A rare-earth barium copper-oxygen superconducting tape with high quench propagation velocity, its preparation method and application
By setting an interface impedance control layer between the silver protective layer and the copper stabilizing layer, the current distribution and Joule heat distribution are adjusted, solving the problem of slow quench propagation speed in rare earth barium copper oxide superconducting tapes, and achieving high quench propagation speed and low manufacturing energy consumption.
Patent Information
- Application Number
- CN202611482539.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-22
- Publication Date
- 2026-11-17
AI Technical Summary
Existing rare-earth barium copper oxide superconducting tapes exhibit low quench propagation speeds after localized quench loss, limiting their application in high-field magnets, superconducting motors, and superconducting cables. Furthermore, existing enhancement methods increase the amount of copper used and manufacturing energy consumption.
An interface impedance control layer is set between the silver protective layer and the copper stabilizing layer to adjust the current distribution rate and current transfer region. The longitudinal current ratio and Joule heat distribution in the silver and copper layers are adjusted by the interface impedance control layer, so as to achieve faster quench voltage establishment.
It improves the quench propagation speed, maintains the critical current without decreasing, is suitable for mass production, reduces copper consumption and manufacturing energy consumption, and adapts to the quench propagation requirements of different application scenarios.
Smart Images

Figure CN123120424A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of second-generation high-temperature superconducting tapes and superconducting cables, and particularly to a rare-earth barium copper oxide superconducting tape with high quench propagation velocity, its preparation method, and its application. Background Technology
[0002] Rare-earth barium copper oxide (REBCO)-based second-generation high-temperature superconducting coated conductors possess high critical temperatures, critical current densities, and irreversible fields, enabling them to withstand high current densities in the liquid nitrogen temperature range or even lower. Therefore, they are widely used in high-field magnets, superconducting motors, superconducting cables, superconducting energy storage, and power current limiting equipment. As these devices evolve towards higher power densities, miniaturization, and long-term stable operation, the quench detection speed and thermal safety after localized thermal disturbances in the strip have become key factors limiting system reliability.
[0003] In engineering, quench safety is often improved by increasing the thickness of the copper stabilizing layer, increasing the heat capacity, or reducing the operating current margin. These methods can reduce transient peak temperature rise, but they increase copper usage, strip mass, winding volume, and subsequent electroplating time. For superconducting motors, compact magnets, and long-distance cables, they may further increase structural weight and manufacturing energy consumption. Therefore, for advanced manufacturing and energy-saving equipment, there is a need for a strip structure that can maintain the low-resistance bypass capability of the copper stabilizing layer, actively regulate the early thermo-electric response of quench, and is suitable for continuous mass production.
[0004] The silver layer in existing superconducting tapes serves two purposes: protecting the REBCO surface and reducing the risk of chemical and mechanical damage to the superconducting layer during processing, and also participating in current carrying after quench. The copper stabilizing layer has a much larger cross-sectional area than the silver layer and lower resistivity. Therefore, in conventional silver-copper direct contact structures, the current entering the silver layer after a localized quench will quickly be diverted to the copper layer. The limited longitudinal current and Joule heating distance within the silver layer results in a low quench propagation speed, thus restricting its further applications. Therefore, it is necessary to explore effective methods to improve the quench propagation speed of superconducting tapes and enhance the reliability of REBCO superconducting materials in applications. Summary of the Invention
[0005] To address the aforementioned problems, this invention provides a rare-earth barium copper-oxygen superconducting tape with high quench propagation velocity, its preparation method, and its applications.
[0006] In a first aspect, the present invention provides a high quench propagation velocity rare earth barium copper oxide superconducting tape, which, along the thickness direction of the high quench propagation velocity rare earth barium copper oxide superconducting tape, includes a substrate layer, a buffer layer, a rare earth barium copper oxide superconducting layer, a silver protective layer and a copper stabilizing layer.
[0007] An interface impedance control layer is provided between the silver protective layer and the copper stabilizing layer.
[0008] Furthermore, the thickness c of the interface impedance regulation layer is 5nm to 2000nm;
[0009] The thickness 'a' of the silver protective layer is 0.5 μm to 5 μm;
[0010] The thickness b of the copper stabilizing layer is 2μm to 50μm.
[0011] Furthermore, the bulk resistivity of the interface impedance regulation layer is 0.1 Ω·m to 1 × 10⁻⁶. 12 Ω·m.
[0012] Furthermore, the surface coverage of the interface impedance regulating layer on the silver protective layer is 30% to 100%.
[0013] Furthermore, the arrangement of the interface impedance control layer includes at least one of the following: a continuous central region along the strip length direction, segmented regions spaced apart along the strip length direction, strip regions distributed along the strip width direction, lattice regions distributed along the strip width direction, grid regions distributed along the strip width direction, and coverage gradient regions distributed along the strip width direction.
