A non-shaped core optical fiber and its fabrication method
By performing multi-angle side polishing and fused tapering combined with torsion treatment on double-clad optical fibers, irregular core optical fibers were prepared, solving the problems of precision and integration in the preparation of irregular core optical fibers in the prior art, and realizing efficient mode field transformation and vortex light generation.
Patent Information
- Application Number
- CN202611144343.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-30
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies make it difficult to fabricate complex geometric shapes of optical fibers with high precision, low cost, and high efficiency. Furthermore, the generation of vortex light heavily relies on free-space optical systems, making it impossible to achieve full fiber integration.
By polishing the double-clad fiber from multiple angles to form a non-circular irregular inner cladding, and then combining it with a quartz capillary melt tapering and twisting treatment, an irregular core fiber is prepared, achieving efficient mode field coupling and vortex light generation.
It achieves efficient mode field transformation and all-fiber integration of vortex light, improving the integration and optical performance of optical fibers, and is suitable for high-power laser transmission, fiber optic sensing and quantum communication.
Smart Images

Figure CN123113086A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to an irregularly shaped fiber core and its fabrication method. Specifically, it relates to an irregularly shaped fiber core with various cross-sections such as elliptical, triangular, square, hexagonal, and octagonal, and its fabrication method, which can be used in optical application systems such as high-power laser transmission, fiber optic sensing, and vortex light generation. It belongs to the field of special fiber fabrication technology. Background Technology
[0002] Specialty optical fibers play an irreplaceable role in fields such as fiber optic sensing, optical imaging, high-power lasers, and quantum communication due to their unique optical properties. Among them, irregularly shaped core fibers (such as elliptical, triangular, square, hexagonal, and octagonal core cross-sections) can achieve functions such as maintaining polarization, specific mode field distribution, large mode field area, or generating orbital angular momentum (OAM) vortex light. Their unique advantages in beam shaping, energy homogenization, high-power laser transmission, and multi-core few-mode transmission have made them an important research direction in the field of specialty optical fiber fabrication.
[0003] However, existing methods for preparing irregularly shaped optical fiber preforms still have many shortcomings in terms of processing accuracy, process stability, and cost control. The specific existing technical solutions and their limitations are as follows.
[0004] By aligning the drill bit's rotation axis with the geometric axis of the circular cavity cladding sleeve, a square cavity cladding sleeve can be obtained by drilling a rounded square hole with its width as the side length into a brittle material such as quartz glass. A square core rod is then inserted into this sleeve and stretched or fused into a solid circular rod, ultimately fabricating a square-core optical fiber preform according to the designed refractive index profile. Chinese invention patent application number CN117756397B, "A Method, Product, and Apparatus for Preparing a Square-Core Optical Fiber Preform," provides a method for coaxially drilling square cladding sleeves using a Reilly triangular drill bit. This scheme utilizes the Reilly triangle's fixed width principle, which to some extent reduces the core-cladding interface gas line problem caused by the combination of square mandrels and circular sleeves in wire drawing. However, this method still has significant shortcomings: First, it relies on a dedicated Reilly triangle drill bit for mechanical drilling of the cladding sleeve, making the process relatively complex. The drilling accuracy is directly limited by the drill bit's manufacturing precision and the coaxial alignment precision of the processing device. The difference in side length between the mandrel and the sleeve must be strictly controlled within a narrow range of 1.0 to 4.0 mm to ensure a good match. Second, the drilling and grinding processes require an additional grinding oil supply device, making the overall processing steps cumbersome and highly dependent on equipment. Third, the drilling method is only suitable for single square or near-square structures, and its ability to expand to more complex polygonal irregular cores such as triangles and hexagons is limited, making it difficult to adapt to the flexible fabrication needs of various irregular cross-sectional shapes.
