A cold-resistant cable and its preparation method

By using compounded cold-resistant plasticizers and modified basalt fibers, the flexibility and mechanical strength of cold-resistant cables are improved, solving the problems of migration and precipitation of cable sheath materials and weak interfacial bonding in low-temperature environments, thus achieving stable operation of cables in extremely cold environments.

CN123120412APending Publication Date: 2026-11-17FOSHAN HONGTUBAO CABLE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611491625.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-23
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing cold-resistant cables suffer from problems such as plasticizer migration and precipitation in the sheath material, weak interfacial bonding, and insufficient mechanical strength in low-temperature environments, which affect the cable's flexibility and service life.

Method used

By using a compound cold-resistant plasticizer, modified basalt fiber and active nano calcium carbonate, and by modifying the fiber-rubber interface with polydopamine and silane coupling agent, the cable's structural stability and mechanical strength are ensured in low-temperature environments.

Benefits of technology

It significantly improves the flexibility and mechanical strength of cables in low-temperature environments, prevents embrittlement and cracking, extends service life, and reduces the risk of plasticizer migration and precipitation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120412A_ABST
    Figure CN123120412A_ABST
Patent Text Reader

Abstract

This invention discloses a cold-resistant cable and its preparation method, relating to the field of power cables. A cold-resistant cable includes a core unit, a filling layer wrapped around the core unit, a polyethylene insulating sleeve, a steel tape layer, and an outer sheath. The outer sheath comprises the following raw materials in parts by weight: 100 parts EPDM rubber; 14-18 parts cold-resistant plasticizer; 6-11 parts modified basalt fiber; 24-30 parts active nano-calcium carbonate; 2-3 parts vulcanizing agent; 1-2 parts crosslinking agent; 2-4 parts lubricant; and 1-3 parts antioxidant. The cold-resistant plasticizer is a mixture of di(2-propylheptyl) adipate and triethylene glycol diisooctanoate. The modified basalt fiber is modified with polydopamine and a silane coupling agent. The active nano-calcium carbonate is modified with stearic acid or methacrylic acid. The cable of this application maintains good flexibility and mechanical strength in extremely cold environments, meeting the long-term stable operation requirements of cables in low-temperature regions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of power cables, and in particular to a cold-resistant cable and its preparation method. Background Technology

[0002] Cables are made of several or groups of conductors (at least two conductors per group) twisted together, covered with a highly insulating outer layer. Each group of conductors is insulated from each other and is often twisted around a central conductor. As an important component of modern power and communication systems, cables are widely used in industry, construction, transportation, and other fields.

[0003] With the development of technology, the demand for cables in low-temperature environments is constantly increasing. Therefore, cold-resistant cables that can operate stably in low-temperature environments have been specially designed. They can maintain good electrical performance, mechanical performance and structural stability at low temperatures, avoid insulation or sheath cracking and embrittlement caused by low temperatures, and ensure reliable transmission of power and signals.

[0004] Existing cold-resistant cables primarily improve low-temperature resistance by modifying the materials of the sheath layer. The sheath matrix material can be elastomers, rubber, etc. One modification method is to significantly increase cold-resistant plasticizers to enhance cold resistance. However, the addition of plasticizers can lead to migration and precipitation problems, affecting the mechanical strength and long-term lifespan of the sheath. Furthermore, to improve the mechanical strength of the sheath, fibers and inorganic fillers are often added. However, the interfacial bonding between the filler and the matrix material is weak, leading to stress concentration at low temperatures, which can become the starting point for crack propagation and adversely affect the low-temperature impact resistance of the sheath.

[0005] Therefore, there is an urgent need to develop a cold-resistant cable that can maintain good flexibility and mechanical strength in extremely cold environments to meet the long-term stable operation requirements of cables in low-temperature regions. Summary of the Invention

[0006] To address the aforementioned problems, this application provides a cold-resistant cable and a method for its preparation.

[0007] This application provides a cold-resistant cable and its manufacturing method, which adopts the following technical solution: In a first aspect, a cold-resistant cable includes a core unit, a filling layer sequentially wrapped around the outside of the core unit, a polyethylene insulating sleeve, a steel tape layer, and an outer sheath. The core unit includes a conductor, an insulation layer, and a shielding layer. The outer sheath comprises the following raw materials in parts by weight: 100 parts of EPDM rubber; 14-18 parts of cold-resistant plasticizer; 6-11 parts of modified basalt fiber; 24-30 parts of active nano-calcium carbonate; 2-3 parts of vulcanizing agent; 1-2 parts of crosslinking agent; 2-4 parts lubricant; Anti-aging agent 1-3 parts; The cold-resistant plasticizer is a mixture of di(2-propylheptyl) adipate and triethylene glycol diisooctanoate in a weight ratio of (2-3):1; The modified basalt fiber is modified by synergistic modification with polydopamine and silane coupling agent; The active nano-calcium carbonate is modified with stearic acid or methacrylic acid.