[0014] Furthermore, the material of the interface impedance regulation layer includes one or more of SiO2, Al2O3, TiO2, MgO, AlN, Y2O3, Cr2O3, CeO2, LaMnO3, HfO2, BaZrO3, Ta2O5, Si3N4, La2O3, CaF2, MgF2 and LiF;
[0015] Alternatively, the material of the interface impedance control layer may include at least one of ceramic compounds, nitrides, and fluorides.
[0016] Furthermore, at least one silver-copper resistive connection area is retained outside the interface impedance control layer, and the silver-copper resistive connection area is located at the strip edge, strip end, predetermined welding area or current lead-out area;
[0017] An adhesive layer is provided between the silver protective layer and the interface impedance regulation layer;
[0018] A conductive seed layer is provided between the interface impedance control layer and the copper stabilizing layer.
[0019] Furthermore, the thickness of the substrate layer is 20 μm to 150 μm; the material of the substrate layer includes at least one of nickel-based alloys and iron-based alloys;
[0020] The buffer layer is a single-layer or multi-layer structure with a total thickness of 10 nm to 2 μm, preferably 50 nm to 500 nm; the buffer layer material includes, but is not limited to, one or more of MgO, Al2O3, Y2O3, CeO2, LaMnO3, YSZ, Y2Zr2O7, Gd2Zr2O7, La2Zr2O7, SrTiO3, and BaZrO3.
[0021] The thickness of the rare earth barium copper oxide superconducting layer is 0.5 μm to 3 μm;
[0022] The thickness of the adhesive layer is 1 / 10 to 3 / 10 of the thickness of the interface impedance control layer, and the material of the adhesive layer includes one or more of Ti or its alloys, Cr or its alloys, and Ta or its alloys.
[0023] The thickness of the conductive seed layer is 20 nm to 500 nm, and the material of the conductive seed layer includes at least one of Ag, Cu and Ni.
[0024] Secondly, based on the same inventive concept, this invention provides a method for preparing the high quench propagation velocity rare-earth barium copper-oxygen superconducting tape described in the first aspect, comprising the following steps:
[0025] A REBCO tape semi-finished product with a base layer, buffer layer, rare earth barium copper oxide superconducting layer, and silver protective layer was obtained;
[0026] According to the preset structural composition, a residual structural layer is formed on the surface of the silver protective layer of the REBCO tape semi-finished product to obtain the high quench propagation velocity rare earth barium copper oxide superconducting tape.
[0027] Thirdly, based on the same inventive concept, this invention provides the application of the high quench propagation velocity rare earth barium copper oxide superconducting tape described in any of the first aspects or the high quench propagation velocity rare earth barium copper oxide superconducting tape prepared by the preparation method of the high quench propagation velocity rare earth barium copper oxide superconducting tape described in the second aspect in superconducting magnets, superconducting motors, generators, superconducting cables, superconducting energy storage devices, superconducting current limiters, and fusion magnets.
[0028] The technical solutions provided in the embodiments of the present invention have at least the following advantages compared with the prior art:
[0029] This invention provides a high quench propagation velocity rare-earth barium copper-oxide superconducting tape, its preparation method, and its applications. Based on existing rare-earth barium copper-oxide superconducting tapes, this invention primarily improves stability and quench propagation velocity by setting an interface impedance control layer between the silver protective layer and the copper stabilizing layer. This layer regulates the current distribution rate and current transfer region between the silver protective layer and the copper stabilizing layer during quench propagation, and allows the copper stabilizing layer to continue providing low-resistance bypass and thermal stability after current redistribution. This achieves a synergistic improvement in stability and quench propagation velocity, thus meeting the application requirements in fields such as high-field magnets, superconducting motors, superconducting cables, energy storage devices, and current-limiting equipment. Specifically:
[0030] (1) The superconducting layer has zero process disturbance and is compatible with commercial strip structure.
[0031] The interface impedance control layer is located at the secondary current distribution interface between the silver protective layer and the copper stabilizing layer. It does not touch the REBCO superconducting layer, the buffer layer, or the REBCO / silver primary current injection interface, thus avoiding reprocessing disturbances to the surface states, epitaxial relationships, and critical current injection conditions of the superconducting layer. Commercial silver-coated REBCO tapes can have this structure added without modifying the original roll-to-roll epitaxial lines, and are directly compatible with existing industrial tape systems without reducing the critical current Ic.
[0032] (2) The quench response can be quantitatively controlled.
[0033] By selecting four parameters—resistivity, thickness, coverage, and morphology (continuous, segmented, striped, lattice, mesh, gradient)—of the interface impedance control layer material, the longitudinal current ratio and Joule heat distribution within the silver and copper layers can be adjusted, enabling the quench voltage to establish more quickly over a longer range.
[0034] (3) Stability and protection speed are improved in tandem.
[0035] After the current completes the secondary redistribution, the copper stabilizing layer still undertakes the main bypass current and heat diffusion functions; a low-resistance connection area is retained at the end of the strip or the edge of the width to reduce current output and additional losses at the joint, taking into account both high propagation speed and low operating loss, and is suitable for different chemical conditions of high field magnets, superconducting motors, superconducting cables, energy storage devices and current limiting equipment.