[0005] Shaped optical fibers can be obtained by precision grinding and splicing of irregularly shaped quartz tubing and multi-core rods. Cylindrical core rods are finely ground into hexagonal or other polygonal cross-sections. Pure quartz preforms are then finely polished into irregularly shaped quartz preforms according to the shape of the gaps created after the core rods are assembled. Multiple core rod blanks are then tightly spliced with the irregularly shaped quartz preforms without gaps. After being fitted with a cladding quartz tube, a large-size multi-core few-mode optical fiber preform can be formed. The Chinese invention patent CN113979631A, entitled "Method for Preparing Large-Size Multi-Core Optical Fiber Preforms Based on Perfect Combination of Irregularly Shaped Tubes," achieves gapless filling between core rods through irregularly shaped quartz filling components. This solves, to some extent, the problems of insufficient gaps, uneven heating leading to poor length consistency, and high costs in the preparation of multi-core optical fiber preforms. However, it still has significant shortcomings: the irregularly shaped quartz filling components are custom-polished according to the specific gap shape generated after the core rods are assembled. Each assembly scheme, such as honeycomb, triangular, and square structures, requires redesigning the processing surface of the filling components, resulting in poor process versatility and high mold and polishing costs. This type of solution is mainly aimed at multi-core optical fiber structure design, and the core rods themselves are still ground into circles or simple polygons. It does not fundamentally solve the problems of poor concentricity and geometric consistency between a single irregularly shaped core (such as a square core) and a circular cladding tube.
[0006] In the fabrication of optical fiber preforms, capillary / rod stacking and die extrusion molding are common methods. Capillary rods are filled into the gaps between polygonal capillary components, and a multi-module tube-laying device is used to arrange and fix the circular and polygonal components in an orderly manner, forming a stacked structure with irregular cross-sections. Chinese invention patent application CN113979631A, "A method for fabricating photonic crystal fiber preforms and its tube-laying device," proposes this method. However, this type of stacking method relies on the dimensional consistency and arrangement accuracy among a large number of capillary tubes, capillary rods, and tube-laying modules. Even slight deviations during stacking can introduce structural defects, and the stability and efficiency of stacking are still limited by the mechanical adjustment capabilities of the stacking device. Meanwhile, the extrusion molding method requires high precision in die surface accuracy and coordinated control of process parameters such as extrusion temperature and pressure. Layering defects, porosity, or cross-sectional deformation are prone to occur during the process, necessitating additional anti-rotation and anti-rotation structures to suppress these defects. Regardless of whether it is stacking or extrusion, the overall accuracy of its irregular cross-section is still inferior to that of mechanical grinding or precision assembly. Its applicability to irregular core structures with complex shapes and high precision requirements (such as asymmetric polygonal cores) is limited. Moreover, extrusion is mostly used for circular or simple structure preforms with adjustable core-cladding ratios, and has not yet fully covered the needs for mass production and high-precision fabrication of complex irregular cores.
[0007] The application scenarios of vortex beam generation place new technological demands on the fabrication of irregularly shaped optical fibers. Vortex beams carrying orbital angular momentum (OAM) have significant application value in high-bandwidth optical communication, optical manipulation, precision measurement, and imaging due to their mode orthogonality and theoretically infinite mode dimensions. Efficiently and stably generating vortex beams is a core technological challenge for related systems. However, current technologies heavily rely on spatial optical elements (such as spiral phase plates, spatial light modulators, and q-plates) to convert the Gaussian beam output from traditional lasers into vortex beams. This method requires high alignment accuracy, suffers from poor environmental stability, and is difficult to integrate with all-fiber systems.
[0008] In summary, traditional methods struggle to fabricate solid, complex geometrically shaped, and mode-field-controllable irregular-core optical fibers (such as triangular, square, and octagonal fibers) with high precision, low cost, and high efficiency. Existing technologies often compromise on flexibility, mechanical strength, or optical performance, failing to simultaneously meet the requirements of high-intensity, low-loss, and high-efficiency mode-field coupling. Furthermore, the generation of vortex light heavily relies on free-space optical systems, making it impossible to achieve a structurally stable, all-fiber integrated vortex light source.
[0009] The present invention aims to overcome the shortcomings of the prior art and provide a non-circular core optical fiber with flexible process, stable structure, high-efficiency mode field coupling and direct generation of vortex light, and its preparation method. Summary of the Invention
[0010] The purpose of this invention is to provide a non-circular core optical fiber with flexible structure, high efficiency in preparation, stable performance and the ability to directly generate vortex light, and a method for preparing the same.
[0011] The objective of this invention is achieved as follows:
[0012] The irregular core fiber is prepared by multi-angle side polishing of double-clad fiber. The cross-section of the inner cladding of the side-polished section of the double-clad fiber is polished into a non-circular irregular shape. This section is inserted into a quartz capillary tube and, after high-temperature negative pressure fusion shrinking and tapering, the double-clad fiber and the quartz capillary tube are fused together. The original core of the double-clad fiber gradually becomes thinner and no longer has the ability to confine light waves. The light waves gradually transition to the thinner irregular inner cladding for transmission. The thinner irregular inner cladding becomes the new core. After the overall cross-section is scaled to a suitable proportion and the diameter is kept uniform, the fiber is drawn to obtain the irregular core fiber.