[0008] By adopting the above technical solutions and through the overall cable structure design, the structural stability and electromagnetic interference resistance of the cable are guaranteed. Through the specific outer sheath formula, the cable has excellent cold resistance in low-temperature environments, can maintain flexibility, and avoid embrittlement and cracking. At the same time, through the reinforcing effect of modified fibers and fillers, the mechanical strength and service life of the cable are guaranteed.

[0009] In the outer sheath, a compound cold-resistant plasticizer was selected, which significantly lowers the glass transition temperature compared to a single plasticizer, while reducing the risk of plasticizer migration and precipitation. Basalt fibers were modified using polydopamine and silane coupling agents. The adhesive effect of polydopamine improves the physical wetting of the fiber and rubber, while the chemical bridging effect of the silane coupling agent achieves chemical bonding, significantly improving interfacial bonding strength and thus enhancing the mechanical properties of the sheath. Stearic acid / methacrylic acid modification improves the dispersibility of nano-calcium carbonate in the rubber, facilitating its reinforcing effect and improving the sheath's abrasion resistance.

[0010] Optionally, the EPDM rubber is a mixture of EPDM rubber and modified EPDM rubber in a weight ratio of (3.5-4):1, wherein the modified EPDM rubber comprises the following parts by weight of raw materials: 100 parts of EPDM rubber; 6-12 parts of epoxidized soybean oil; 0.3-0.8 parts of dicumyl peroxide; 1-3 parts styrene.

[0011] By adopting the above technical solution, polar epoxy groups are introduced into the molecular chain of EPDM rubber, which improves the polarity of the rubber matrix and makes it more compatible with fillers and plasticizers. At the same time, the long-chain alkyl groups play an internal plasticizing role, further reducing the glass transition temperature of the matrix and making it more resistant to low temperatures.

[0012] Optionally, the modified EPDM rubber is prepared by the following steps: Ethylene propylene diene monomer (EPDM) rubber is dried at 60-80℃ for 2-4 hours in advance, epoxidized soybean oil is dried for 24 hours, and dicumyl peroxide is dissolved in 3-4 times its volume of acetone to obtain a mixture. Ethylene propylene diene monomer (EPDM) rubber is put into a high-speed mixer, the mixture is sprayed and epoxidized soybean oil and styrene are added, and the mixture is mixed for 15-20 minutes and left to stand for 15 minutes to obtain a premix. The premixed material is added to a twin-screw extruder and extruded. The temperature is set as follows: feeding section 130-150℃, reaction section 170-180℃, venting section 160-170℃, and die head 150-160℃. The extrudate is cooled with water and then pelletized. It is then dried at 60-70℃ for 4-6 hours to obtain modified EPDM rubber.

[0013] By adopting the above technical solution, epoxidized soybean oil and styrene are ensured to achieve uniform dispersion and effective grafting reaction in the EPDM rubber matrix, thus obtaining modified EPDM rubber.

[0014] Optionally, the modified basalt fiber is prepared by the following method: Basalt fibers were placed in acetone solution and ultrasonically treated for 1-1.5 hours. They were then removed, washed, calcined at 550-570℃ for 1.5-2 hours, washed again, and dried at 60-63℃ for 8 hours to obtain pretreated basalt fibers. Dopamine hydrochloride was dissolved in deionized water to prepare a solution with a concentration of 2-2.5 g / L. Tris(hydroxymethyl)aminomethane hydrochloride was dissolved in deionized water to prepare a buffer solution of 1 mol / L. The pretreated basalt fiber was added to the dopamine solution, and then the buffer solution was added to adjust the pH of the solution to 8-8.5. After soaking for 8-12 hours, the fiber was taken out and washed with deionized water. It was then dried at 60-63℃ for 2-3 hours to obtain PDA-basalt fiber. Take 3%-5% of the weight of A-172 coupling agent of basalt fiber, dissolve it in ethanol aqueous solution, add acetic acid to adjust the pH to 4.5-5 to obtain solvent, soak PDA-basalt fiber in solvent for 30-45 min, take it out and place it at 115-120℃ for condensation for 2-2.5 h to obtain modified basalt fiber.

[0015] By adopting the above technical solutions, the pretreatment can remove impurities from the surface of basalt fibers, etch the fiber surface to increase roughness, and introduce a large number of phenolic hydroxyl and amino active sites through polydopamine coating, providing a platform for the grafting of A-172 coupling agent, while improving the physical compatibility between fibers and rubber; the ethylene end of A-152 coupling agent will participate in the subsequent vulcanization reaction, and facilitate stress transfer by forming covalent bridges, thereby improving mechanical strength.