[0036] (4) The process temperature is low and it is compatible with roll-to-roll production lines.
[0037] After the silver protective layer is completed, the interface impedance control layer is formed using low-temperature processes such as magnetron sputtering, atomic layer deposition (ALD), and chemical vapor deposition (CVD) at ≤180℃. It is connected in series with the subsequent continuous copper electroplating process and does not interfere with the REBCO native epitaxial process. It is suitable for long strip roll-to-roll patterned manufacturing and online inspection, avoiding the problem that CFD solutions need to be embedded in the original production line and are difficult to scale up.
[0038] (5) Reduce copper material redundancy and manufacturing costs.
[0039] While achieving the same safety margin for quench protection, the reliance on "simply increasing the thickness of the copper stabilizing layer" is reduced, thereby reducing the amount of copper used, the overall weight of the strip, and the electroplating time for long strips, which is beneficial for energy consumption and raw material saving of long strips.
[0040] (6) The structure can be customized and expanded according to working conditions.
[0041] To address the differences in thermal boundary and current-carrying distribution of magnets, motors, cables, or current limiters, continuous, segmented, lattice, grid, or gradient impedance patterns can be selected to achieve customized design of protection characteristics at different locations of the strip, adapting to the quench propagation requirements of multiple application scenarios.
[0042] (7) Quality can be quantified and controlled online / offline.
[0043] Since the interface impedance control layer is located in the metallization process on the outside of the strip, it can be tested online or offline using indicators such as sheet resistance, film thickness, optical reflectivity, adhesion and local voltage response, which facilitates the establishment of a manufacturing consistency and batch traceability system.
[0044] (8) Without sacrificing superconducting transport performance.
[0045] Since the interface impedance modulation layer is not located at the superconducting current main channel and the REBCO / silver first-stage injection interface, the critical current Ic, n value and transport characteristics under magnetic field of the REBCO layer remain unchanged. The protection function is achieved by improving the structure of the metallized section, which decouples it from the intrinsic superconducting properties. Attached Figure Description
[0046] The accompanying drawings, which are incorporated in and form part of this specification, illustrate embodiments consistent with the invention and, together with the description, serve to explain the principles of the invention.
[0047] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, for those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0048] Figure 1 This is a structural comparison diagram of the rare earth barium copper oxide superconducting tapes provided in Example 1 and Comparative Example 1 of the present invention.
[0049] Figure 2 This is a comparison of the quench propagation velocities of the rare-earth barium copper oxide superconducting tapes provided in Example 1 and Comparative Example 1 under different current carrying conditions at 77 K.
[0050] Figure 3 This is a comparison of the quench propagation velocities of the rare-earth barium copper-oxygen superconducting tapes provided in Example 1 and Comparative Example 1 under different current carrying conditions at 20K.
[0051] Figure 4 The graph shows the variation of quench propagation velocity with the resistivity of the functional layer material under different current-carrying conditions at 77 K for the rare-earth barium copper oxide superconducting tape provided in Example 1 of the present invention when the impedance modulation layer thickness is 100 nm.
[0052] Figure 5 The graph shows the result of the change in quench propagation velocity of the rare earth barium copper oxide superconducting tape provided in Example 1 of the present invention at 77 K as a function of the coverage of the interface impedance modulation layer.
[0053] Figure 6 This is a comparison diagram of the quenching region expansion of the rare earth barium copper oxide superconducting tapes provided in Embodiment 1 and Comparative Example 1 of the present invention.
[0054] Figure 1 In the middle: 1-base layer, 2-buffer layer, 3-rare earth barium copper oxide superconducting layer, 4-silver protective layer, 5-copper stabilizing layer, 6-interface impedance regulation layer, 7-adhesion layer, 8-conductive seed layer. Detailed Implementation
[0055] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0056] The technical concept of this invention is as follows:
[0057] This invention enables structured control of the second-stage current distribution between the silver and copper layers without altering the REBCO / silver contact interface. By regulating the redistribution of the early quench current between the silver protective layer and the copper stabilizing layer, it creates controllable distributed heating within both layers, thereby increasing the heating and voltage build-up rate in the adjacent region and improving the normal zone expansion capability. Simultaneously, it retains the low-resistance bypass and thermal diffusion functions of the copper stabilizing layer in subsequent stages, achieving a synergistic improvement in stability and quench propagation speed. Furthermore, it avoids introducing additional interface processes into the superconducting functional layer, making it compatible with existing REBCO epitaxial fabrication processes. It can be integrated with mature processes such as vacuum deposition, patterned deposition, and copper electroplating, achieving a balance between performance regulation, manufacturing compatibility, and material utilization efficiency. This allows for mass production using roll-to-roll surface fabrication processes. Therefore, the core focus of this invention is on regulating the current distribution within the stabilizing layer between the silver protective layer and the copper stabilizing layer, rather than relying on altering the superconducting / stabilizing layer contact interface to achieve performance changes. This back-end metallization structure design allows for the optimization of quench response to be adapted to the fabrication of REBCO superconducting layers and silver protection processes.
