50 is used to block infrared light from passing through, preventing noise from the image sensing element; the anti-reflection film 60 is used to increase the transmittance of visible light and reduce light reflection loss. The infrared cut-off filter 50 and the anti-reflection film 60 are formed on different surfaces of the filter substrate 10, and since they have different functions, they are not formed on the same surface. Both the infrared cut-off filter 50 and the anti-reflection film 60 can be formed using conventional vacuum deposition processes in the art, such as electron beam evaporation, magnetron sputtering, or ion-assisted deposition. The material, thickness, and number of layers of the film can be designed according to the actual optical performance requirements, and this application does not impose any special limitations on this. By forming the infrared cut-off filter 50 and the anti-reflection film 60 on both sides of the filter substrate 10, the infrared cut-off filter can simultaneously possess infrared cut-off and visible light enhancement functions, meeting the optical performance requirements of the camera module. In other embodiments, an infrared cut-off filter film 50 may be formed only on the first surface of the filter substrate 10, or an antireflection film 60 may be formed only on the second surface of the filter substrate 10. This application does not impose any special limitations on this.

[0047] In one possible implementation, the filter substrate 10 includes a plurality of effective light-transmitting areas and a peripheral area, the peripheral area surrounding the periphery of the plurality of effective light-transmitting areas, and one effective light-transmitting area corresponding to one infrared cut-off filter. The method further includes: S800, laser cutting is performed along the middle position of the outer area between two adjacent effective light-transmitting areas.

[0048] It should be noted that in actual production, large-area filter substrates 10 are typically used for batch processing. The substrate is divided into multiple effective light-transmitting areas, each corresponding to an infrared cut-off filter. An outer region surrounds each effective light-transmitting area, and light-shielding ink is screen-printed on this outer region, separating the effective light-transmitting areas. After completing steps such as plasma treatment, polymer resin aqueous solution coating, centrifugal drying, and UV anti-adhesion film 40 coating, a laser is used to cut along the middle of the outer region between two adjacent effective light-transmitting areas, dividing the large-area substrate into multiple independent infrared cut-off filters. Laser cutting has advantages such as high cutting precision, narrow kerf, and small heat-affected zone, ensuring the flatness and dimensional accuracy of the cut edges and avoiding damage to the light-shielding ink layer 20 and the polymer resin film layer 30. The cutting position is located in the middle of the outer region between two adjacent effective light-transmitting areas, ensuring that each infrared cut-off filter retains sufficient light-shielding ink layer 20 at its edge, meeting the light-shielding requirements.

[0049] like Figure 2 and Figure 3 As shown, this application embodiment also provides an infrared cut-off filter, which is prepared by the above-described method for preparing an infrared cut-off filter. It includes a filter substrate 10, a light-shielding ink layer 20 disposed on the peripheral region of the first surface of the filter substrate 10, and a polymer resin film layer 30 disposed on the surface of the light-shielding ink layer 20. The polymer resin film layer 30 is made of one or more of acrylic resin, polyurethane resin, polyester resin, modified cellulose, and polyvinyl alcohol with a degree of hydrolysis of 50% to 99%. The water droplet angle on the surface of the light-shielding ink layer 20 is less than or equal to 35°.

[0050] It should be noted that, thanks to the polymer resin film layer 30, the water droplet angle on the surface of the light-shielding ink layer 20 of this infrared cut-off filter can be consistently maintained below 35°, far lower than the level of over 60° on the surface of the light-shielding ink of existing commercially available infrared cut-off filters. The low water droplet angle indicates that the surface of the light-shielding ink layer 20 has good hydrophilicity, which is beneficial for the encapsulating adhesive to fully wet and spread on the ink surface, thereby forming a strong bonding interface between the light-shielding ink layer 20 and the adhesive, reducing the risk of ink and adhesive separation failure during drop tests. The polymer resin film layer 30 is disposed on the surface of the light-shielding ink layer 20, and its material is one or more of acrylic resin, polyurethane resin, polyester resin, modified cellulose, and polyvinyl alcohol with a degree of alcoholysis of 50%~99%. These polymer resins all have abundant polar groups, which can form a stable film layer on the ink surface and form a strong chemical bond or strong intermolecular interaction with the encapsulating adhesive. The polymer resin film layer 30 is extremely thin, typically ranging from nanometer to submicron thickness, and will not affect the light-shielding performance of the light-shielding ink layer 20 or the appearance of the filter.