[0013] The double-clad optical fiber has a three-layer quartz structure consisting of a single-mode core, an inner cladding, and an outer cladding. After the quartz capillary is subjected to negative pressure melting and tapering, the core shape of the resulting shaped core optical fiber is similar to the inner cladding shape formed by multi-angle side polishing of the double-clad optical fiber.
[0014] The double-clad fiber can achieve mode field matching with the standard single-mode fiber. After tapering to form a non-standard core fiber, the standard single-mode mode field can be thermally transitioned to the non-standard core through the tapered region, forming a new non-standard mode field and achieving efficient mode field transformation.
[0015] The irregularly shaped fiber can be rotated during the drawing process, transforming the irregularly shaped core into a helical irregularly shaped core, resulting in a helical irregularly shaped fiber. The drawn fiber is then twisted to generate vortexes of different orders based on the fiber core's geometric characteristics.
[0016] The twisting process is characterized by the following: the twisting rate and twisting angle are controlled according to the geometric characteristics of the fiber core. For example, the twisting of a triangular fiber core generates ℓ=±1 order vortex light, and the twisting of a square fiber core generates ℓ=±2 order vortex light. The twisting can be performed online or offline during fiber drawing and supports OAM mode transmission.
[0017] The fabrication steps of the irregular core optical fiber are as follows: Step 1: Select a double-clad optical fiber, remove a suitable length of coating, and then perform side polishing to create a flat surface on the cylindrical optical fiber. Step 2: Rotate the double-clad fiber and side-polish another plane at the same position. Multiple planes can be side-polished in this way until the inner cladding of the double-clad fiber cross-section forms a preset geometric shape, such as an elliptical, triangular, square, hexagonal, or octagonal irregular inner cladding structure. Step 3: Insert the side-thrown region of the double-clad fiber into a quartz capillary tube, melt and shrink it under high temperature and negative pressure conditions, and then slowly draw it to a suitable outer diameter. Keep the diameter and draw a section of fiber to form a non-shaped core fiber.
[0018] The characteristic of the rotation angle grinding is that the rotation angle and grinding thickness of the double-clad optical fiber are controlled by a precision rotating fixture to form 2-8 planes, corresponding to irregular structures such as elliptical (2 planes), triangular (3 planes), square (4 planes), hexagonal (6 planes) or octagonal (8 planes), ensuring that the inner cladding part is deformed while the fiber core and outer cladding remain intact.
[0019] Advantages of this invention: simple and flexible process, avoiding the defects of traditional methods; irregular structure ensures efficient mode field coupling; twisting treatment realizes all-fiber vortex light generation, improving integration. It can be used for high-power laser transmission, fiber optic sensing, and quantum communication.
[0020] This invention organically integrates the fabrication of irregular structures, the drawing of high-performance optical fibers, and the generation of vortex light through a process route of "side polishing—capillary sizing—fusion strengthening—fiber drawing—torsion empowerment," forming a continuous and controllable process. This method not only overcomes the shortcomings of traditional technologies, such as high loss, poor flexibility, and low strength, but also proposes a solution to directly generate vortex light in an all-fiber by combining the geometric symmetry of the fiber core with torsion. This provides a core component for next-generation high-performance, integrated fiber lasers and optical communication systems. Attached Figure Description
[0021] Figure 1 is a flowchart of the overall process for fabricating the irregularly shaped core optical fiber of the present invention. The optical fiber is formed by rotating and grinding the inner cladding portion of a double-clad optical fiber to create multiple planes (taking an elliptical shape as an example), which are then inserted into a quartz capillary tube. After high-temperature rod shrinking and tapering processes, an optical fiber with a corresponding irregularly shaped core is fabricated. Furthermore, by twisting the optical fiber, vortexes of different orders can be generated according to the geometric characteristics of the core.
[0022] Figure 2 This is a schematic diagram of the structure of an integrated solid irregular-shaped preform formed after high-temperature melting and shrinkage.
[0023] Figure 3 This is a schematic diagram of the cross-sectional structure of the preform 7 (taking the elliptical core as an example) after being ground and inserted into the quartz capillary tube 8.