[0016] Optionally, the epoxy value of the epoxidized soybean oil is 6.0%-6.5%, and the EPDM rubber is selected from ENB type EPDM with an ENB content of 4%-5% and an ethylene content of 50%-55%.

[0017] Optionally, the vulcanizing agent is dicumyl peroxide, and the co-crosslinking agent is triallyl isocyanurate.

[0018] Optionally, the lubricant is selected from one or more of polyethylene wax, zinc stearate, and microcrystalline wax, and the antioxidant is selected from two or more of antioxidants RD, MB, and 4010NA.

[0019] Optionally, the conductor is formed by stranding several insulated copper cores, and the shielding layer includes an inner semiconducting shielding layer, an outer semiconducting shielding layer, and a copper strip shielding layer from the inside out, with the insulating layer disposed between the inner semiconducting shielding layer and the outer semiconducting shielding layer.

[0020] By adopting the above technical solutions, the three-layer shielding structure effectively homogenizes the electric field and avoids partial discharge. The copper tape shielding can also serve as electromagnetic shielding and a fault current path, significantly improving the electrical safety and anti-interference capability of the cable.

[0021] Secondly, a method for preparing a cold-resistant cable includes the following steps: After drawing copper core wire, heat treatment and tin plating are performed. After annealing, the wire is stranded to obtain a conductor. An insulation layer and a shielding layer are extruded on the outer layer of the conductor to obtain a cable core unit. Rubber strips are filled on the outside of the cable core unit and non-woven fabric tape is wrapped to form a filling layer. Polyethylene material is extruded on the outside of the filling layer and cooled to form a polyethylene isolation sleeve. A galvanized steel strip is then wrapped around the gaps to form an outer sheath layer.

[0022] Optionally, the outer sheath material is prepared by the following steps: EPDM rubber is pre-plasticized by thin-passing, with the roller temperature controlled at 40-50℃, and thin-passed 5-6 times. Nano-calcium carbonate and modified basalt fiber are dried at 75-80℃ for 3-4 hours. Antioxidant and lubricant are mixed evenly to obtain the additives. Take out 20-25 parts of EPDM rubber and put it into the open mill. Control the roller temperature at 50-60℃. Add modified basalt fiber multiple times until the fiber is completely wrapped by the rubber compound. Adjust the roller gap and pass through the mill 3 times. Make triangular wraps twice. After sheeting, cut it into 3-5mm rubber granules to obtain fiber reinforced masterbatch. Add the remaining EPDM rubber and fiber-reinforced masterbatch to the internal mixer, and mix under pressure for 2-3 minutes until the rubber compound is completely melted and plasticized. Then add 70%-75% of the total weight of cold-resistant plasticizer, and continue mixing for 2-2.5 minutes. Add active nano calcium carbonate and additives, and mix for 1-2 minutes. Add the remaining cold-resistant plasticizer, and continue mixing for 2-3 minutes. When the rubber compound temperature reaches 125-130℃, discharge the rubber and transfer it to an open mill for thin passing 2-3 times. Air cool to room temperature to obtain the initial rubber compound. Put the primary rubber into an internal mixer and plasticize for 1-1.5 minutes. Add vulcanizing agent and crosslinking agent and mix for 3-4 minutes. During this period, the rubber temperature should not exceed 120℃. After mixing evenly, discharge the rubber and pass it through a two-roll mill 3 times and make triangular wraps 2 times. After sheeting and cooling to room temperature, the outer sheath material is obtained.

[0023] The above technical solution involves first premixing basalt fiber with a portion of EPDM rubber to form a masterbatch, ensuring uniform fiber dispersion; then adding plasticizer in two stages to avoid excessive addition at one time, which could cause the rubber compound to slip and have difficulty absorbing powder. The preparation process ensures the processing safety of the rubber compound and ensures that all components are mixed evenly to obtain the outer sheath material.

[0024] In summary, this application has at least one of the following beneficial effects: 1. The overall cable structure design ensures the cable's structural stability and electromagnetic interference resistance. The specific outer sheath formula enables the cable to have excellent cold resistance in low-temperature environments, maintain flexibility, and avoid embrittlement and cracking. At the same time, the reinforcement effect of modified fibers and fillers ensures the cable's mechanical strength and service life.

[0025] In the outer sheath, a compound cold-resistant plasticizer was selected, which significantly lowers the glass transition temperature compared to a single plasticizer, while reducing the risk of plasticizer migration and precipitation. Basalt fibers were modified using polydopamine and silane coupling agents. The adhesive effect of polydopamine improves the physical wetting of the fiber and rubber, while the chemical bridging effect of the silane coupling agent achieves chemical bonding, significantly improving interfacial bonding strength and thus enhancing the mechanical properties of the sheath. Stearic acid / methacrylic acid modification improves the dispersibility of nano-calcium carbonate in the rubber, facilitating its reinforcing effect and improving the sheath's abrasion resistance.