[0058] Specifically, the technical solution provided by this invention is as follows:
[0059] In a first aspect, the present invention provides a high quench propagation velocity rare earth barium copper oxide superconducting tape, which, along the thickness direction of the high quench propagation velocity rare earth barium copper oxide superconducting tape, includes a substrate layer, a buffer layer, a rare earth barium copper oxide superconducting layer, a silver protective layer and a copper stabilizing layer.
[0060] An interface impedance control layer is provided between the silver protective layer and the copper stabilizing layer.
[0061] The interface impedance control layer introduced in this invention is located between the silver protective layer and the copper stabilizing layer, rather than between the REBCO superconducting layer and the silver protective layer. This not only improves stability and propagation speed, but also allows for the maintenance of existing mature processes for REBCO epitaxial growth, buffer layer structure, and REBCO / silver contact interface. The additional steps can be concentrated in the metallization stage at the back of the strip. Furthermore, the interface impedance control layer in this invention can be an electrically insulating layer, a high-resistivity semiconductor layer, or an equivalent high-resistivity structure composed of multiple thin films.
[0062] Furthermore, the thickness c of the interface impedance control layer is 5nm to 2000nm, for example, it can be 5nm, 50nm, 100nm, 500nm, 1000nm, 1500nm, 2000nm or any of the aforementioned values, preferably 20nm to 500nm.
[0063] The thickness 'a' of the silver protective layer is 0.5 μm to 5 μm, for example, it can be 0.5 μm, 1 μm, 3 μm, 5 μm or any of the aforementioned values;
[0064] The thickness b of the copper stabilizing layer is 2μm to 50μm, for example, it can be 2μm, 10μm, 20μm, 40μm, 50μm or any of the aforementioned values, preferably 8μm to 20μm.
[0065] Furthermore, the bulk resistivity of the interface impedance regulation layer is 0.1 Ω·m to 1 × 10⁻⁶. 12 Ω·m, for example, can be 0.1Ω·m, 50Ω·m, 100Ω·m, 1×10 5 Ω·m, 1×10 8 Ω·m, 1×10 12 The range of Ω·m or any of the aforementioned values is preferably 10 Ω·m to 1 × 10⁻⁶. 8 Ω·m.
[0066] Further, the surface coverage of the interface impedance control layer over the silver protective layer is 30% to 100%, for example, it can be 30%, 40%, 50%, 60%, 80%, 100% or any range between the aforementioned values, preferably 50% to 95%. The arrangement of the interface impedance control layer includes at least one of the following: a continuous central region along the strip length direction, segmented regions spaced along the strip length direction, strip regions distributed along the strip width direction, lattice regions distributed along the strip width direction, grid regions distributed along the strip width direction, and regions with gradually changing coverage along the strip width direction. In this invention, the interface impedance control layer can be fully covered or partially covered. When partially covered, it is preferable to retain the silver-copper direct contact area as a low-resistance connection area. The low-resistance connection area can be located at both edges of the strip, or it can be set as a spaced window, lattice window, grid window, or end-dedicated connection area along the length direction. By adjusting the coverage, window size, and pattern period, the ratio of longitudinal current in the timeout silver layer to the ratio of copper layer current can be adjusted.
[0067] When the strip is operating normally, the temperature is below the critical temperature, and the current carrying capacity is below the allowable value, the majority of the current is carried by the REBCO superconducting layer, and the silver-copper interface impedance modulation layer has little impact on steady-state losses. When a local REBCO enters a resistive state, the current first enters the silver protective layer through the existing REBCO / silver interface. Due to the local conductivity of the silver-copper interface being limited by the impedance modulation layer, some current does not immediately enter the copper layer at that location. Instead, it continues to propagate a certain distance along the length of the strip in the thin silver layer, and then enters the copper stabilizing layer through uncovered areas, conductive windows, or finite resistance channels. Because the cross-sectional area of the silver layer is small, its resistance per unit length is higher than that of the thick copper layer, thus forming a relatively dispersed Joule heat wave near the local quench front. This heat wave can increase the temperature of adjacent areas and expand the end-to-end voltage build-up range, thereby facilitating quench propagation and protection detection.
[0068] Furthermore, the material of the interface impedance control layer includes one or more of SiO2, Al2O3, TiO2, MgO, AlN, Y2O3, Cr2O3, CeO2, LaMnO3, HfO2, BaZrO3, Ta2O5, Si3N4, La2O3, CaF2, MgF2, and LiF; or, the material of the interface impedance control layer includes at least one of ceramic compounds, nitrides, and fluorides. For applications requiring both resistance control and improved lateral thermal conductivity, insulating materials with relatively high thermal conductivity, such as AlN or MgO, are preferred.