[0051] This application embodiment also provides a camera module, including a chip packaging base and the aforementioned infrared cut-off filter, wherein the light-shielding ink layer 20 of the infrared cut-off filter is bonded to the chip packaging base by adhesive.

[0052] It should be noted that the chip packaging base in the camera module serves to support the image sensor and provide a mounting foundation for the infrared cut-off filter. The infrared cut-off filter is bonded to the chip packaging base with adhesive via a polymer resin film layer 30 on the surface of its light-shielding ink layer 20. Because the polymer resin film layer 30 is rich in polar groups, it can form strong chemical bonds or strong intermolecular interactions with the active groups in the adhesive, thereby significantly improving the adhesion strength between the light-shielding ink layer 20 and the chip packaging base. In drop tests of the camera module, the light-shielding ink layer 20 and the adhesive layer are unlikely to separate, effectively ensuring the overall reliability of the camera module.

[0053] The technical solutions and effects of this application will be described in detail below through specific embodiments and comparative examples.

[0054] Comparative Example 1 Referring to the current scheme, light-shielding ink is screen-printed and cured on the outer area of ​​the first surface of the filter substrate 10 without plasma treatment or polymer resin aqueous solution treatment, and the water droplet angle on the ink surface is tested to be 70°.

[0055] Comparative Example 2 After screen printing and curing light-shielding ink on the outer area of ​​the first surface of the filter substrate 10, only the surface of the light-shielding ink is subjected to plasma treatment, without polymer resin aqueous solution treatment, and the water droplet angle on the ink surface is tested to be 65°.

[0056] Example 1 After screen printing and curing the light-shielding ink on the outer region of the first surface of the filter substrate 10, the surface of the light-shielding ink is subjected to plasma treatment; then, a 1% (w / w) polyvinyl alcohol aqueous solution is used to coat the ink surface, wherein the degree of alcoholysis of polyvinyl alcohol is 99% and the degree of polymerization is 1700; after centrifugation and drying, the water droplet angle of the ink surface is tested to be 30°.

[0057] Example 2 After screen printing and curing the light-shielding ink on the outer region of the first surface of the filter substrate 10, the surface of the light-shielding ink is subjected to plasma treatment; then, the ink surface is coated with a 0.1% (w / w) polyvinyl alcohol aqueous solution, wherein the degree of alcoholysis of polyvinyl alcohol is 88% and the degree of polymerization is 1700; after centrifugation and drying, the water droplet angle of the ink surface is tested to be 32°.

[0058] Example 3 After screen printing and curing the light-shielding ink on the outer region of the first surface of the filter substrate 10, the surface of the light-shielding ink is subjected to plasma treatment; then, the ink surface is coated with a 1% (w / w) aqueous solution of carboxymethyl cellulose, wherein the degree of substitution of carboxymethyl cellulose is 0.7~0.8 and the degree of polymerization is 7200; after centrifugation and drying, the water droplet angle of the ink surface is tested to be 35°.

[0059] The test results from Comparative Examples 1 to 3 show that the water droplet angle on the surface of the untreated opaque ink was 70° (Comparative Example 1), the water droplet angle on the surface of the opaque ink treated only with plasma was 65° (Comparative Example 2), while the water droplet angle on the surface of the opaque ink treated with "plasma treatment and polymer resin aqueous solution treatment" could be reduced to 30°~35° (Examples 1 to 3). This indicates that the combined process of plasma treatment and polymer resin aqueous solution treatment in this application can significantly reduce the water droplet angle on the surface of opaque ink. In particular, although plasma treatment alone in Comparative Example 2 can reduce the water droplet angle on the ink surface in a short time, the water droplet angle is greater than 60° again after the ink surface is covered with UV anti-adhesion tape; while in Examples 1 to 3, after treatment with polymer resin aqueous solution, the water droplet angle on the ink surface is still stable at 30°~35° after being covered with UV anti-adhesion tape, which is much less than 60°. This indicates that the polymer resin film layer 30 can effectively "lock" the polar groups formed on the surface of the ink after plasma treatment, preventing them from migrating into the ink, thereby achieving a long-lasting and stable low water droplet angle effect.

[0060] The above are merely optional embodiments of this application and are not intended to limit this application. Various modifications and variations can be made to this application by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the protection scope of this application.

[0061] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable way without contradiction. In order to avoid unnecessary repetition, this application will not describe the various possible combinations separately. At the same time, the various embodiments of this application can be combined with each other. As long as they do not violate the spirit of this application, they should also be regarded as the content disclosed in this application.

