Design Methods for Sulfate-Resistant Concrete Cementitious Materials in Hydraulic Engineering

By classifying and determining the level of sulfate corrosion in water and the lithological risk of aggregates, and by adopting cementitious material systems adapted to different working conditions, the problem of sulfate erosion in water conservancy and hydropower projects in Northwest China has been solved, improving the durability and design efficiency of concrete and reducing costs.

CN123120134APending Publication Date: 2026-11-17NORTHWEST ENGINEERING CORPORATION LIMITED
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611267976.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-20
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies cannot effectively adapt to sulfate erosion under various working conditions in Northwest China, resulting in poor concrete durability, low design efficiency, and high material costs.

Method used

By classifying and determining the level of sulfate corrosion in water and the lithological risk of aggregates, different erosion conditions are identified, and different combinations of cementitious material systems are adopted, including P•O42.5, P.MSR42.5, P.HSR42.5 cement and fly ash, combined with sulfate-resistant corrosion inhibitors, to form cementitious material systems suitable for different working conditions.

Benefits of technology

It improves the corrosion resistance of concrete, reduces the cost of engineering materials, enhances design efficiency, and ensures long-term service reliability.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention discloses a design method for cementitious materials in hydraulic engineering concrete resistant to sulfate corrosion. The method includes a tiered assessment of sulfate corrosion levels in water, aggregate lithological risk, and corrosion conditions. The tiered assessment results include weak sulfate corrosion + alkali-free aggregate reaction, weak sulfate corrosion + alkali-containing aggregate reaction, moderate sulfate corrosion, strong sulfate corrosion, freeze-thaw sulfate coupled corrosion, and aggregate TSA corrosion. Finally, based on the tiered assessment results, a cementitious material system adapted to different working conditions is formed. This invention designs a cementitious material system in layers according to weak / moderate / strong / coupled corrosion scenarios. For weak corrosion scenarios, ordinary silicate cement is used in combination with fly ash to control costs. For moderate / strong corrosion and coupled corrosion scenarios, special cement or matching anti-corrosion admixtures are selected to enhance concrete durability, adapting to multiple working environments and effectively controlling raw material costs while meeting the long-term service durability requirements of hydraulic concrete.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the technical field of concrete durability design for water conservancy and hydropower projects, and relates to a design method for cementitious materials for hydraulic concrete resistant to sulfate attack. Background Technology

[0002] Northwest my country has large areas of saline land and high-altitude salt lakes. The soil and water in these areas are rich in sulfates, and the temperature difference between day and night is extremely large, with severe winters. Most engineering concrete structures in this region, such as dam panels, underground powerhouses, roads, bridges, and tunnels, are in long-term contact with sulfate-containing soil and water, which will be subject to sulfate erosion and freeze-thaw damage, seriously endangering the service life of concrete and posing safety hazards to the building structure.

[0003] Currently, the technical methods used in water conservancy and hydropower projects in Northwest my country to address sulfate erosion can be mainly divided into three categories: (1) Fixed concrete mix proportion scheme: The vast majority of related patents and engineering schemes are fixed mix proportions, which uniquely limit the dosage of cement, fly ash, slag and admixtures, and are only suitable for single water quality and single aggregate conditions. There is no universal design process.

[0004] (2) Single disease-specific technology: only develops for a single destructive factor, such as only developing sulfate-resistant preservatives or only inhibiting alkali-aggregate reaction, which cannot take into account multiple coupled corrosion.

[0005] (3) Standard and specification clause guidance: Standards such as DL / T 5801 and DL / T 5151 only specify single test and inspection methods, and do not form a complete design process from site survey → raw material screening → durability verification → scenario-specific selection. Engineering design is highly dependent on personnel experience.

[0006] The core shortcomings of existing technologies for addressing sulfate corrosion can be summarized in the following aspects: (1) Poor versatility and unable to adapt to the diverse working conditions in Northwest China. Multiple overlapping problems exist at water conservancy and hydropower project sites in Northwest China: medium / high concentration sulfate-laden water, reactive excavated aggregates, coupled damage from freeze-thaw sulfate, and TSA erosion. Existing formulations can only cope with single conditions; different cement types and different lithological aggregates require retesting when facing different concentrations of ambient water, resulting in low design efficiency.