[0026] 2. Introducing polar epoxy groups into the molecular chain of EPDM rubber increases the polarity of the rubber matrix, making it more compatible with fillers and plasticizers. At the same time, the long-chain alkyl groups act as internal plasticizers, further reducing the glass transition temperature of the matrix and making it more resistant to low temperatures. Attached Figure Description

[0027] Figure 1 This is a schematic diagram of the structure of the cold-resistant cable in Embodiment 1 of this application.

[0028] Explanation of reference numerals in the attached figures: 1. Conductor; 2. Inner semiconductive shielding layer; 3. Insulating layer; 4. Outer semiconductive shielding layer; 5. Copper strip shielding layer; 6. Rubber strip; 7. Non-woven fabric wrapping tape; 8. Polyethylene isolation sleeve; 9. Steel strip layer; 10. Outer sheath layer. Detailed Implementation

[0029] The present application will be further described in detail below with reference to Examples 1-4 and Comparative Examples 1-2.

[0030] Raw material source: The ethylene propylene diene monomer (EPDM) rubber used is ENB type EPDM rubber with an ENB content of 4%-5% and an ethylene content of 50%-55%, and the model is Dow 4770R. The epoxy value of epoxidized soybean oil is 6.0%-6.5%, and the acid value is ≤0.5mg KOH / g; Basalt fiber, using short-cut basalt fiber with a length of 3-6mm. Preparation Example

[0031] Preparation Example 1-1 A modified EPDM rubber comprises the following raw materials: 100 kg of EPDM rubber, 6 kg of epoxidized soybean oil 0.3 kg of dicumyl peroxide and 1 kg of styrene.

[0032] Modified EPDM rubber is prepared through the following steps: Ethylene propylene diene monomer (EPDM) rubber was dried at 60°C for 4 hours in advance, epoxidized soybean oil was dried with molecular sieves for 24 hours, and dicumyl peroxide was dissolved in 3 times its volume of acetone to obtain a mixture. Ethylene propylene diene monomer (EPDM) rubber was put into a high-speed mixer, the mixture was sprayed and epoxidized soybean oil and styrene were added, and the mixture was mixed for 15 minutes and then left to stand for 15 minutes to obtain a premix. The premixed material was added to a twin-screw extruder and extruded. The temperatures were set as follows: feeding section 130℃, reaction section 170℃, venting section 160℃, die 150℃, length-to-diameter ratio L / D 40, screw speed 60 rpm, residence time 5 min. The extrudate was water-cooled, pelletized, and dried at 60℃ for 4 h to obtain modified EPDM rubber.

[0033] Preparation Examples 1-2 A modified EPDM rubber comprises the following raw materials: 100 kg of EPDM rubber, 12 kg of epoxidized soybean oil 0.8 kg of dicumyl peroxide and 3 kg of styrene.

[0034] Modified EPDM rubber is prepared through the following steps: Ethylene propylene diene monomer (EPDM) rubber was dried at 80°C for 2 hours in advance, epoxidized soybean oil was dried with molecular sieves for 24 hours, and dicumyl peroxide was dissolved in 4 times its volume of acetone to obtain a mixture. Ethylene propylene diene monomer (EPDM) rubber was put into a high-speed mixer, the mixture was sprayed and epoxidized soybean oil and styrene were added, and the mixture was mixed for 15 minutes and then left to stand for 15 minutes to obtain a premix. The premixed material was added to a twin-screw extruder and extruded. The temperatures were set as follows: feeding section 150℃, reaction section 180℃, venting section 170℃, and die 160℃. The length-to-diameter ratio (L / D) was 38, the screw speed was 80 rpm, and the residence time was 4 min. The extrudate was water-cooled, pelletized, and dried at 70℃ for 6 h to obtain modified EPDM rubber.

[0035] Preparation Example 2-1 A modified basalt fiber, synergistically modified with polydopamine and a silane coupling agent, is prepared through the following steps: Basalt fibers were placed in acetone solution and ultrasonically treated for 1 hour. They were then removed, washed, calcined at 550°C for 2 hours, washed again, and dried at 60°C for 8 hours to obtain pretreated basalt fibers. Dopamine hydrochloride was dissolved in deionized water to prepare a 2 g / L solution. Tris(hydroxymethyl)aminomethane hydrochloride was dissolved in deionized water to prepare a 1 mol / L buffer solution. The pretreated basalt fibers were added to the dopamine solution, and then the buffer solution was added to adjust the pH of the solution to 8.5. After soaking for 8 hours, the fibers were removed and repeatedly washed with deionized water until the filtrate was colorless. The fibers were then dried at 60°C for 2 hours to obtain PDA-basalt fibers, wherein the weight of the polydopamine coating was 1% of the basalt fibers. Take 3% of the weight of A-172 coupling agent of basalt fiber, dissolve it in an ethanol aqueous solution with a volume ratio of 9:1, add acetic acid to adjust the pH to 4.5 to obtain a solvent, and the weight of A-172 coupling agent accounts for 1% of the weight of the solvent. Soak PDA-basalt fiber in the solvent for 30 min, take it out and place it at 115℃ for polycondensation and curing for 2 h to obtain modified basalt fiber.