[0024] Figure 4 These are schematic diagrams illustrating various irregular cross-sectional structures formed after double-clad optical fiber preforms undergo processes such as rotational grinding, capillary assembly, high-temperature melting and shrinking, and fiber drawing and twisting. 1. Original circular double-clad preform cross-section; 2. Elliptical-like cross-section formed after grinding two symmetrical planes; 3. Triangular-like cross-section formed after grinding three planes; 4. Square-like cross-section formed after grinding four planes; 5. Hexagonal-like cross-section formed after grinding six planes; 6. Hexagonal-like cross-section formed after grinding eight planes.
[0025] Figure 5 This is a schematic diagram of the cross-sectional structure of the irregular core optical fiber 9 (taking an elliptical core as an example) finally prepared by this invention.
[0026] Figure 6 is a schematic diagram of the vortex light field generated at the output end of the optical fiber after the twisting process.
[0027] Figure 7 This is a schematic diagram of a specific embodiment of the present invention, illustrating the application of the irregular core fiber as a gain medium in an all-fiber integrated vortex laser. Detailed Implementation
[0028] The present invention will be further illustrated below with reference to specific embodiments. It should be noted that the following embodiments are only for illustrating the technical solutions of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
[0029] Example 1: Fabrication of an elliptical core optical fiber capable of generating first-order vortex optical fibers
[0030] This embodiment describes in detail the fabrication process of an elliptical core optical fiber for generating first-order vortex light (topological charge number ℓ=±1).
[0031] Step 1: Preform processing and grinding Take a section of quartz double-clad optical fiber. Using a side polishing system, fix the fiber onto a precision rotary fixture. On a 10 cm section of bare fiber with the coating removed, control the rotation speed and polishing length, while simultaneously monitoring the remaining thickness in real time using "one-click perfect side polishing technology." After polishing a flat surface, rotate the precision rotary fixture 180° for a second polishing, ultimately creating two symmetrical flat surfaces, forming a near-elliptical cross-section. After polishing, perform a final polish to ensure a smooth surface free of obvious scratches.
[0032] Step 2: Capillary assembly Select a pure quartz capillary tube with an outer diameter of 1000 μm and an inner diameter of 130 μm. Slowly insert the elliptical preform prepared in step S1 into the capillary tube, ensuring that the side-polishing zone of the elliptical structure is located in the central region of the capillary tube. Use high-temperature resistant quartz adhesive to temporarily fix the preform at both ends of the capillary tube to prevent displacement of the preform during subsequent high-temperature treatment.
[0033] Step 3: High-temperature melting and shrinkage The assembled "elliptical preform-capillary" structure is vertically placed above the feeder of the fiber drawing tower. It is then slowly fed into the drawing furnace, where the temperature is stabilized at 1980℃. At this high temperature, the quartz material softens, allowing the outer wall of the capillary and the inner preform to fully melt and form a single unit. The elliptical structure inside the capillary maintains its shape under surface tension, forming a solid, integrated elliptical preform. During this process, a small amount of dry chlorine gas is continuously introduced for dehydration.
[0034] Step 4: Tapering and wire drawing After fusion shrinkage is completed, the drawing tower parameters are adjusted to stabilize the furnace temperature at 1950℃. The fused preform is fed down at a rate of 5 mm per minute, and the fiber is drawn at a rate of 1 m per second. Using this 1:200 drawing ratio, the irregular structure of the preform is perfectly scaled to the fiber scale, ultimately producing an elliptical core fiber with an outer diameter of 125 μm. The fiber's geometry and optical consistency are monitored in real time using a diameter gauge and an optical monitoring system.
[0035] Step 5: Twisting treatment The drawn elliptical core fiber is passed around two precisely positioned clamps, one of which is fixed, while the other is mounted on a precision turntable that can be rotated by a motor. The turntable is started to permanently twist a 1-meter section of fiber at a twisting rate of 3 rad / m. Under the shear stress generated by the torsion, the geometric anisotropy of the elliptical core introduces helical refractive index modulation, thereby breaking the mode degeneracy and effectively exciting a first-order (ℓ=±1) orbital angular momentum vortex.
[0036] Verification of results: A 1550 nm distributed feedback (DFB) laser was used to inject light into the twisted elliptical core fiber. After collimation, the output light field was projected onto a camera for observation, and a clear ring-shaped light spot could be seen. Furthermore, the output light was made to interfere with a planar reference light, and a characteristic pattern with a fork-shaped fringe was observed in the interference pattern, confirming that the output light is a vortex light with a topological charge of ℓ = ±1.