[0007] (2) No screening process for cement selection The application scenarios of the four types of cement, namely P•O (ordinary Portland cement), P•MH (medium-heat Portland cement), P.MSR (medium-sulfate resistant Portland cement), and P.HSR (high-sulfate resistant Portland cement), were not distinguished. The cement was not selected according to the sulfate concentration. In some highly corrosive projects, ordinary Portland cement with low fly ash content was used. The corrosion resistance coefficient has a low safety reserve, and there are risks in long-term operation.

[0008] (3) Lack of economic stratification selection logic To ensure project quality, the plan prioritized the use of high sulfur-resistant cement and did not establish specific working conditions such as "moderate corrosion, strong corrosion, freeze-thaw sulfate coupling, and TSA (carbon-sulfur-silicon-calcium-stone type sulfate attack)," resulting in a significant increase in project material costs. Summary of the Invention

[0009] The purpose of this invention is to provide a design method for cementitious materials for sulfate-resistant concrete in hydraulic engineering, which solves the problems that existing sulfate-resistant concrete cementitious materials cannot adapt to various working conditions and have poor corrosion resistance.

[0010] The technical solution adopted in this invention is a design method for cementitious materials of hydraulic concrete resistant to sulfate corrosion. This method includes classifying and determining the level of sulfate corrosion in water, the lithological risk of aggregates, and the corrosion conditions. The classification and determination results include weak sulfate corrosion + non-alkali aggregate reaction, weak sulfate corrosion + alkali aggregate reaction, moderate sulfate corrosion, strong sulfate corrosion, freeze-thaw sulfate coupled corrosion, and aggregate TSA corrosion. Finally, a cementitious material system adapted to different working conditions is formed based on the classification and determination results.

[0011] Among them, the classification determines the degree of sulfate corrosion in water, when SO4 in the water 2- <400 mg / L, classified as weak sulfate corrosion; when SO4 ≤ 400 mg / L in water... 2- <600 mg / L, classified as moderate sulfate attack, when SO4 in the water 2- A concentration of ≥600 mg / L is considered strong sulfate attack.

[0012] Aggregate lithology risk includes the presence or absence of alkali-aggregate reaction and the presence or absence of TSA erosion. The presence or absence of alkali-aggregate reaction is determined by the mortar bar rapid method, and limestone aggregate is marked as having TSA erosion risk.

[0013] The erosion conditions are divided into single sulfate erosion and freeze-thaw sulfate coupled erosion.

[0014] When the grading result is weak sulfate attack + alkali-free aggregate reaction, the corresponding cementitious material system is P•O42.5 cement + 15%~20% fly ash. When the grading result is weak sulfate attack + alkali-containing aggregate reaction, the corresponding cementitious material system is P•O42.5 cement + 20%~25% fly ash.

[0015] When the grading result is moderate sulfate attack + with / without alkali aggregate reaction, the corresponding cementitious material system is P•O42.5 / P.MSR42.5 cement + 20%~25% fly ash. When the grading result is strong sulfate attack + with / without alkali aggregate reaction, the corresponding cementitious material system is P•O42.5 cement + 20%~25% fly ash + 3%~12% sulfate-resistant corrosion inhibitor, or P•MH42.5 / P.MSR42.5 / P.HSR42.5 cement + 20~25% fly ash.

[0016] When the grading result is freeze-thaw sulfate coupled erosion + alkali-aggregate reaction with or without alkali, the corresponding cementitious material system is P•MH42.5 / P.MSR42.5 / P.HSR42.5 cement + 20%~25% fly ash. When the grading result is aggregate TSA erosion + alkali-aggregate reaction with or without alkali, the corresponding cementitious material system is P•MH42.5 / P.MSR42.5 / P.HSR42.5 cement + 25%~35% fly ash.

[0017] The classification determines the degree of sulfate corrosion in water. When SO4 in the water... 2- When the concentration is ≥2000mg / L, the corresponding cementitious material system is P•MH42.5 / P.MSR42.5 / P.HSR42.5 cement + 30~35% fly ash.