[0036] Preparation Example 2-2 A modified basalt fiber, synergistically modified with polydopamine and a silane coupling agent, is prepared through the following steps: Basalt fibers were placed in acetone solution and ultrasonically treated for 1.5 hours. They were then removed, washed, calcined at 570°C for 1.5 hours, washed again, and dried at 63°C for 8 hours to obtain pretreated basalt fibers. Dopamine hydrochloride was dissolved in deionized water to prepare a 2.5 g / L solution. Tris(hydroxymethyl)aminomethane hydrochloride was dissolved in deionized water to prepare a 1 mol / L buffer solution. The pretreated basalt fibers were added to the dopamine solution, and then the buffer solution was added to adjust the pH of the solution to 8. After soaking for 12 h, the fibers were removed and repeatedly washed with deionized water until the filtrate was colorless. The fibers were dried at 63 °C for 3 h to obtain PDA-basalt fibers, wherein the weight of the polydopamine coating was 2% of the basalt fibers. Take 5% of the weight of A-172 coupling agent of basalt fiber, dissolve it in an ethanol aqueous solution with a volume ratio of 9:1, add acetic acid to adjust the pH to 4.5 to obtain a solvent, and the weight of A-172 coupling agent accounts for 1.5% of the weight of the solvent. Soak PDA-basalt fiber in the solvent for 45 min, take it out and place it at 120℃ for polycondensation and curing for 2.5 h to obtain modified basalt fiber. Example

[0037] Example 1 This embodiment discloses a cold-resistant cable, comprising a core unit, a filling layer sequentially wrapped around the outside of the core unit, a polyethylene insulating sleeve, a steel tape layer, and an outer sheath. The core unit includes a conductor, an insulation layer, and a shielding layer. The conductor is composed of several insulated copper cores twisted together. The shielding layer includes an inner semi-conductive shielding layer, an outer semi-conductive shielding layer, and a copper tape shielding layer. The insulation layer is located between the inner and outer semi-conductive shielding layers. From the inside out, the core unit consists of a conductor, an inner semi-conductive shielding layer, an insulation layer, an outer semi-conductive shielding layer, and a copper tape shielding layer. The filling layer includes rubber strips and non-woven fabric wrapping tape, and the steel tape layer is made of galvanized steel tape.

[0038] The outer sheath comprises the following parts by weight of raw materials: 100 kg of EPDM rubber was prepared by mixing ordinary EPDM rubber and modified EPDM rubber in a weight ratio of 3.5:1. The modified EPDM rubber was obtained from Preparation Example 1-1. 14 kg of cold-resistant plasticizer is a mixture of di(2-propylheptyl) adipate and triethylene glycol diisooctanoate in a weight ratio of 2:1. 6 kg of modified basalt fiber, sourced from Preparation Example 2-1; 24 kg of active nano-calcium carbonate was prepared by modifying the nano-calcium carbonate with stearic acid. 2 kg of vulcanizing agent, using dicumyl peroxide; 1 kg of crosslinking agent, selected from triallyl isocyanurate; 2 kg of lubricant, consisting of 1 kg of polyethylene wax and 1 kg of zinc stearate; 1 kg of antioxidant is used, with 0.5 kg of antioxidant MB and 0.5 kg of antioxidant RD selected.

[0039] The method for preparing cold-resistant cables includes the following steps: After drawing copper core wire, heat treatment and tin plating are performed. After annealing, the wire is stranded to obtain a conductor. An insulation layer and a shielding layer are extruded on the outer layer of the conductor to obtain a cable core unit. Rubber strips are filled on the outside of the cable core unit and non-woven fabric tape is wrapped to form a filling layer. Polyethylene material is extruded on the outside of the filling layer and cooled to form a polyethylene isolation sleeve. A galvanized steel strip is then wrapped around the gaps to form an outer sheath layer.