Claims

1. A method for preparing an infrared cutoff filter, characterized in that, The method includes: A filter substrate is provided, and a light-shielding ink is screen-printed on a peripheral area of ​​a first surface of the filter substrate; The surface of the light-shielding ink is subjected to plasma treatment to introduce polar groups onto the surface of the light-shielding ink; The surface of the light-shielding ink is coated with an aqueous solution of a polymeric resin, wherein the mass percentage of the aqueous solution of the polymeric resin is 0.1% to 10%, and the polymeric resin is one or more selected from acrylic resin, polyurethane resin, polyester resin, modified cellulose, and polyvinyl alcohol with a degree of hydrolysis of 50% to 99%. Remove the unattached aqueous polymer resin from the surface of the light-shielding ink to form a polymer resin film layer on the surface of the light-shielding ink, thereby obtaining an infrared cut-off filter.

2. The method for preparing the infrared cutoff filter according to claim 1, characterized in that, In the plasma treatment, the treatment gas is oxygen, or a mixture of oxygen with one or two of argon and nitrogen; the gas flow rate is 50~500 SCCM; the vacuum degree of the plasma cavity is less than 100 Pa; the treatment power is 50~1000 W; and the treatment time is 5~120 seconds.

3. The method for preparing the infrared cutoff filter according to claim 1, characterized in that, The mass percentage of the polymer resin aqueous solution is 0.1% to 5%; the polymer resin is polyvinyl alcohol, and the degree of alcoholysis of the polyvinyl alcohol is 85% to 99%, and the degree of polymerization is 1500 to 2000.

4. The method for preparing the infrared cutoff filter according to claim 1, characterized in that, The mass percentage of the aqueous solution of the polymeric resin is 0.1% to 5%; the polymeric resin is carboxymethyl cellulose, and the degree of substitution of the carboxymethyl cellulose is 0.7 to 0.8, and the degree of polymerization is 7000 to 7500.

5. The method for preparing the infrared cutoff filter according to claim 1, characterized in that, After plasma treatment of the surface of the light-shielding ink, the method further includes: Rinse the surface of the light-blocking ink with pure water.

6. The method for preparing the infrared cutoff filter according to claim 1, characterized in that, The aqueous polymeric resin solution used to remove the unadhered polymeric resin from the surface of the light-shielding ink includes: The unadhered polymer resin aqueous solution on the surface of the light-shielding ink is removed by centrifugal drying.

7. The method for preparing the infrared cutoff filter according to claim 1, characterized in that, After forming a polymer resin film layer from the aqueous polymer resin solution adhering to the surface of the light-shielding ink, the method further includes: A UV-resistant anti-adhesion film is coated on the polymer resin film layer.

8. The method for preparing the infrared cutoff filter according to claim 1, characterized in that, Before screen printing light-shielding ink on the peripheral area of ​​the first surface of the filter substrate, the method further includes: An infrared cut-off filter film is formed on the first surface of the filter substrate, and an anti-reflection film is formed on the second surface of the filter substrate; or, an anti-reflection film is formed on the first surface of the filter substrate, and an infrared cut-off filter film is formed on the second surface of the filter substrate.

9. The method for preparing the infrared cutoff filter according to claim 1, characterized in that, The filter substrate includes multiple effective light-transmitting areas and a peripheral area, the peripheral area surrounding the periphery of the multiple effective light-transmitting areas, and one effective light-transmitting area corresponds to one infrared cut-off filter. The method further includes: Laser cutting is performed along the middle position of the outer region between two adjacent effective light-transmitting areas.

10. An infrared cutoff filter, characterized in that, The infrared cutoff filter is prepared by the method described in any one of claims 1 to 9, comprising a filter substrate, a light-shielding ink layer disposed on a peripheral region of a first surface of the filter substrate, and a polymer resin film layer disposed on the surface of the light-shielding ink layer; the polymer resin film layer is made of one or more of acrylic resin, polyurethane resin, polyester resin, modified cellulose, and polyvinyl alcohol with a degree of hydrolysis of 50% to 99%; the water droplet angle on the surface of the light-shielding ink layer is less than or equal to 35°.

11. A camera module, characterized in that, The device includes a chip packaging base and the infrared cut-off filter as described in claim 10, wherein the light-shielding ink layer of the infrared cut-off filter is bonded to the chip packaging base by adhesive.