[0018] The fly ash in the cementitious material system is either Class II or Class I fly ash (F-type), and the C3A content in the P•O42.5 cement clinker is 5%~8%.

[0019] When the classification result is weak sulfate attack, the corrosion resistance coefficient K of the cementitious material system is ≥0.8. When the classification result is moderate sulfate attack, strong sulfate attack, or freeze-thaw sulfate coupled attack, the corrosion resistance coefficient K of the cementitious material system is ≥0.85.

[0020] The beneficial effects of this invention are as follows: (1) According to the layered design and selection scheme of weak / medium / strong / coupled erosion: ordinary silicate cement and fly ash are used to control costs in weak corrosion scenarios; special cement or matching anti-corrosion admixtures are used to enhance the durability of concrete in medium / strong corrosion and coupled erosion scenarios, and the cost of raw materials is effectively controlled under the premise of meeting the long-term service durability of hydraulic concrete. (2) All tests are performed in accordance with DL and GB standards. The tests can be completed by the on-site laboratory and the design institute's testing equipment. There is no need to customize non-standard equipment. It can be directly promoted and applied in various water conservancy and hydropower projects in Northwest China. It has strong versatility and practicality. (3) Based on specific working conditions, six sets of cementitious materials for hydraulic engineering anti-sulfate erosion concrete were developed, which improved the efficiency of concrete mix design by more than 60%. (4) The corrosion resistance coefficient K of the cementitious material system is limited to 0.8 in weak sulfate erosion environment and 0.85 in medium sulfate erosion, strong sulfate erosion or freeze-thaw sulfate coupled erosion environment. By imposing constraints through quantitative indicators, the problem of insufficient durability safety reserve caused by empirical design is avoided, and the long-term service reliability of hydraulic concrete is significantly improved. Detailed Implementation

[0021] The present invention will now be described in detail with reference to specific embodiments.

[0022] Example 1 A design method for cementitious materials used in hydraulic engineering to resist sulfate attack includes the following steps: Step 1: Determine the sulfate corrosion level, aggregate lithology risk, and erosion conditions in the construction environment based on the classification of working conditions; Step 1.1, Water quality testing: Determine the SO4 content in water samples from the construction environment. 2- Concentration of SO4 in water 2- <400 mg / L, classified as weak sulfate corrosion; Step 1.2, aggregate lithological risks include the presence or absence of alkali-aggregate reaction and the presence or absence of TSA erosion; The presence of alkali-aggregate reaction (ASR) is determined using the rapid mortar bar method, also known as the rapid mortar bar method. This involves preparing mortar specimens from aggregates and high-alkali cement, immersing them in a high-temperature (typically 80±2℃) sodium hydroxide solution to accelerate the ASR. The change in specimen length is measured to determine if the aggregates exhibit potentially hazardous activity. If the 14-day expansion rate is ≤0.10%, the aggregates are considered to have no potential alkali activity; if it is ≥0.20%, they exhibit hazardous activity; if 0.10% < expansion rate < 0.20%, further assessment is required, combining this with other tests or extending the curing period. Limestone aggregate is marked as having a risk of TSA erosion, while the rest are marked as having no risk of TSA erosion. TSA (Thin-Sulphurous Sulfate) corrosion refers to the corrosion of CSH gel. Unlike traditional sulfate corrosion, TSA directly destroys the CSH gel, rather than generating expansive products that damage its essence. TSA directly decomposes the CSH gel, transforming it into non-cementing CSH gel, thus losing its binding ability. Unlike traditional sulfate corrosion, this process does not rely on expansive products to cause cracking. The product, CSH gel, is characterized by a white, muddy appearance, a loose structure, and lack of strength, seriously affecting engineering safety and service life.