[0069] Furthermore, at least one silver-copper resistive connection region is retained outside the interface impedance control layer. This silver-copper resistive connection region is located at the strip edge, strip end, predetermined welding area, or current lead-out area. An adhesive layer is provided between the silver protective layer and the interface impedance control layer. A conductive seed layer is provided between the interface impedance control layer and the copper stabilizing layer. To ensure the continuity of subsequent copper electroplating, an Ag, Cu, or Ni conductive seed layer can be deposited on the surface of the impedance control layer. The seed layer mainly provides a continuous electroplating surface, and its thickness can be 20 nm to 500 nm. The copper stabilizing layer can be formed by electroplating, and its single-sided or equivalent total thickness can be designed to be 2 μm to 50 μm according to the required thermal stability of the equipment.
[0070] Specifically, for a 12 mm wide strip, a continuous impedance control layer can be set in the middle 11 mm region, with approximately 0.5 mm silver-copper direct connection areas reserved on both sides; alternatively, the middle functional layer can be divided into multiple units spaced along the length direction to reduce the risk of cracking in the continuous ceramic film when bending long strips. For applications requiring current leads to be welded at the ends, it is preferable to reserve a 5 mm to 50 mm low-resistance connection area without functional layer deposition at both ends of the strip.
[0071] Furthermore, the thickness of the substrate layer is 20μm to 150μm, preferably 30μm to 100μm, and even more preferably 40μm to 60μm; the material of the substrate layer includes nickel-based alloys and iron-based alloys, such as Hastelloy alloys.
[0072] The buffer layer is a single-layer or multi-layer structure with a total thickness of 10 nm to 2 μm, preferably 50 nm to 500 nm; the buffer layer material includes, but is not limited to, one or more of MgO, Al2O3, Y2O3, CeO2, LaMnO3, YSZ, Y2Zr2O7, Gd2Zr2O7, La2Zr2O7, SrTiO3, and BaZrO3.
[0073] The thickness of the rare earth barium copper oxide superconducting layer is 0.5 μm to 3 μm, for example, it can be 0.5 μm, 1 μm, 2 μm, 3 μm or any of the aforementioned values;
[0074] The thickness of the adhesive layer is 1 / 10 to 3 / 10 of the thickness of the interface impedance control layer, for example, it can be 5nm to 100nm; the material of the adhesive layer includes one or more of Ti or its alloys, Cr or its alloys, and Ta or its alloys.
[0075] The thickness of the conductive seed layer is 20 nm to 500 nm, for example, it can be 20 nm, 50 nm, 100 nm, 200 nm, 500 nm or any range between the aforementioned values, preferably 50 nm to 150 nm; the material of the conductive seed layer includes at least one of Ag, Cu and Ni. Specifically:
[0076] When Ti is selected as the adhesive layer, Al2O3 is the preferred choice as the interface impedance control layer, and SiO2, Si3N4, AlN, and MgO are the secondary choices.
[0077] When Cr is selected as the adhesive layer, Al2O3 or Cr2O3 is preferred as the interface impedance control layer, and SiO2 is the second choice.
[0078] When Ta is selected as the adhesive layer, Al2O3 or Ta2O5 is preferred as the interfacial impedance control layer, followed by Al2O3, AlN, and Si3N4. Although fluorides have high resistivity, their interfacial chemical bonding with Ti, Cr, and Ta metal adhesive layers is generally less reliable than that of oxide systems when in direct contact. Therefore, when fluorides are used, a metal adhesive layer / Al2O3 transition layer / fluoride approach is more suitable.
[0079] Secondly, based on the same inventive concept, this invention provides a method for preparing the high quench propagation velocity rare-earth barium copper-oxygen superconducting tape described in the first aspect, comprising the following steps:
[0080] A REBCO tape semi-finished product with a base layer, buffer layer, rare earth barium copper oxide superconducting layer, and silver protective layer was obtained;
[0081] According to the preset structural composition, a residual structural layer is formed on the surface of the silver protective layer of the REBCO tape semi-finished product to obtain the high quench propagation velocity rare earth barium copper oxide superconducting tape.
[0082] Specifically, the preparation method of the above-mentioned rare-earth barium copper-oxygen superconducting tape with high quench propagation velocity may include the following steps in actual operation:
[0083] The REBCO tape semi-finished product with a base layer, buffer layer, rare earth barium copper oxide superconducting layer and silver protective layer is surface cleaned and activated; the interface impedance control region is defined by masking, photolithography, laser patterning or selective deposition; an interface impedance control layer is formed in the region; a conductive seed layer is formed on it; and then a copper stabilizing layer is formed by electroplating or chemical deposition.
[0084] The interface impedance control layer is prepared by at least one of magnetron sputtering, reactive magnetron sputtering, chemical vapor deposition, pulsed laser deposition, spraying or printing, and the highest process temperature for forming the interface impedance control layer is ≤180℃.
[0085] The process employs a roll-to-roll method to complete at least three consecutive steps: unwinding, surface cleaning, patterned deposition, seed layer deposition, copper electroplating, online thickness detection, online resistance detection, and rewinding. The process stability is determined online based on the sheet resistance, film thickness, or voltage response of the interface region.