[0040] The outer sheath material is prepared through the following steps: EPDM rubber was pre-plasticized by thin-pass molding, with the roller temperature controlled at 40℃ and thin-passed 5 times. Nano-calcium carbonate and modified basalt fiber were dried at 75℃ for 4 hours. Antioxidant and lubricant were mixed evenly to obtain the additives. Take out 20kg of EPDM rubber and put it into the open mill. The roller temperature is controlled at 50℃. Add modified basalt fiber multiple times until the fiber is completely wrapped by the rubber compound. Adjust the roller gap and pass through the mill 3 times. Make triangular wraps twice. After sheeting, cut it into 3-5mm rubber granules to obtain fiber reinforced masterbatch. Add the remaining EPDM rubber and fiber-reinforced masterbatch to the internal mixer, and mix under pressure for 2 minutes until the rubber compound is completely melted and plasticized. Then add 70% of the total weight of cold-resistant plasticizer, continue mixing for 2 minutes, add active nano calcium carbonate and additives, mix for 1 minute, add the remaining cold-resistant plasticizer, and continue mixing for 2 minutes. When the temperature of the rubber compound reaches 125-130℃, discharge the rubber, transfer it to an open mill for two thin passes, and air cool it to room temperature to obtain the initial rubber compound. Put the primary rubber into an internal mixer and plasticize for 1 minute. Add vulcanizing agent and crosslinking agent and mix for 3 minutes. During this period, the rubber temperature should not exceed 120℃. After mixing evenly, discharge the rubber and pass it through a two-roll mill 3 times and make triangular wraps 2 times. After sheeting and cooling to room temperature, the outer sheath material is obtained.

[0041] Example 2 This embodiment discloses a cold-resistant cable, which differs from Embodiment 1 in that the raw materials and preparation methods of the outer sheath are different.

[0042] In this embodiment, the outer sheath comprises the following parts by weight of raw materials: 100 kg of EPDM rubber was prepared by mixing ordinary EPDM rubber and modified EPDM rubber in a weight ratio of 4:1. The modified EPDM rubber was obtained from Preparation Examples 1-2. 18 kg of cold-resistant plasticizer is a mixture of di(2-propylheptyl) adipate and triethylene glycol diisooctanoate in a weight ratio of 2:1. 11 kg of modified basalt fiber, sourced from Preparation Example 2-2; 30 kg of active nano-calcium carbonate was prepared by modifying the nano-calcium carbonate with methacrylic acid. 3 kg of vulcanizing agent, using dicumyl peroxide; 2 kg of crosslinking agent, selected from triallyl isocyanurate; 4 kg of lubricant, consisting of 2 kg of microcrystalline wax and 2 kg of zinc stearate; 3 kg of antioxidants were used, with 2 kg of antioxidant 4010NA and 1 kg of antioxidant RD selected.

[0043] The outer sheath material is prepared through the following steps: EPDM rubber is pre-processed through thin-pass plasticizing, with the roller temperature controlled at 50℃ and thin-passed 6 times. Nano-calcium carbonate and modified basalt fiber are dried at 80℃ for 3 hours. Antioxidant and lubricant are mixed evenly to obtain the additives. Take out 25kg of EPDM rubber and put it into the open mill. The roller temperature is controlled at 60℃. Add modified basalt fiber multiple times until the fiber is completely wrapped by the rubber compound. Adjust the roller gap and pass through the mill 3 times. Make triangular wraps twice. After sheeting, cut it into 3-5mm rubber granules to obtain fiber reinforced masterbatch. Add the remaining EPDM rubber and fiber-reinforced masterbatch to the internal mixer, and mix under pressure for 3 minutes until the rubber compound is completely melted and plasticized. Then add 75% of the total weight of cold-resistant plasticizer and continue mixing for 2.5 minutes. Add active nano calcium carbonate and additives and mix for 2 minutes. Add the remaining cold-resistant plasticizer and continue mixing for 3 minutes. When the rubber compound temperature reaches 125-130℃, discharge the rubber and transfer it to an open mill for three thin passes. Air cool to room temperature to obtain the initial rubber compound. Put the primary rubber into an internal mixer and plasticize for 1.5 minutes. Add vulcanizing agent and crosslinking agent and mix for 4 minutes. During this period, the rubber temperature should not exceed 120°C. After mixing evenly, discharge the rubber and pass it through a two-roll mill 3 times and make triangular wraps 2 times. After sheeting and cooling to room temperature, the outer sheath material is obtained.

[0044] Example 3 The difference between this embodiment and Embodiment 1 is that the raw materials of the outer sheath are different.

[0045] In this embodiment, the outer sheath comprises the following parts by weight of raw materials: 100 kg of EPDM rubber was prepared by mixing ordinary EPDM rubber and modified EPDM rubber in a weight ratio of 3.5:1. The modified EPDM rubber was obtained from Preparation Example 1-1. 16 kg of cold-resistant plasticizer is a mixture of di(2-propylheptyl) adipate and triethylene glycol diisooctanoate in a weight ratio of 3:1. 9 kg of modified basalt fiber, sourced from Preparation Example 2-1; 26 kg of active nano-calcium carbonate was prepared by modifying the nano-calcium carbonate with methacrylic acid. 2.5 kg of vulcanizing agent, using dicumyl peroxide; 1.5 kg of crosslinking agent, selected from triallyl isocyanurate; 2 kg of lubricant, consisting of 1.5 kg of microcrystalline wax and 0.5 kg of zinc stearate; 2 kg of antioxidants were used, with 1 kg of antioxidant 4010NA and 1 kg of antioxidant MB selected.