[0023] Step 1.3, Classification of erosion conditions: single sulfate erosion, freeze-thaw sulfate coupled erosion (i.e., freeze-thaw cycle and sulfate erosion coexist). After testing, the construction environment in this embodiment was a single sulfate attack, specifically a weak sulfate attack + no alkali aggregate reaction, and no risk of aggregate TSA attack. Step 2: Based on the classification results, form a cementitious material system suitable for different working conditions; Because the construction environment in this embodiment is weak sulfate erosion + no alkali aggregate reaction, there is no risk of aggregate TSA erosion. The cementitious material system is P•O42.5 cement + 15%~20% fly ash (that is, the weight percentage of fly ash in the cementitious material system is 15%~20%, and the rest is P•O42.5 cement).

[0024] In this embodiment, the corrosion resistance coefficient K of the cementitious material system is ≥0.8, the tricalcium aluminate (C3A) content of P•O42.5 cement clinker in the cementitious material system is 5%, and the fly ash is Class F, Grade II fly ash.

[0025] Example 2 A design method for cementitious materials used in hydraulic engineering to resist sulfate attack includes the following steps: Step 1: Determine the sulfate corrosion level, aggregate lithology risk, and erosion conditions in the construction environment based on the classification of working conditions; Step 1.1, Water quality testing: Determine the SO4 content in water samples from the construction environment. 2- Concentration of SO4 in water 2- <400 mg / L, classified as weak sulfate corrosion; Step 1.2, aggregate lithological risks include the presence or absence of alkali-aggregate reaction and the presence or absence of TSA erosion; The presence or absence of alkali-aggregate reaction was determined using the mortar bar rapid method. Limestone aggregate was marked as having a risk of TSA erosion, while the rest were marked as not having a risk of TSA erosion. Step 1.3, Classification of erosion conditions: single sulfate erosion, freeze-thaw sulfate coupled erosion; After testing, the construction environment in this embodiment was a single sulfate attack, specifically a weak sulfate attack plus an alkaline aggregate reaction, with no risk of aggregate TSA attack. Step 2: Based on the classification results, form a cementitious material system suitable for different working conditions; Because the construction environment in this embodiment is weak sulfate erosion + alkali aggregate reaction, there is no risk of aggregate TSA erosion, the cementitious material system is P•O42.5 cement + 20%~25% fly ash (that is, the weight percentage of fly ash in the cementitious material system is 20%~25%, and the rest is P•O42.5 cement).

[0026] In this embodiment, the corrosion resistance coefficient K of the cementitious material system is ≥0.8, the tricalcium aluminate (C3A) content of P•O42.5 cement clinker in the cementitious material system is 6%, and the fly ash is Class F, Grade II fly ash.

[0027] Example 3 A design method for cementitious materials used in hydraulic engineering to resist sulfate attack includes the following steps: Step 1: Determine the sulfate corrosion level, aggregate lithology risk, and erosion conditions in the construction environment based on the classification of working conditions; Step 1.1, Water quality testing: Determine the SO4 content in water samples from the construction environment. 2- Concentration, SO4 in water ≤ 400 2- <600 mg / L, classified as moderate sulfate attack; Step 1.2, aggregate lithological risks include the presence or absence of alkali-aggregate reaction and the presence or absence of TSA erosion; The presence or absence of alkali-aggregate reaction was determined using the mortar bar rapid method. Limestone aggregate was marked as having a risk of TSA erosion, while the rest were marked as not having a risk of TSA erosion. Step 1.3, Classification of erosion conditions: single sulfate erosion, freeze-thaw sulfate coupled erosion; After testing, the construction environment in this embodiment was a single sulfate attack, specifically a moderate sulfate attack + no alkali aggregate reaction, and no risk of aggregate TSA attack. Step 2: Based on the classification results, form a cementitious material system suitable for different working conditions; Because the construction environment in this embodiment is moderate sulfate attack + no alkali aggregate reaction, there is no risk of aggregate TSA attack. The cementitious material system is P•O42.5 cement + 20%~25% fly ash (that is, the weight percentage of fly ash in the cementitious material system is 20%~25%, and the rest is P•O42.5 cement).

[0028] In this embodiment, the corrosion resistance coefficient K of the cementitious material system is ≥0.85, the tricalcium aluminate (C3A) content of P•O42.5 cement clinker in the cementitious material system is 7%, and the fly ash is Class I fly ash of type F.