[0086] Thirdly, based on the same inventive concept, this invention provides the application of the high quench propagation velocity rare earth barium copper oxide superconducting tape described in any of the first aspects or the high quench propagation velocity rare earth barium copper oxide superconducting tape prepared by the preparation method of the high quench propagation velocity rare earth barium copper oxide superconducting tape described in the second aspect in superconducting magnets, superconducting motors, generators, superconducting cables, superconducting energy storage devices, superconducting current limiters, and fusion magnets.
[0087] Unless otherwise specified, all raw materials, reagents, instruments, and equipment used in this invention can be purchased commercially or prepared using existing methods. Furthermore, unless otherwise specified or detailed, the steps and parameters involved can be performed according to the existing rare-earth barium copper oxide superconducting tape preparation process and parameters, or directly using existing equipment according to the instruction manual. These will not be elaborated upon further in this invention document.
[0088] The present invention will be further illustrated below with reference to specific embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the invention. Experimental methods in the following embodiments, unless otherwise specified, are generally performed according to national standards. If no corresponding national standard exists, then generally accepted international standards, conventional conditions, or conditions recommended by the manufacturer are followed.
[0089] Example 1
[0090] This example provides a rare-earth barium copper-oxygen superconducting tape with high quench propagation velocity, such as... Figure 1 As shown in (b) Figure 1 The structure consists of: 1-base layer, 2-buffer layer, 3-rare earth barium copper oxide superconducting layer, 4-silver protective layer, 5-copper stabilizing layer, 6-interface impedance control layer, 7-adhesion layer, 8-conductive seed layer), and sequentially includes the base layer, buffer layer, rare earth barium copper oxide superconducting layer, silver protective layer, adhesion layer, interface impedance control layer, conductive seed layer, and copper stabilizing layer along its thickness direction.
[0091] The base layer is made of Hastelloy alloy and has a thickness of 50 mm. ;
[0092] The buffer layer is made of Y2O3 and has a thickness of 325 nm;
[0093] The thickness of the rare earth barium copper oxide superconducting layer is 1.5 μm;
[0094] The thickness of the silver protective layer is 1.5 μm;
[0095] The adhesive layer is made of Ti and has a thickness of 30 nm;
[0096] The interface impedance control layer is made of Al2O3 and has a thickness of 100nm. It has a surface coverage of 91.7% of the silver protective layer and is arranged in a way that it is evenly distributed from the center of the width of the superconducting tape to both sides.
[0097] The conductive seed layer is made of Ag and has a thickness of 70 nm;
[0098] The thickness of the copper stabilizing layer is 8 μm.
[0099] The preparation method of the above-mentioned high quench propagation velocity rare earth barium copper oxide superconducting tape includes the following steps:
[0100] Step (1): A commercial REBCO tape sample with the above-mentioned structural parameters, including a base layer, a buffer layer, a rare earth barium copper oxide superconducting layer, and a silver protective layer, is used. The sample is 12 mm wide and 100 mm long. The silver surface near the REBCO superconducting layer is patterned: a polyimide mask of about 0.5 mm wide is covered on both sides, and the middle area of about 11 mm is left exposed.
[0101] Step (2): After plasma activation of the exposed silver surface, a 30 nm Ti layer was first deposited as an adhesion layer by magnetron sputtering, followed by a 100 nm Al2O3 layer as an interface impedance control layer, and then a 70 nm Ag layer as a conductive seed layer. After removing the mask, silver-copper direct connection channels were formed on both sides, and a Ti / Al2O3 / Ag functional stack was formed in the middle; finally, an 8 μm copper stabilizing layer was formed around the perimeter.
[0102] Example 2
[0103] The only difference between this example and Example 1 is that:
[0104] (1) The thickness of the silver protective layer is 1 μm;
[0105] (2) The thickness of the interface impedance control layer is 8 nm;
[0106] (3) The thickness of the copper stabilizing layer is 2 μm.
[0107] Example 3
[0108] The only difference between this example and Example 1 is that:
[0109] (1) The thickness of the silver protective layer is 5 μm;
[0110] (2) The thickness of the interface impedance control layer is 2000 nm;
[0111] (3) The thickness of the copper stabilizing layer is 50 μm.
[0112] Example 4
[0113] The only difference between this example and Example 1 is that:
[0114] (1) The buffer layer is made of CeO2;
[0115] (2) The thickness of the rare earth barium copper oxide superconducting layer is 2.5 μm;
[0116] (3) The thickness of the silver protective layer is 3.0 μm;
[0117] (4) The adhesive layer is made of Ti and has a thickness of 20 nm;
[0118] (5) The interface impedance control layer is made of Al2O3 with a thickness of 200nm and a surface coverage of 35% of the silver protective layer. Its arrangement is evenly distributed along the center of the width of the superconducting tape to both sides.
[0119] The conductive seed layer is made of Ag and has a thickness of 70 nm;
[0120] The thickness of the copper stabilizing layer is 8 μm.