[0046] Example 4 The difference between this embodiment and Embodiment 1 is that the raw materials of the outer sheath are different.

[0047] In this embodiment, all the EPDM rubber in the outer sheath material is ordinary EPDM rubber, that is, the weight of modified EPDM rubber is 0.

[0048] Comparative Example Comparative Example 1 The difference between this comparative example and Example 1 is that the raw materials of the outer sheath are different.

[0049] In this comparative example, an equal amount of unmodified basalt fiber was used instead of modified basalt fiber in the raw materials of the outer sheath.

[0050] Comparative Example 2 The difference between this comparative example and Example 1 is that the raw materials of the outer sheath are different.

[0051] In this comparative example, the cold-resistant plasticizer used in the outer sheath was all di(2-propylheptyl) adipate, i.e., 14 kg of di(2-propylheptyl) adipate and 0 kg of triethylene glycol diisooctanoate.

[0052] The following performance tests were conducted on the outer sheath materials and cold-resistant cables prepared from the above Examples 1-4 and Comparative Examples 1-2, and the test results were recorded.

[0053] Low-temperature elongation at break of the outer sheath: The reference standard is GB / T 1040.3-2006, and the temperature is -50℃; Tear resistance of the outer sheath layer: Refer to standard GB / T 1040.3-2006; Low-temperature embrittlement test: In accordance with GB / T 5470-2008 standard, 15 sheath material samples were prepared. After being kept at a test temperature of -50℃ for 5 minutes, the samples were subjected to impact testing using a low-temperature brittle impact testing machine. The number of fractured samples was recorded and counted. The impact head speed was set to 2.0 m / s.

[0054] Sample Low temperature elongation at break / % Tear resistance / MPa Low temperature embrittlement number of broken samples / pieces Example 1 370 45 0 Example 2 370 43 0 Example 3 380 46 0 Example 4 290 37 5 Comparative Example 1 310 34 6 Comparative Example 2 330 39 3

[0055] As shown in the table above, the cold-resistant cable of this application improves the interfacial bonding force and mechanical strength of the sheath material and reduces the glass transition temperature by using a specific outer sheath formulation and combining specific cold-resistant plasticizers, modified basalt fibers and modified EPDM rubber.

[0056] This specific embodiment is merely an explanation of this application and is not intended to limit it. After reading this specification, those skilled in the art can make modifications to this specific embodiment without contributing any inventive step, but such modifications are protected by patent law as long as they fall within the scope of the claims of this application.

Claims

1. A cold-resistant cable, characterized in that: The cable core unit comprises a core unit, a filling layer sequentially wrapped around the core unit, a polyethylene insulating sleeve, a steel tape layer, and an outer sheath. The core unit includes a conductor, an insulation layer, and a shielding layer. The outer sheath comprises the following raw materials in parts by weight: 100 parts of EPDM rubber; 14-18 parts of cold-resistant plasticizer; 6-11 parts of modified basalt fiber; 24-30 parts of active nano-calcium carbonate; 2-3 parts of vulcanizing agent; 1-2 parts of crosslinking agent; 2-4 parts lubricant; Anti-aging agent 1-3 parts; The cold-resistant plasticizer is a mixture of di(2-propylheptyl) adipate and triethylene glycol diisooctanoate in a weight ratio of (2-3):1; The modified basalt fiber is modified by synergistic modification with polydopamine and silane coupling agent; The active nano-calcium carbonate is modified with stearic acid or methacrylic acid.

2. The cold-resistant cable according to claim 1, characterized in that: The EPDM rubber is selected from a mixture of EPDM rubber and modified EPDM rubber in a weight ratio of (3.5-4):

1. The modified EPDM rubber comprises the following raw materials in parts by weight: 100 parts of EPDM rubber; 6-12 parts of epoxidized soybean oil; 0.3-0.8 parts of dicumyl peroxide; 1-3 parts styrene.

3. The cold-resistant cable according to claim 1, characterized in that, The modified EPDM rubber is prepared through the following steps: Ethylene propylene diene monomer (EPDM) rubber is dried at 60-80℃ for 2-4 hours in advance, epoxidized soybean oil is dried for 24 hours, and dicumyl peroxide is dissolved in 3-4 times its volume of acetone to obtain a mixture. Ethylene propylene diene monomer (EPDM) rubber is put into a high-speed mixer, the mixture is sprayed and epoxidized soybean oil and styrene are added, and the mixture is mixed for 15-20 minutes and left to stand for 15 minutes to obtain a premix. The premixed material is added to a twin-screw extruder and extruded. The temperature is set as follows: feeding section 130-150℃, reaction section 170-180℃, venting section 160-170℃, and die head 150-160℃. The extrudate is cooled with water and then pelletized. It is then dried at 60-70℃ for 4-6 hours to obtain modified EPDM rubber.