[0029] Example 4 A design method for cementitious materials used in hydraulic engineering to resist sulfate attack includes the following steps: Step 1: Determine the sulfate corrosion level, aggregate lithology risk, and erosion conditions in the construction environment based on the classification of working conditions; Step 1.1, Water quality testing: Determine the SO4 content in water samples from the construction environment. 2- Concentration, SO4 in water ≤ 400 2- <600 mg / L, classified as moderate sulfate attack; Step 1.2, aggregate lithological risks include the presence or absence of alkali-aggregate reaction and the presence or absence of TSA erosion; The presence or absence of alkali-aggregate reaction was determined using the mortar bar rapid method. Limestone aggregate was marked as having a risk of TSA erosion, while the rest were marked as not having a risk of TSA erosion. Step 1.3, Classification of erosion conditions: single sulfate erosion, freeze-thaw sulfate coupled erosion; After testing, the construction environment in this embodiment was a single sulfate attack, specifically a moderate sulfate attack plus alkali aggregate reaction, with no risk of aggregate TSA attack. Step 2: Based on the classification results, form a cementitious material system suitable for different working conditions; Because the construction environment in this embodiment is moderate sulfate erosion + alkali aggregate reaction, and there is no risk of aggregate TSA erosion, the cementitious material system uses P.MSR42.5 cement + 20%~25% fly ash (that is, the weight percentage of fly ash in the cementitious material system is 20%~25%, and the rest is P.MSR42.5 cement).

[0030] In this embodiment, the corrosion resistance coefficient K of the cementitious material system is ≥0.85, and the fly ash in the cementitious material system is Class F Grade I fly ash.

[0031] Example 5 A design method for cementitious materials used in hydraulic engineering to resist sulfate attack includes the following steps: Step 1: Determine the sulfate corrosion level, aggregate lithology risk, and erosion conditions in the construction environment based on the classification of working conditions; Step 1.1, Water quality testing: Determine the SO4 content in water samples from the construction environment. 2- Concentration of SO4 in water 2- ≥600 mg / L is considered strong sulfate attack; Step 1.2, aggregate lithological risks include the presence or absence of alkali-aggregate reaction and the presence or absence of TSA erosion; The presence or absence of alkali-aggregate reaction was determined using the mortar bar rapid method. Limestone aggregate was marked as having a risk of TSA erosion, while the rest were marked as not having a risk of TSA erosion. Step 1.3, Classification of erosion conditions: single sulfate erosion, freeze-thaw sulfate coupled erosion; After testing, the construction environment in this embodiment was a single sulfate attack, specifically strong sulfate attack + non-alkali aggregate reaction, with no risk of aggregate TSA attack. Step 2: Based on the classification results, form a cementitious material system suitable for different working conditions; Because the construction environment in this embodiment is strong sulfate attack + no alkali aggregate reaction, there is no risk of aggregate TSA attack. The cementitious material system is P•O42.5 cement + 20%~25% fly ash + 3%~12% sulfate-resistant corrosion inhibitor (that is, the weight percentage of fly ash in the cementitious material system is 20%~25%, the weight percentage of sulfate-resistant corrosion inhibitor is 3%~12%, and the rest is P•O42.5 cement).

[0032] In the event of strong sulfate attack, in addition to specialized sulfate-resistant corrosion inhibitors, silica fume and nano-calcium carbonate mineral modifiers can be used to replace organic corrosion inhibitors and compounded in ordinary silicate cement systems to achieve the same sulfate resistance enhancement effect.

[0033] In this embodiment, the corrosion resistance coefficient K of the cementitious material system is ≥0.85, and the fly ash is Class F Grade I fly ash.