[0121] Comparative Example 1
[0122] This example provides a rare-earth barium copper oxide superconducting tape, such as Figure 1 As shown in Figure (a), the difference from Example 1 is that the interface impedance control layer, adhesive layer, and conductive seed layer are not provided.
[0123] The preparation method of the above-mentioned rare earth barium copper oxide superconducting tape includes the following steps:
[0124] Select REBCO tape samples from the same batch as in Example 1, which have already formed the above-mentioned structural parameters, including the substrate layer, buffer layer, rare earth barium copper oxide superconducting layer, and silver protective layer. The tapes are 12 mm wide and 100 mm long. After cleaning, an 8 μm copper stabilizing layer is formed directly around the edges.
[0125] Comparative Example 2
[0126] This example provides a rare-earth barium copper oxide superconducting tape, which differs from Example 1 in that:
[0127] (1) An interface impedance control layer is set between the rare earth barium copper oxide superconducting layer and the silver protective layer.
[0128] Test case
[0129] This example demonstrates the performance testing of the high quench propagation velocity rare-earth barium copper oxide superconducting tapes obtained in the above embodiments and comparative examples.
[0130] The testing method is as follows:
[0131] The testing process for the critical current and quench propagation velocity of the superconducting tape is as follows: First, the rare-earth barium copper oxide superconducting tape to be tested is installed in a cryogenic testing device and cooled to the set operating temperature. The critical current is tested using the four-lead method, that is, a transport current is applied to both ends of the tape, and independent voltage leads are arranged in the effective testing range of the sample. The current flowing into the tape is gradually increased while the voltage signal is collected simultaneously. The critical current Ic of the tape is determined according to the specified critical electric field criterion. After the critical current test is completed, the operating current of the quench propagation experiment is set according to the measured Ic, so that the sample can operate stably under a constant transport current. Then, a controllable thermal disturbance is applied locally to the tape to trigger quench, and multiple temperature sensors are arranged at equal intervals along the length of the tape to record the temperature change over time at different locations in real time. As the quench zone propagates sequentially to each temperature measuring point, the arrival time of the quench front at each measuring point is determined according to a unified temperature criterion (92 K). Combining the actual distance between adjacent thermometers and the corresponding time difference, the quench propagation velocity along the length of the strip is calculated using v = Δx / Δt, where Δx is the displacement of the quench zone during the time interval Δt. To ensure comparability of results between different samples, the test temperature, current carrying capacity, thermal disturbance location, and thermal disturbance conditions are kept consistent across all experimental groups, and multiple repeated tests are conducted to obtain the average value.
[0132] Table 1
[0133] Test sample Critical current degradation (%) Chuck propagation speed (cm / s) Example 1 0 42.5 Example 2 0 124.6 Example 3 0 21.2 Example 4 0 26.4 Comparative Example 1 0 18.6 Comparative Example 2 24.5% 19.8
[0134] As shown in Table 1, after introducing an interface impedance control layer between the silver and copper interfaces, the critical current does not degrade significantly, and the quench propagation speed is improved to a certain extent relative to the control.
[0135] In addition, other performance tests of Embodiment 1 and Comparative Example 1 of the present invention are as follows: Figure 2 , Figure 3 , Figure 4 , Figure 5 , Figure 6 As shown ( Figure 2 , Figure 3 , Figure 6 In the text: "Conventional tape" refers to the tape obtained in Comparative Example 1, and "Silver-copper interface set with 100 nm Al2O3" refers to the tape obtained in Example 1.
[0136] from Figure 2 and Figure 3 It can be seen that when superconducting tapes are used at 20 K and 77 K, after introducing an interface impedance modulation layer at the silver-copper interface, the increase in quench propagation velocity becomes more and more significant with the increase of current carrying capacity.
[0137] Figure 4The study analyzed that when the thickness of the interfacial impedance control layer is fixed at 100 nm, the quench propagation velocity increases with the increase of the resistivity of the interfacial impedance control layer material, and tends to stabilize when the resistivity is 10 Ω·m.
[0138] Figure 5 This indicates that when the thickness of the interface impedance control layer is 100 nm and the resistivity is 10 Ω·m, the quench propagation velocity increases with the increase of the coverage of the interface impedance control layer.
[0139] Figure 6 The study analyzed the expansion trend of the quenching region in superconducting tapes after introducing a 100 nm thick, 10 Ω·m resistivity interfacial impedance modulation layer at the silver-copper interface. Comparing the coverage of the layer with different widths, it was found that the larger the coverage of the interfacial impedance modulation layer within the same time period, the faster the quenching region propagated, further supporting this finding. Figure 5 The result.
[0140] Various embodiments of the present invention may exist in the form of a range; it should be understood that the description in the form of a range is merely for convenience and brevity and should not be construed as a hard limitation on the scope of the invention; therefore, it should be considered that the range description has specifically disclosed all possible subranges and single numerical values within that range. For example, it should be considered that the range description from 1 to 6 has specifically disclosed subranges such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., and single numbers within the range, such as 1, 2, 3, 4, 5, and 6, regardless of the range. Furthermore, whenever a numerical range is referred to herein, it means including any referenced number (fraction or integer) within the range referred to.