4. The cold-resistant cable according to claim 1, characterized in that: The modified basalt fiber is prepared by the following method: Basalt fibers were placed in acetone solution and ultrasonically treated for 1-1.5 hours. They were then removed, washed, calcined at 550-570℃ for 1.5-2 hours, washed again, and dried at 60-63℃ for 8 hours to obtain pretreated basalt fibers. Dopamine hydrochloride was dissolved in deionized water to prepare a solution with a concentration of 2-2.5 g / L. Tris(hydroxymethyl)aminomethane hydrochloride was dissolved in deionized water to prepare a buffer solution of 1 mol / L. The pretreated basalt fiber was added to the dopamine solution, and then the buffer solution was added to adjust the pH of the solution to 8-8.

5. After soaking for 8-12 hours, the fiber was taken out and washed with deionized water. It was then dried at 60-63℃ for 2-3 hours to obtain PDA-basalt fiber. Take 3%-5% of the weight of basalt fiber of A-172 coupling agent, dissolve it in ethanol aqueous solution, add acetic acid to adjust the pH to 4.5-5 to obtain solvent, immerse PDA-basalt fiber in solvent for 30-45 min, take it out and place it at 115-120℃ for condensation for 2-2.5 h to obtain modified basalt fiber.

5. A cold-resistant cable according to claim 2, characterized in that: The epoxy value of the epoxidized soybean oil is 6.0%-6.5%, and the EPDM rubber is ENB type EPDM with an ENB content of 4%-5% and an ethylene content of 50%-55%.

6. The cold-resistant cable according to claim 1, characterized in that: The vulcanizing agent is dicumyl peroxide, and the crosslinking agent is triallyl isocyanurate.

7. A cold-resistant cable according to claim 1, characterized in that: The lubricant is selected from one or more of polyethylene wax, zinc stearate, and microcrystalline wax, and the antioxidant is selected from two or more of antioxidants RD, MB, and 4010NA.

8. A cold-resistant cable according to claim 1, characterized in that: The conductor is made of several insulated copper cores twisted together. The shielding layer includes an inner semiconducting shielding layer, an outer semiconducting shielding layer and a copper strip shielding layer from the inside out. The insulating layer is disposed between the inner semiconducting shielding layer and the outer semiconducting shielding layer.

9. A method for preparing a cold-resistant cable according to any one of claims 1-8, characterized in that, Includes the following steps: After drawing copper core wire, heat treatment and tin plating are performed. After annealing, the wire is stranded to obtain a conductor. An insulation layer and a shielding layer are extruded on the outer layer of the conductor to obtain a cable core unit. Rubber strips are filled on the outside of the cable core unit and non-woven fabric tape is wrapped to form a filling layer. Polyethylene material is extruded on the outside of the filling layer and cooled to form a polyethylene isolation sleeve. A galvanized steel strip is then wrapped around the gaps to form an outer sheath layer.

10. The method for preparing a cold-resistant cable according to claim 9, characterized in that, The outer sheath material is prepared through the following steps: EPDM rubber is pre-plasticized by thin-passing, with the roller temperature controlled at 40-50℃, and thin-passed 5-6 times. Nano-calcium carbonate and modified basalt fiber are dried at 75-80℃ for 3-4 hours. Antioxidant and lubricant are mixed evenly to obtain the additives. Take out 20-25 parts of EPDM rubber and put it into the open mill. Control the roller temperature at 50-60℃. Add modified basalt fiber multiple times until the fiber is completely wrapped by the rubber compound. Adjust the roller gap and pass through the mill 3 times. Make triangular wraps twice. After sheeting, cut it into 3-5mm rubber granules to obtain fiber reinforced masterbatch. Add the remaining EPDM rubber and fiber-reinforced masterbatch to the internal mixer, and mix under pressure for 2-3 minutes until the rubber compound is completely melted and plasticized. Then add 70%-75% of the total weight of cold-resistant plasticizer, and continue mixing for 2-2.5 minutes. Add active nano calcium carbonate and additives, and mix for 1-2 minutes. Add the remaining cold-resistant plasticizer, and continue mixing for 2-3 minutes. When the rubber compound temperature reaches 125-130℃, discharge the rubber and transfer it to an open mill for thin passing 2-3 times. Air cool to room temperature to obtain the initial rubber compound. Put the primary rubber into an internal mixer and plasticize for 1-1.5 minutes. Add vulcanizing agent and crosslinking agent and mix for 3-4 minutes. During this period, the rubber temperature should not exceed 120℃. After mixing evenly, discharge the rubber and pass it through a two-roll mill 3 times and make triangular wraps 2 times. After sheeting and cooling to room temperature, the outer sheath material is obtained.