[0034] Example 6 A design method for cementitious materials used in hydraulic engineering to resist sulfate attack includes the following steps: Step 1: Determine the sulfate corrosion level, aggregate lithology risk, and erosion conditions in the construction environment based on the classification of working conditions; Step 1.1, Water quality testing: Determine the SO4 content in water samples from the construction environment. 2- Concentration of SO4 in water 2- ≥2000 mg / L is considered strong sulfate attack; Step 1.2, aggregate lithological risks include the presence or absence of alkali-aggregate reaction and the presence or absence of TSA erosion; The presence or absence of alkali-aggregate reaction was determined using the mortar bar rapid method. Limestone aggregate was marked as having a risk of TSA erosion, while the rest were marked as not having a risk of TSA erosion. Step 1.3, Classification of erosion conditions: single sulfate erosion, freeze-thaw sulfate coupled erosion; After testing, the construction environment in this embodiment was a single sulfate attack, specifically strong sulfate attack + alkali aggregate reaction, with no risk of aggregate TSA attack. Step 2: Based on the classification results, form a cementitious material system suitable for different working conditions; Because the construction environment in this embodiment is characterized by strong sulfate attack and alkali-aggregate reaction, with no risk of aggregate TSA attack, the cementitious material system uses P•MH42.5 / P.MSR42.5 / P.HSR42.5 cement + 30~35% fly ash (i.e., the weight percentage of fly ash in the cementitious material system is 30%~35%, and the remainder is P•MH42.5 / P.MSR42.5 / P.HSR42.5 cement), and the water-cement ratio is reduced by 0.03~0.05 to enhance density and inhibit ion penetration.

[0035] In this embodiment, the corrosion resistance coefficient K of the cementitious material system is ≥0.85, and the fly ash is Class F Grade I fly ash.

[0036] Example 7 A design method for cementitious materials used in hydraulic engineering to resist sulfate attack includes the following steps: Step 1: Determine the sulfate corrosion level, aggregate lithology risk, and erosion conditions in the construction environment based on the classification of working conditions; Step 1.1, Water quality testing: Determine the SO4 content in water samples from the construction environment. 2- Concentration, SO4 in water ≤ 400 2- <600 mg / L, classified as moderate sulfate attack; Step 1.2, aggregate lithological risks include the presence or absence of alkali-aggregate reaction and the presence or absence of TSA erosion; The presence or absence of alkali-aggregate reaction was determined using the mortar bar rapid method. Limestone aggregate was marked as having a risk of TSA erosion, while the rest were marked as not having a risk of TSA erosion. Step 1.3, Classification of erosion conditions: single sulfate erosion, freeze-thaw sulfate coupled erosion; After testing, the construction environment in this embodiment was a combination of freeze-thaw sulfate erosion and non-alkali aggregate reaction, with no risk of aggregate TSA erosion. Step 2: Based on the classification results, form a cementitious material system suitable for different working conditions; Because the construction environment in this embodiment is freeze-thaw sulfate coupled erosion + alkali-free aggregate reaction, the cementitious material system is P•MH42.5 cement + 20%~25% fly ash (that is, the weight percentage of fly ash in the cementitious material system is 20%~25%, and the rest is P•MH42.5 cement).

[0037] In this embodiment, the corrosion resistance coefficient K of the cementitious material system is ≥0.85, and the fly ash is Class F, Grade II fly ash.

[0038] Example 8 A design method for cementitious materials used in hydraulic engineering to resist sulfate attack includes the following steps: Step 1: Determine the sulfate corrosion level, aggregate lithology risk, and erosion conditions in the construction environment based on the classification of working conditions; Step 1.1, Water quality testing: Determine the SO4 content in water samples from the construction environment. 2- Concentration of SO4 in water 2- <400 mg / L, classified as weak sulfate corrosion; Step 1.2, aggregate lithological risks include the presence or absence of alkali-aggregate reaction and the presence or absence of TSA erosion; The presence or absence of alkali-aggregate reaction was determined using the mortar bar rapid method. Limestone aggregate was marked as having a risk of TSA erosion, while the rest were marked as not having a risk of TSA erosion. Step 1.3, Classification of erosion conditions: single sulfate erosion, freeze-thaw sulfate coupled erosion; After testing, the construction environment in this embodiment was a combination of freeze-thaw sulfate erosion and alkali-aggregate reaction, but there was no risk of aggregate TSA erosion. Step 2: Based on the classification results, form a cementitious material system suitable for different working conditions; Because the construction environment in this embodiment is freeze-thaw sulfate coupled erosion + alkali aggregate reaction, the cementitious material system is selected as P.MSR42.5 cement + 20%~25% fly ash (that is, the weight percentage of fly ash in the cementitious material system is 20%~25%, and the rest is P.MSR42.5 cement).