[0141] The above description is merely a specific embodiment of the present invention, enabling those skilled in the art to understand or implement the invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the present invention is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features claimed herein.
Claims
1. A rare-earth barium copper-oxygen superconducting tape with high quench propagation velocity, characterized in that, Along the thickness direction of the high quench propagation velocity rare earth barium copper oxide superconducting tape, it includes a base layer, a buffer layer, a rare earth barium copper oxide superconducting layer, a silver protective layer, and a copper stabilizing layer. An interface impedance control layer is provided between the silver protective layer and the copper stabilizing layer.
2. The high quench propagation velocity rare-earth barium copper-oxygen superconducting tape according to claim 1, characterized in that, The thickness c of the interface impedance regulation layer is 5nm to 2000nm; The thickness 'a' of the silver protective layer is 0.5 μm to 5 μm; The thickness b of the copper stabilizing layer is 2μm to 50μm.
3. The high quench propagation velocity rare-earth barium copper-oxygen superconducting tape according to claim 1, characterized in that, The bulk resistivity of the interface impedance control layer is 0.1 Ω·m to 1 × 10⁻⁶. 12 Ω·m.
4. The high quench propagation velocity rare-earth barium copper-oxygen superconducting tape according to claim 1, characterized in that, The surface coverage of the interface impedance control layer on the silver protective layer is 30% to 100%.
5. The high quench propagation velocity rare-earth barium copper-oxygen superconducting tape according to claim 1, characterized in that, The arrangement of the interface impedance control layer includes at least one of the following: a continuous central region along the strip length direction, segmented regions spaced apart along the strip length direction, strip regions distributed along the strip width direction, lattice regions distributed along the strip width direction, grid regions distributed along the strip width direction, and coverage gradient regions distributed along the strip width direction.
6. The high quench propagation velocity rare-earth barium copper-oxygen superconducting tape according to claim 1, characterized in that, The material of the interface impedance regulation layer includes one or more of SiO2, Al2O3, TiO2, MgO, AlN, Y2O3, Cr2O3, CeO2, LaMnO3, HfO2, BaZrO3, Ta2O5, Si3N4, La2O3, CaF2, MgF2 and LiF; Alternatively, the material of the interface impedance control layer may include at least one of ceramic compounds, nitrides, and fluorides.
7. The high quench propagation velocity rare-earth barium copper-oxygen superconducting tape according to claim 1, characterized in that, At least one silver-copper resistive connection area is retained outside the interface impedance control layer. The silver-copper resistive connection area is located at the strip edge, strip end, predetermined welding area, or current lead-out area. An adhesive layer is provided between the silver protective layer and the interface impedance regulation layer; A conductive seed layer is provided between the interface impedance control layer and the copper stabilizing layer.
8. The high quench propagation velocity rare-earth barium copper-oxygen superconducting tape according to claim 7, characterized in that, The thickness of the substrate layer is 20 μm to 150 μm, and the material of the substrate layer includes at least one of nickel-based alloys and iron-based alloys; The buffer layer is a single-layer or multi-layer structure with a total thickness of 10 nm to 2 μm; the buffer layer material includes, but is not limited to, one or more of MgO, Al2O3, Y2O3, CeO2, LaMnO3, YSZ, Y2Zr2O7, Gd2Zr2O7, La2Zr2O7, SrTiO3, and BaZrO3. The thickness of the rare earth barium copper oxide superconducting layer is 0.5 μm to 3 μm; The thickness of the adhesive layer is 1 / 10 to 3 / 10 of the thickness of the interface impedance control layer, and the material of the adhesive layer includes one or more of Ti or its alloys, Cr or its alloys, and Ta or its alloys. The thickness of the conductive seed layer is 20 nm to 500 nm, and the material of the conductive seed layer includes at least one of Ag, Cu and Ni.
9. A method for preparing a high quench propagation velocity rare-earth barium copper-oxygen superconducting tape according to any one of claims 1-8, characterized in that, Includes the following steps: A REBCO tape semi-finished product with a base layer, buffer layer, rare earth barium copper oxide superconducting layer, and silver protective layer was obtained; According to the preset structural composition, a residual structural layer is formed on the surface of the silver protective layer of the REBCO tape semi-finished product to obtain the high quench propagation velocity rare earth barium copper oxide superconducting tape.
10. The application of a high quench propagation velocity rare earth barium copper oxide superconducting tape according to any one of claims 1-8, or a high quench propagation velocity rare earth barium copper oxide superconducting tape prepared by the preparation method of the high quench propagation velocity rare earth barium copper oxide superconducting tape according to claim 9, in superconducting magnets, superconducting motors, generators, superconducting cables, superconducting energy storage devices, superconducting current limiters, and fusion magnets.