[0037] Example 2: Fabrication of a square-core fiber capable of generating second-order vortex optical fibers
[0038] This embodiment describes the fabrication process of a square-core optical fiber for generating second-order vortex light (topological charge number ℓ = ±2).
[0039] Step 1. Preform processing and grinding: Similar to Example 1, but in this step, after each plane is ground, the precision rotary fixture is adjusted to rotate 90°. After three rotations, four symmetrical planes are ground, ultimately forming a square cross-sectional structure.
[0040] Step 2: Capillary assembly The same quartz capillary tubes (130 μm / 1000 μm) were used.
[0041] Step 3: High-temperature melting and shrinkage The high-temperature treatment temperature and process are the same as in Example 1, forming an integrated elliptical preform.
[0042] Step 4: Tapering and wire drawing The fiber drawing process parameters were the same as in Example 1, and a square-core optical fiber with an outer diameter of 125 μm was finally drawn.
[0043] Step 5: Twisting treatment Due to the fourfold rotational symmetry of the square core, a higher torsion rate is required to excite higher-order vortex modes. A 1-meter-long square-core fiber was permanently torsioned at a torsion rate of 6 rad / m. This torsion rate matches the fourfold rotational symmetry of the square core and can effectively excite second-order (ℓ=±2) orbital angular momentum vortices.
[0044] Effect verification: Using the same test method as in Example 1, a larger diameter annular spot with zero central light intensity was observed at the output end; its interference pattern with the reference light showed two forked patterns, confirming it as a second-order vortex light with a topological charge number ℓ = ±2.
[0045] In summary, this invention achieves the fabrication of optical fibers with complex irregular core structures through a process flow of "rotational angle polishing, capillary assembly, high-temperature melting, tapering and drawing, and twisting treatment," while simultaneously generating vortex light. This method offers advantages such as a clear process, high material utilization, strong controllability, and the ability to realize fully integrated optical fiber devices, opening new avenues for the application of high-performance specialty optical fibers.
Claims
1. A profiled core optical fiber, characterized by: The irregular core fiber is prepared by multi-angle side polishing of double-clad fiber. The cross-section of the inner cladding of the side-polished section of the double-clad fiber is polished into a non-circular irregular shape. This section is inserted into a quartz capillary tube and, after high-temperature negative pressure fusion shrinking and tapering, the double-clad fiber and the quartz capillary tube are fused together. The original core of the double-clad fiber gradually becomes thinner and no longer has the ability to confine light waves. The light waves gradually transition to the thinner irregular inner cladding for transmission. The thinner irregular inner cladding becomes the new core. After the overall cross-section is scaled to a suitable proportion and the diameter is kept uniform, the fiber is drawn to obtain the irregular core fiber.
2. A hetero-core optical fiber according to claim 1, characterized in that: The double-clad optical fiber has a three-layer quartz structure consisting of a single-mode core, an inner cladding, and an outer cladding. After the quartz capillary is subjected to negative pressure melting and tapering, the core shape of the resulting shaped core optical fiber is similar to the inner cladding shape formed by multi-angle side polishing of the double-clad optical fiber.
3. A hetero-core optical fiber according to claim 1, characterized in that: The double-clad fiber can achieve mode field matching with the standard single-mode fiber. After tapering to form a non-standard core fiber, the standard single-mode mode field can be thermally transitioned to the non-standard core through the tapered region, forming a new non-standard mode field and achieving efficient mode field transformation.
4. The specialty core fiber of claim 1, wherein: The irregular core fiber can be rotated during the drawing process, and the irregular core is processed into a spiral irregular core to obtain a spiral irregular core fiber.
5. A method of making a profiled core optical fiber, characterized by: The fabrication steps of the irregular core optical fiber are as follows: Step 1: Select a double-clad optical fiber, remove a suitable length of coating, and then perform side polishing to create a flat surface on the cylindrical optical fiber. Step 2: Rotate the double-clad fiber and side-polish another plane at the same position. Repeat this process to side-polish multiple planes until the inner cladding of the double-clad fiber cross-section forms the preset geometry. Step 3: Insert the side-thrown region of the double-clad fiber into a quartz capillary tube, melt and shrink it under high temperature and negative pressure conditions, and then slowly draw it to a suitable outer diameter. Keep the diameter and draw a section of fiber to form a non-shaped core fiber.
Citation Information
Patent Citations
Preparation method of large-size multi-core optical fiber preform rod based on perfect combination of special-shaped bushing
CN113979631A
A method of making a square core optical fiber preform, product and apparatus
CN117756397B