[0039] In this embodiment, the corrosion resistance coefficient K of the cementitious material system is ≥0.85, and the fly ash is Class F, Grade II fly ash.

[0040] Example 9 A design method for cementitious materials used in hydraulic engineering to resist sulfate attack includes the following steps: Step 1: Determine the sulfate corrosion level, aggregate lithology risk, and erosion conditions in the construction environment based on the classification of working conditions; Step 1.1, Water quality testing: Determine the SO4 content in water samples from the construction environment. 2- Concentration of SO4 in water 2- <400 mg / L, classified as weak sulfate corrosion; Step 1.2, aggregate lithological risks include the presence or absence of alkali-aggregate reaction and the presence or absence of TSA erosion; The presence or absence of alkali-aggregate reaction was determined using the mortar bar rapid method. Limestone aggregate was marked as having a risk of TSA erosion, while the rest were marked as not having a risk of TSA erosion. Step 1.3, Classification of erosion conditions: single sulfate erosion, freeze-thaw sulfate coupled erosion; After testing, the construction environment in this embodiment was TSA erosion of aggregates + alkali-free aggregate reaction; Step 2: Based on the classification results, form a cementitious material system suitable for different working conditions; Because the construction environment in this embodiment is aggregate TSA erosion + alkali-free aggregate reaction, the cementitious material system is P.MSR42.5 cement + 25%~35% fly ash (that is, the weight percentage of fly ash in the cementitious material system is 25%~35%, and the rest is P.MSR42.5 cement).

[0041] Example 10 A design method for cementitious materials used in hydraulic engineering to resist sulfate attack includes the following steps: Step 1: Determine the sulfate corrosion level, aggregate lithology risk, and erosion conditions in the construction environment based on the classification of working conditions; Step 1.1, Water quality testing, measuring SO4 in water samples from the construction environment. 2- Concentration of SO4 in water 2- The concentration was 825 mg / L, which was determined to be strong sulfate corrosion. Step 1.2, aggregate lithological risks include the presence or absence of alkali-aggregate reaction and the presence or absence of TSA erosion; The presence or absence of alkali-aggregate reaction was determined using the mortar bar rapid method. Limestone aggregate was marked as having a risk of TSA erosion, while the rest were marked as not having a risk of TSA erosion. Step 1.3, Classification of erosion conditions: single sulfate erosion, freeze-thaw sulfate coupled erosion; After testing, the construction environment in this embodiment was TSA erosion of aggregates + alkali-affected aggregate reaction; Step 2: Based on the classification results, form a cementitious material system suitable for different working conditions; Because the construction environment in this embodiment is TSA erosion of aggregates + alkali-aggregate reaction, the cementitious material system uses P.HSR42.5 cement + 25%~35% fly ash (that is, the weight percentage of fly ash in the cementitious material system is 25%~35%, and the rest is P.HSR42.5 cement). The fly ash in the cementitious material system is Class F Grade I fly ash, which meets the corresponding specification requirements of GB / T1596 or DL / T5055.

[0042] In extreme low-temperature (annual average temperature <5℃) limestone aggregate TSA erosion scenarios, 3%~5% silica fume can be added to the base of 25%~35% fly ash to further inhibit CSH gel decomposition and block the TSA erosion reaction pathway.

[0043] The design method of the cementitious material for sulfate-resistant concrete in hydraulic engineering of the present invention can replace part of the S75 and above grade slag powder on the basis of fly ash, forming a fly ash-slag double-blended composite cementitious system. The total proportion of admixtures remains unchanged within the specified range of fly ash in the cementitious material system of the present invention. It is suitable for hydraulic structures such as dams and gate chambers with large volume temperature control requirements.

Claims

1. A design method for cementitious materials in hydraulic engineering concrete resistant to sulfate attack, characterized in that, The classification process includes determining the level of sulfate corrosion in water, the lithological risk of aggregates, and the erosion conditions. The classification results include weak sulfate corrosion + non-alkali aggregate reaction, weak sulfate corrosion + alkali aggregate reaction, moderate sulfate corrosion, strong sulfate corrosion, freeze-thaw sulfate coupled corrosion, and aggregate TSA corrosion. Finally, based on the classification results, a cementitious material system adapted to different working conditions is formed.

2. The design method for cementitious materials of sulfate-resistant concrete in hydraulic engineering according to claim 1, characterized in that, Classification of the degree of sulfate corrosion in water, when SO4 2- <400 mg / L, weak sulfate corrosion is determined, when SO4 2- 400 < SO4 < 600 mg / L, medium sulfate corrosion is determined, when SO4 2- ≥ 600 mg / L, strong sulfate corrosion is determined.

3. The design method for cementitious materials of sulfate-resistant concrete in hydraulic engineering according to claim 2, characterized in that, The aggregate lithological risk includes whether there is alkali-aggregate reaction and whether there is TSA erosion. The presence of alkali-aggregate reaction is determined by the mortar bar rapid method, and limestone aggregate is marked as having TSA erosion risk.

4. The design method for cementitious materials of sulfate-resistant concrete in hydraulic engineering according to claim 3, characterized in that, The erosion conditions are divided into single sulfate erosion and freeze-thaw sulfate coupled erosion.

5. The design method for cementitious materials of sulfate-resistant concrete in hydraulic engineering according to claim 4, characterized in that, When the grading result is weak sulfate attack + alkali-free aggregate reaction, the corresponding cementitious material system is P•O42.5 cement + 15%~20% fly ash; when the grading result is weak sulfate attack + alkali-containing aggregate reaction, the corresponding cementitious material system is P•O42.5 cement + 20%~25% fly ash.

6. The design method for cementitious materials of sulfate-resistant concrete in hydraulic engineering according to claim 5, characterized in that, When the grading result is moderate sulfate attack + with / without alkali aggregate reaction, the corresponding cementitious material system is P•O42.5 / P.MSR42.5 cement + 20%~25% fly ash. When the grading result is strong sulfate attack + with / without alkali aggregate reaction, the corresponding cementitious material system is P•O42.5 cement + 20%~25% fly ash + 3%~12% sulfate-resistant corrosion inhibitor, or P•MH42.5 / P.MSR42.5 / P.HSR42.5 cement + 20~25% fly ash.

7. The design method for cementitious materials of sulfate-resistant concrete in hydraulic engineering according to claim 6, characterized in that, When the grading result is freeze-thaw sulfate coupled erosion + alkali-aggregate reaction (with or without alkali), the corresponding cementitious material system is P•MH42.5 / P.MSR42.5 / P.HSR42.5 cement + 20%~25% fly ash. When the grading result is aggregate TSA erosion + alkali-aggregate reaction (with or without alkali), the corresponding cementitious material system is P•MH42.5 / P.MSR42.5 / P.HSR42.5 cement + 25%~35% fly ash.

8. The design method for cementitious materials of sulfate-resistant concrete in hydraulic engineering according to claim 7, characterized in that, The classification determines the degree of sulfate corrosion in water. When SO4 in the water... 2- When the concentration is ≥2000mg / L, the corresponding cementitious material system is P•MH42.5 / P.MSR42.5 / P.HSR42.5 cement + 30~35% fly ash.

9. The design method for cementitious materials of sulfate-resistant concrete in hydraulic engineering according to claim 8, characterized in that, The fly ash in the cementitious material system is either Class II or Class I F fly ash, and the C3A content in the P•O42.5 cement clinker is 5%~8%.

10. The design method for cementitious materials of sulfate-resistant concrete in hydraulic engineering according to claim 7, characterized in that, When the classification result is weak sulfate attack, the corrosion resistance coefficient K of the cementitious material system is ≥0.8; when the classification result is moderate sulfate attack, strong sulfate attack, or freeze-thaw sulfate coupled attack, the corrosion resistance coefficient K of the cementitious material system is ≥0.85.